Quick-drying light filler
By using aluminate cement and calcium sulfate mortar compositions and inorganic light fillers in the light filler floor structure, the problems of insufficient load capacity and long curing time are solved, rapid curing and high mechanical properties are achieved, suitable for The substrate with limited load-bearing capacity improves fire resistance and working efficiency.
Patent Information
- Application Number
- CN202380019330.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-04
- Filing Date
- 2023-01-16
- Publication Date
- 2024-11-15
AI Technical Summary
The existing lightweight filler ground structure based on cement bonding has problems such as insufficient load-bearing capacity, long curing time, long drying time, non-refractory and complex working steps, which limits its application on substrates with limited load-bearing capacity.
Aluminate cement and calcium sulfate as binder mortar compositions are used to add a large amount of inorganic light fillers, especially expanded glass, to form a fast cured two- or one-component mortar composition, optimized mechanical properties and curing time.
Achieve rapid and good mechanical properties on substrates with limited load capacity, shorten curing and drying time, reduce weight per unit area, improve fire resistance and maximum load capacity, reduce working steps, and is suitable for residential and commercial Area ground renovation.
Smart Images

Figure GDA0005009073700000171 
Figure GDA0005009073700000172 
Figure GDA0005009073700000191
Abstract
Description
Technical Field
[0001] The invention relates to a mortar composition based on calcium sulfate which is suitable for lightweight fillers and to a floor structure comprising such a lightweight filler. Background Art
[0002] Floor structures are usually based on a cement-bonded screed applied to an existing subfloor. Here, a substrate with a relatively low load-bearing capacity as subfloor may be encountered, for example during floor renovation.
[0003] Conventional screeds usually have a relatively high inherent weight and therefore cannot be used for substrates with critical load-bearing capacity. In such cases, lightweight fillers are used, which are lightened by using lightweight fillers such as polystyrene foam (Styropor).
[0004] Such cementitious bonding systems take a relatively long time to dry, so that they are only ready for application after a relatively long time.
[0005] Floor structures based on lightweight fillers also have a relatively complex structure and usually require the installation of a reinforcement layer and a further levelling layer in addition to the lightweight filler before the final floor covering, such as tiles, can be applied. Therefore, multiple work steps are required.
[0006] Therefore, the common ground structure based on cement-bonded lightweight filler in the prior art has the following problems:
[0007] - Restrictions on the way work is done, such as time limits or space limits for the next work step
[0008] - Short shelf life
[0009] - Long waiting time for walkability
[0010] - Long curing time required for initial strength (sufficient flexural and compressive strength)
[0011] - Long drying time
[0012] - The application of the final coat depends on the drying time of the floor structure - different floor coverings (e.g. tiles, PVC, parquet) require different times
[0013] - long waiting times for the next work step or application of floor coverings
[0014] - Many different work steps, e.g. additional primer
[0015] - Not fire resistant as the filler is polymer based (additional protective structures may be required)
[0016] So-called binary and ternary binders are increasingly used in formulating building materials, for example for mortar compositions which can be used as screeds. Binary binders include aluminate cement and calcium sulfate as hydraulic binders. Ternary binders additionally contain Portland cement as a third hydraulic binder. The advantage of binary and ternary binders compared to standard cements is that the time until they are ready for application is shortened.
[0017] For example, WO 2015 / 150319 A1 relates to fast-drying gypsum compositions based on calcium aluminate and calcium sulfate as hydraulic binders. Summary of the invention
[0018] The object of the present invention is to provide a mortar composition for lightweight fillers which cures quickly and is suitable for producing floor structures on substrates with relatively low load-bearing capacity. In particular, the mortar composition should also be able to achieve a facilitating effect when producing floor structures on bases or substrates with limited load-bearing capacity. Furthermore, the system should exhibit good mechanical properties and achieve good mechanical properties quickly.
[0019] The inventors have found that this object can be achieved by using a mortar composition based on aluminate cement and calcium sulfate, to which a large amount of lightweight fillers, in particular inorganic lightweight fillers, is added.
[0020] The present invention therefore relates to a one-component or two-component mortar composition comprising
[0021] i) an aluminate binder selected from calcium aluminate cement and / or calcium sulphoaluminate cement,
[0022] ii) a calcium sulfate binder selected from calcium sulfate hemihydrate and / or anhydrous calcium sulfate,
[0023] iii) one or more apparent densities of at least 2.0 g / cm 3 of fillers, and
[0024] iv) One or more apparent densities less than 1.5 g / cm 3 Lightweight fillers, especially inorganic lightweight fillers,
[0025] The apparent density is less than 1.5g / cm 3 The amount of lightweight filler, in particular inorganic lightweight filler, is 30 wt % to 70 wt %, and the total amount of aluminate binder and calcium sulfate binder is 20 wt % to 65 wt %, wherein the weight ratio of aluminate binder to calcium sulfate binder is in the range of 1:1 to 1:10, wherein the weight data are based on the dry weight of the mortar composition.
[0026] In the present application, the dry weight of the mortar composition refers to the dry weight of the mortar composition as a whole, ie, in the case of a two-component mortar composition, refers to the combined total weight of the two components.
[0027] The mortar composition according to the invention cures quickly and is particularly suitable as a lightweight filler for producing floor structures on substrates with limited load-bearing capacity. The rapid curing has advantages in terms of the walkability and strength development of the screed and enables production with fewer work steps and faster work processes. In addition, the lightweight filler used has a relatively high strength. On this basis, a typical screed treatment can be realized very well.
[0028] In particular, due to the rapid hydration process of the mortar composition of the present invention when mixed with water, the curing, strength development and the entire drying process are very rapid. This is a prerequisite for shortening the waiting time for the next work step and finally using the ground structure.
[0029] With the mortar composition according to the invention, the next work step (final screeding, ie final levelling of the floor) can be carried out after a waiting time of a few hours (instead of more than a day as in the prior art systems).
[0030] It may be advantageous to use inorganic lightweight fillers, which are fire resistant compared to the commonly used organic polymer-based materials.
[0031] In summary, the mortar composition of the present invention or the mortar composition (leveling layer) mixed with water and applied to a substrate has the following advantages:
[0032] ·You can walk after a few hours
[0033] Quick drying properties
[0034] High and rapid strength development
[0035] Low density
[0036] Low pH (due to gypsum-based technology)
[0037] Shorter working hours
[0038] Ground renovation and final ground structure leveling only requires one day of work
[0039] Fire resistance achieved through the use of mineral materials and inorganic lightweight fillers, especially intumescent glass
[0040] For the ground structure as a whole according to the invention (which will be explained in detail below), there are other advantages:
[0041] · Prepare the final floor covering (tiles, PVC or parquet) in less than 48 hours after work starts
[0042] Reduced work steps, no primer required (using materials based on the same basic formulation)
[0043] Higher maximum loads are possible, therefore suitable for residential and commercial areas
[0044] Extremely low weight per unit area
[0045] Low installation height
[0046] Any layer thickness
[0047] Small deformation under load DETAILED DESCRIPTION
[0048] The present invention relates to a one-component or two-component mortar composition. In a one-component mortar composition, all components are combined in one component, while in a two-component mortar composition, the components are distributed in two components. In the two-component mortar composition of the present invention, preferably one component contains or is formed of one or more lightweight fillers, and the other component contains the other components of the mortar composition. In the two-component mortar composition, the component containing the binder is preferably mixed with water before mixing the component containing the lightweight filler.
[0049] The one-component mortar composition is preferably a dry mortar. Accordingly, the component of the two-component mortar composition that does not contain one or more lightweight fillers is preferably a dry mortar.
[0050] The one-component or two-component mortar composition of the present invention comprises:
[0051] i) an aluminate binder selected from calcium aluminate cement and / or calcium sulphoaluminate cement,
[0052] ii) a calcium sulfate binder selected from calcium sulfate hemihydrate and / or anhydrous calcium sulfate,
[0053] iii) one or more apparent densities of at least 2.0 g / cm 3 of fillers, and
[0054] iv) One or more apparent densities less than 1.5 g / cm 3 Lightweight fillers, especially inorganic lightweight fillers.
[0055] The aluminate binder is calcium aluminate cement and / or calcium sulphoaluminate cement. The aluminate binder is preferably calcium sulphoaluminate cement. The aluminate binder is a hydraulic binder.
[0056] According to one embodiment, the aluminate binder comprises at least one calcium aluminate cement (CAC). The calcium aluminate cement (CAC) according to the invention is in particular a cement comprising clinker comprising hydraulic calcium aluminate, wherein the main phase is preferably CA (C:CaO; A:Al 2 O 3 ). Other calcium aluminates are often present, such as C 2 A.C 3 A.C 12 A 7 The CAC used in the present invention may also generally contain other phases selected from the group consisting of gehlenite (C 2 AS, where C:CaO, A:Al 2 O 3 ,S:SiO 2 ), perovskite (CT, where C:CaO, T:TiO 2 ), Belite (C 2 S, where C:Ca0, S:SiO 2 ), tricalcium silicate, ferrite (C 2 F, C 2 AF, C 4 AF, C:CaO; A:Al 2 O 3 ; F:Fe 2 O 3 ), Ternesit (C 5 S 2 $, where C:CaO, S:SiO 2 ;$:SO 3 ) and aluminum oxide. The CAC of the present invention may additionally contain calcium carbonate. In particular, the CAC of the present invention preferably complies with standard EN 14647. CACs described in other standards (such as ASTM or Chinese standards) are also applicable. Suitable CACs can be commercially obtained, for example, from Royal White Cement.
[0057] According to one embodiment, the aluminate binder comprises at least one calcium sulfoaluminate (CSA) cement. According to the invention, the CSA cement is in particular a cement comprising clinker comprising C 4 (A 3-X F X )$(C:CaO;A:Al 2 O 3 ; F:Fe 2 O 3 ;$:SO 3 ), wherein x is an integer from 0 to 3. The CSA used in the present invention may generally contain other phases selected from aluminates (CA, C 3 A.C12 A 7 , where C:CaO; A:Al 2 O 3 ), Belite (C 2 S, of which C:CaO, S:SiO 2 ), ferrite (C 2 F.C 2 AF, C 4 AF, where C:CaO; A:Al 2 O 3 ; F:Fe 2 O 3 ), calcium sulfide silicate (C 5 S 2 $, where C:CaO, S:SiO 2 ;$:SO 3 ) and anhydrite. In certain embodiments of the present invention, the CSA comprises 15-75 wt.% C 4 A 3 %, 0-10 wt. % aluminate, 0-70 wt. % belite, 0-35 wt. % ferrite, 0-20 wt. % calcite and 0-25 wt. % anhydrite, respectively, based on the total dry weight of the CSA cement. The optional anhydrite is a component of the CSA cement and is accounted for therein. Suitable CSA can be obtained, for example, from Caltra BV under the trade name Calumex.
[0058] The calcium sulfate binder is a hydraulic binder. The calcium sulfate binder is selected from calcium sulfate hemihydrate (CaSO 4 -1 / 2H 2 O) and / or anhydrous calcium sulfate (CaSO 4 ), wherein calcium sulfate hemihydrate is preferred. Anhydrous calcium sulfate is calcium sulfate without water (without crystal water). Calcium sulfate hemihydrate includes α-calcium sulfate hemihydrate and β-calcium sulfate hemihydrate, wherein α-calcium sulfate hemihydrate is preferred.
[0059] As for the calcium sulfate binder, it is preferably composed essentially or completely of calcium sulfate hemihydrate, because too high anhydrous gypsum content can lead to too rapid water absorption by the anhydrous gypsum component, which may affect the workability of the composition. It is therefore preferred that at least 80% by weight, preferably at least 90% by weight, particularly preferably at least 95% by weight of the total amount of calcium sulfate binder consists of calcium sulfate hemihydrate (the remainder being anhydrous calcium sulfate).
[0060] Calcium sulfate dihydrate (CaSO 4 ·2H 2O) cannot bind water and is therefore not a calcium sulfate binder. However, calcium sulfate dihydrate may also be included in the mortar composition. Calcium sulfate dihydrate may act as a so-called nucleating agent and cause a faster reaction of calcium sulfate hemihydrate. Therefore, the mortar composition preferably contains calcium sulfate dihydrate.
[0061] The mortar composition of the present invention further comprises one or more 3 The lightweight filler is preferably made of an inorganic material (such as glass or a mineral material), which generally contains pores or is a hollow body.
[0062] However, suitable lightweight fillers may also be organic materials, in particular recycled plastics, rubber powder or bio-based lightweight fillers, in particular based on hemp (Hanf), rice husks, wood or cork.
[0063] The apparent density of a particulate material such as a filler is the ratio between the mass of the particulate material and the volume occupied by the individual particles. This volume includes the pores within the particles (internal pore volume), but excludes the cavities between the particles. Thus, unlike the bulk density, the apparent density does not take into account the spaces between the particles of the material. The apparent densities given in this application relate to a temperature of 20°C. The apparent density can be determined according to standard EN 1097-6-2013.
[0064] One or more lightweight fillers, such as those exemplified below, particularly expanded glass, having a mass of less than 1.5 g / cm 3 , preferably less than 1.0g / cm 3 , more preferably less than 0.6 g / cm 3 , especially preferably less than 0.5 g / cm 3 Typically, the apparent density is preferably at least 0.05 g / cm 3 , more preferably at least 0.1 g / cm 3 .
[0065] Examples of suitable inorganic lightweight fillers having the above apparent density are selected from expanded glass, hollow glass spheres, foamed glass slag, hollow aluminum silicate spheres, pumice, expanded clay, expanded shale, expanded perlite, regenerated stone particles, such as lightweight concrete or porous concrete, non-expanded perlite, hollow silicate microspheres or a combination thereof, preferably expanded glass, pumice, expanded perlite, expanded clay, expanded shale or a combination thereof.
[0066] In a preferred embodiment, one or more of the apparent densities are less than 1.5 g / cm 3 The lightweight filler is expanded glass.
[0067] The one or more lightweight fillers, such as those exemplified above, in particular inorganic lightweight fillers, preferably expanded glass, preferably have an average particle size in the range of 0.05 to 16 mm, preferably 0.5 to 10 mm, more preferably 1 to 7 mm, particularly preferably 2 to 4 mm. This applies to all the above-mentioned apparent densities or preferred apparent densities.
[0068] The terms particle diameter and particle size or particle size are synonymous here. Unless otherwise specified, the particle diameter or particle size here refers to the average particle diameter or particle size. The average particle diameter corresponds in particular to the D50 value (50% of the particles are smaller than a given value and 50% are respectively larger than a given value).
[0069] The particle size of fine particles up to a particle size of 3.5 mm can be measured by means of laser diffraction as described in ISO 13320:2009. In particular, a Mastersizer 2000 instrument with a Hydro 2000G dispersion unit and the Mastersizer 2000 software from Malvern Instruments GmbH (Germany) are used. Suitable as a measuring medium is, for example, isopropanol. Preferably, the particle size of non-spherical particles or irregular particles is represented by the equivalent spherical diameter of a sphere with the same volume.
[0070] The particle size of coarse particles with a particle size greater than 3.5 mm can be determined by sieve analysis, for example, as described in the standard ASTM C136 / C136M. In this method, particles of different sizes are separated by sieving the material through a series of sieves with different mesh sizes. The material to be analyzed is shaken through a series of successively decreasing sieves with a single movement or a combination of horizontal, vertical or rotational movements. The result is the percentage of particles that pass through a sieve of a certain size. In principle, sieve analysis is also suitable for determining the particle size of particles below 3.5 mm.
[0071] It is also possible to use two or more materials having an apparent density of less than 1.5 g / cm 3 The invention relates to a sieving curve of a composition of lightweight fillers (especially inorganic lightweight fillers) with different particle size distributions, wherein the lightweight fillers can be of the same type or of different types. Such mixtures can be used to influence, in particular, the strength of the mortar composition and other properties resulting from processing.
[0072] Apparent density is less than 1.5 g / cm 3 The lightweight filler, in particular the inorganic lightweight filler, preferably meets the requirements of DIN EN13055:2016 for lightweight fillers.
[0073] Apparent density is less than 1.5 g / cm 3The particles of the lightweight filler (especially inorganic lightweight filler) can have any spherical and / or non-spherical geometric shape, uniform or non-uniform. The shape of the particles can be, for example, spherical, conical, polygonal, cubic, pentagonal, hexagonal, octagonal, prism-shaped and / or polyhedral. The non-uniform particles can, for example, have a circular, oval, elliptical, square, rectangular, triangular or polygonal cross-section at least partially present therein. "Non-uniform" and "irregular" shaped particles refer to three-dimensional particle shapes in which at least two different cross-sections passing through the particles have different shapes. This also applies to particles with an apparent density of at least 2.0 g / cm 3 The particle geometry of the following fillers.
[0074] The mortar composition further comprises one or more 3 The filler, which is also called aggregate, wherein the apparent density of the filler or fillers is preferably at least 2.2 g / cm 3 .
[0075] As an apparent density of at least 2.0 g / cm 3 , preferably at least 2.2 g / cm 3 As fillers, substances known to the person skilled in the art can be used. Examples are stone, crushed stone, gravel, slag, ground stone, recycled stone particles, recycled concrete, sand such as quartz sand or river sand, ground stone, glass, glass ceramics, porcelain, fused or sintered abrasives, sintering aids, silicon dioxide, carbonates such as ground limestone, ground dolomite and chalk, and / or ground aluminum oxide.
[0076] Solid materials for which (re)utilization possibilities are sought can be used. Such materials have an apparent density of at least 2.0 g / cm 3 Examples of fillers or aggregates are as follows, provided that they have a density of at least 2.0 g / cm 3 The apparent density of:
[0077] (i) Materials of biological origin, preferably materials of plant origin, in particular materials of plant origin consisting essentially of cellulose and / or lignin.
[0078] (ii) inorganic aggregates from the demolition of buildings above and below ground, preferably selected from concrete waste, mortar, bricks, natural stone, asphalt, tiles, ceramic tiles, clinker, metal waste
[0079] (iii) Granular materials which have no health problems and are normally landfilled, such as spent foundry sand, catalyst supports, clinker admixtures, fillers from mining sludge, sewage sludge, liquid manure treatment, paper waste, paper combustion ash, municipal solid waste combustion ash.
[0080] In a preferred embodiment, the apparent density is at least 2.0 g / cm 3 The one or more fillers comprise or are in the form of sand and / or carbonates, in particular calcium carbonate. Suitable sands are described, for example, in standards ASTM C778 or EN 196-1.
[0081] Calcium carbonate also includes limestone or limestone powder and chalk. The sand may in particular be quartz sand or river sand.
[0082] The sieving curve of suitable quartz sand is, for example, in the range of about 0 to 0.5 mm, preferably in the range of about 0.08 to 0.4 mm. The particle size of another suitable quartz sand is, for example, in the range of about 0.1 to 1 mm, preferably in the range of about 0.2 to 0.8 mm.
[0083] Suitable calcium carbonate has, for example, an average particle diameter in the range of about 3 μm and a residual-free particle size distribution curve of about 40 μm. Suitable limestone powder has, for example, a fineness of <0.1 mm.
[0084] In the following, unless stated otherwise, the weight data relating to the one-component or two-component mortar compositions of the invention relate to the dry weight of the entire mortar composition.
[0085] The total amount of the aluminate binder and the calcium sulfate binder in the mortar composition of the present invention is 20 to 65 wt %, preferably 20 to 60 wt %, more preferably 35 to 55 wt %, based on the dry weight of the mortar composition.
[0086] The weight ratio of the aluminate binder to the calcium sulfate binder in the mortar composition is in the range of 1:1 to 1:10, preferably 1:1 to 1:5, more preferably 1:1 to 1:3.5.
[0087] The apparent density of the mortar composition is less than 1.5 g / cm 3 (Preferably the apparent density is less than 1.0 g / cm 3 ) has a light filler content (especially inorganic light filler) of 30 to 70 wt %, preferably 35 to 65 wt %, more preferably 40 to 60 wt %.
[0088] The apparent density of the mortar composition is at least 2.0 g / cm 3 , preferably at least 2.2 g / cm 3 The filler may be contained in an amount of 2 to 20 wt %, preferably 4 to 15 wt %, based on the dry weight of the mortar composition.
[0089] In a preferred embodiment, the mortar composition of the present invention comprises:
[0090] i) 8 to 20% by weight of an aluminate binder,
[0091] ii) 20 to 50 wt. % of a calcium sulfate binder, and
[0092] iii) 35% to 65% by weight have an apparent density of less than 1.5 g / cm 3 , preferably less than 1.0 g / cm 3 One or more inorganic lightweight fillers.
[0093] In a preferred embodiment, the mortar composition further comprises at least one lithium salt, which promotes the curing of the composition. Suitable lithium salts are, for example, lithium sulfate and lithium halides (especially lithium chloride) and lithium carbonate. Most preferred is lithium carbonate.
[0094] Lithium salts (particularly lithium carbonate or lithium sulfate) are preferably contained in the mortar composition in an amount of 0.001% to 0.5%, more preferably 0.003% to 0.05% by weight. Below 0.001%, the concentration is generally too low to produce a significant accelerating effect, while additions exceeding 0.5% by weight result in too fast curing of the composition and / or no additional effect is shown at all and the additive acts more as a filler.
[0095] In a preferred embodiment, the mortar composition may further comprise tartaric acid and / or tartaric acid salt, preferably an alkali metal salt of tartaric acid, preferably in an amount of 0.15 wt % to 0.005 wt %, more preferably 0.1 wt % to 0.01 wt %. Preferred is sodium tartrate or potassium tartrate or a mixed salt of sodium tartrate / potassium tartrate.
[0096] The addition of tartaric acid and / or tartrates has a positive effect on the expansion behavior of the mortar composition by inhibiting excessive expansion of the material. In order to achieve a corresponding effect, at least 0.005% by weight is usually used, while more than 0.15% by weight leads to too severe a delay in setting.
[0097] Other suitable retarders which may be added as an alternative or in addition to tartaric acid and / or tartrate salts are gluconates, in particular sodium gluconate, or citric acid and / or citrate salts, for example sodium citrate.
[0098] In a preferred embodiment, the mortar composition may also contain at least one plasticizer. Plasticizers commonly used in this field may be used. Particularly suitable plasticizers are polycarboxylate ethers (PCEs), also known as "superplasticizers". Polycarboxylate ethers preferably have polyethylene glycol side chains.
[0099] The content of the plasticizer (particularly the polycarboxylate ether) in the mortar composition is preferably in the range of 0.005 wt % to 0.5 wt %, more preferably 0.01 wt % to 0.1 wt %.
[0100] Therefore, in a preferred embodiment, the mortar composition of the present invention may further comprise at least one additive selected from lithium salts, at least one retarder, a plasticizer or a combination thereof, the additive being selected from tartaric acid or tartrate, gluconate, in particular sodium gluconate and citric acid or citrate, the plasticizer being preferably a polycarboxylate ether. These additives are as described above. In a particularly preferred embodiment, the mortar composition comprises lithium salts, tartaric acid or tartrate and a plasticizer, preferably a polycarboxylate ether.
[0101] In addition to the additives mentioned, the mortar composition may also comprise one or more other additives, such as thickeners, dyes and / or pigments, setting retarders, stabilizers, defoamers, shrinkage reducers and / or toughening agents.
[0102] Examples of suitable toughening agents are organic polymers based on vinyl acetate and ethylene, such as those available from Wacker 5025L. Suitable retarders are available, for example, from Sika Schweiz AG under the trade name P is obtained. Examples of suitable pigments are inorganic or organic pigments, such as metal oxides and mixed metal oxides, for example iron oxide.
[0103] Examples of shrinkage-reducing agents are polyols having 2 to 4 hydroxyl groups, preferably glycerol and / or erythritol. It has been found that the use of at least one of the abovementioned polyols can lead to a particularly pronounced reduction in shrinkage.
[0104] The mortar composition may also contain Portland cement, but this is generally not preferred. The mortar composition may, for example, contain up to 5 wt. %, preferably not more than 3 wt. %, more preferably not more than 1 wt. %, in particular not more than about 0.1 wt. % of Portland cement. However, the mortar composition preferably does not contain Portland cement.
[0105] The amounts of the individual components in the mortar composition may also depend on the type of application and the thickness of the layer applied.
[0106] An advantageous embodiment of the mortar composition according to the invention comprises:
[0107] 8 to 20% by weight of an aluminate binder,
[0108] 20 to 50 wt. % of a calcium sulfate binder,
[0109] 35% to 65% by weight have an apparent density of less than 1.5 g / cm 3, preferably less than 1.0g / cm 3 one or more inorganic lightweight fillers, in particular expanded glass,
[0110] 4 to 15 wt. % have an apparent density of at least 2.0 g / cm 3 , preferably at least 2.2 g / cm 3 fillers, in particular sand, for example quartz sand, and / or calcium carbonate, for example chalk and / or limestone,
[0111] 0.01% to 0.10% by weight of a tartrate, in particular potassium sodium tartrate,
[0112] 0.003% to 0.5% by weight of a lithium salt, in particular lithium carbonate or lithium sulfate.
[0113] The present invention also relates to a method for manufacturing a ground structure on a substrate, comprising:
[0114] a) applying a mixture of the mortar composition of the present invention as described above and water to a substrate to form a first leveling layer,
[0115] b) applying a reinforcement layer onto said first screed layer,
[0116] c) applying a mixture of levelling material and water onto the reinforcement layer to form a second levelling layer, and
[0117] d) Optionally applying a floor covering to the second screed.
[0118] What has been said above with regard to the mortar composition of the invention applies in the same manner to the method of the invention.
[0119] The method of the present invention relates to the production of a floor structure on a substrate or base. The substrate is not subject to any restrictions. Since the mortar composition of the present invention used can obtain a lightweight filler, the method of the present invention is particularly suitable for substrates with limited load-bearing capacity. The method of the present invention is particularly suitable for floor renovation, for example.
[0120] Examples of suitable substrates are wooden substrates, concrete, flooring, old substrates with ceramic coverings, old substrates based on flooring or concrete. The substrate can be, for example, a cement-based (e.g. Portland cement) or calcium sulfate-based substrate. The substrate is preferably a wooden substrate, or it is a multilayer substrate comprising a wooden layer, such as a subfloor made of wood with an old substrate thereon.
[0121] Before applying the mortar composition mixed with water according to step a), one or more primers can optionally be arranged on the substrate. The primer is applied to the substrate, for example, by painting. The pretreatment is known to the person skilled in the art. Common primer agents can be used, such as plastic dispersions based on organic binders or two-component primer agents, such as epoxy resin binders. Filled painting primers are also suitable as primers, so that the primer is applied and filled in one process. When it is desired to lay the leveling layer in the form of a floating leveling layer, the substrate can also be provided with a separating layer, such as a PE film.
[0122] In the method according to the invention, the mortar composition according to the invention is mixed with water in step a). Since the mortar composition contains hydraulic binders in the form of aluminate binders and calcium sulfate binders, a known hydration reaction will occur after the addition of water. Due to drying or setting, the mortar composition will cure over time. When the mortar composition is still flowable or pasty, it is applied to an optionally primed substrate.
[0123] The mixing of the two-component mortar composition of the present invention, which consists of component A containing a light filler and component B containing the remaining components of the mortar composition, can be carried out, for example, in the following manner. Component B is mixed with water, for example, for about 60 seconds. Suitable mixing ratios of the mortar composition (including a light filler) and water are as follows. Cold, clean water should be used appropriately. With the agitator running, component A (light filler) is added to the uniform mixture obtained, and stirring is continued for a period of time, for example, about 120 seconds, to obtain a ready-to-use mixture. It is also possible to pour component B mixed with water onto component A (light filler) and then mix the mixture again.
[0124] The consistency or rheological behavior of the mortar composition can be adjusted not only by the choice of the additives used, but also by the mixing ratio of the mortar composition and water. Preferably, the mortar composition is mixed with water in a mass ratio of water to mortar composition in the range of 0.08 to 0.50, preferably 0.10 to 0.40, in particular 0.20 to 0.35. The mortar composition obtained is advantageously pumpable, which facilitates transportation.
[0125] The mortar composition mixed with water is then applied to a substrate which is optionally provided with a primer or a separating layer. Application can be carried out by all means known to the person skilled in the art, for example with a spatula, a rake, a scraper or a roller, by pouring or spraying or spraying, preferably by spatula, a scraper, pouring or a rake. After application, the applied mortar composition is optionally scraped, for example with a scraping spatula. The applied material is usually removed by an introduced calliper and then scraped or "compacted" with a scraping spatula.
[0126] After applying the mortar composition, it is usually necessary to wait for the first layer to be walkable before applying the reinforcing fabric. The first screed layer is in particular a lightweight filler.
[0127] As reinforcing layer, the reinforcements or reinforcements commonly used in the art can be used. The reinforcing layer is a sheet-like textile carrier or preferably comprises a sheet-like textile carrier, such as a fabric, a nonwoven fabric or a paving fabric. Preference is given to systems different from nonwoven fabrics, so that the first leveling layer and the leveling layer (second leveling layer) can be closely meshed with each other. Multidimensional or three-dimensional fabrics or paving fabrics (especially glass fiber fabrics) are also conceivable. The reinforcing layer is a reinforcing fabric or preferably comprises a reinforcing fabric.
[0128] The reinforcing layer is or particularly preferably comprises a sheet-like textile carrier made of glass fibers, for example in the form of a woven, nonwoven or woven fabric, in particular a glass fiber woven or woven glass fiber woven fabric. The glass fibers may have a plastic sheath. The sheet-like textile carrier (for example in the form of a woven, nonwoven or woven fabric) may also be formed from another fiber material, for example from polymer fibers.
[0129] The reinforcing layer is preferably mechanically fixed to the first leveling layer, for example by means of a clamp and / or by means of a reinforcing mortar. Particularly suitable as a reinforcing mortar is a calcium sulfate spread based on a calcium sulfate binder. The calcium sulfate binder of the calcium sulfate spread is particularly selected from hemihydrate calcium sulfate and / or anhydrous calcium sulfate corresponding to the calcium sulfate binder of the mortar composition of the present invention. Preferably, an anti-sagging spread is used, in particular an anti-sagging calcium sulfate spread. It is also conceivable to have a spread comprising a calcium sulfate binder and an aluminate binder as binders, wherein the definitions of these binders have already been described for the mortar composition of the present invention.
[0130] One advantage of the method according to the invention is that the mortar composition according to the invention of the first leveling layer dries quickly, so that after a relatively short drying time according to step b), for example less than 6 hours, preferably less than 4 hours, particularly preferably not more than 2 hours of waiting time, the reinforcing fabric can be fixed and then after another short waiting time (for example about 30 minutes) step c), i.e. applying the second leveling layer, can be continued.
[0131] According to step c) of the method of the invention, a mixture of levelling material and water is applied to the reinforcement layer to form a second levelling layer. Conventional application methods can be used. Examples have been described above for the first levelling layer. The levelling material can be self-levelling or optionally levelled, for example with a levelling spatula.
[0132] In particular, fast-curing systems are used as leveling materials. The leveling material is preferably a calcium sulfate coating material containing a calcium sulfate binder, wherein the calcium sulfate coating material preferably contains a calcium sulfate binder and an aluminate binder. Such calcium sulfate coating materials are preferably used because, on the one hand, they dry quickly and, on the other hand, no primer is required beforehand on the first leveling layer produced, which makes the method particularly economical and simple.
[0133] The calcium sulfate binder of the calcium sulfate spread is particularly selected from hemihydrate calcium sulfate and / or anhydrous calcium sulfate corresponding to the calcium sulfate binder of the mortar composition of the present invention, and reference may be made to the relevant contents thereof. The aluminate binder of the calcium sulfate spread (if present) is particularly selected from calcium aluminate cement and / or calcium sulfoaluminate cement corresponding to the aluminate binder of the mortar composition of the present invention, and reference may be made to the relevant contents thereof. The calcium sulfate spread used as a leveling material generally does not contain calcium sulfate having an apparent density of less than 1.5 g / cm 3 Instead of lightweight fillers, the concrete contains a higher proportion of conventional fillers such as sand and / or calcium carbonate.
[0134] The advantage of the floor structure formed by the first leveling layer, the reinforcing layer and the second leveling layer made of the lightweight filler of the invention is that it cures quickly, so that it is ready for application at the latest 48 hours after the application of the second leveling layer, preferably after the application of the first layer. This refers to a continuous process taking into account the waiting time required for drying. It should be understood that the duration may be longer taking into account the working time and the actual process.
[0135] After the application readiness has been reached, a floor covering can optionally and preferably be applied to the second screed. Conventional floor coverings can be applied. Examples of floor coverings are tiles, laminate, PVC (polyvinyl chloride), linoleum or carpet. The floor covering can be fixed to the second screed in the usual way, for example by gluing.
[0136] The layer thickness of the leveling layer is in principle not restricted. In the following text, the layer thickness refers to the dry layer.
[0137] For example, the first leveling layer can have a layer thickness of at least 15 mm, wherein the layer thickness of the first leveling layer is preferably in the range of 15 to 100 mm, more preferably in the range of 20 to 100 mm. The layer thickness can also depend on whether the leveling layer is laid as an adhesive leveling layer or as a floating leveling layer. When laid as an adhesive leveling layer, the layer thickness is preferably at least 15 mm, and when laid as a floating leveling layer, the layer thickness is preferably at least 25 mm. For example, the second leveling layer can have a layer thickness of at least 6 mm, wherein the layer thickness of the second leveling layer is preferably in the range of 6 to 50 mm, more preferably in the range of 6 to 10 mm.
[0138] A preferred embodiment of the method of the present invention for a floor structure with an adhesive screed comprises:
[0139] - Applying a dispersion primer or a filler primer to the underlying floor structure (especially wooden substrates such as wooden floors),
[0140] - application of the mortar composition according to the invention as a first screed (lightweight filling layer) - preferably with a layer thickness between 15 and 100 mm, the drying time required for application of the reinforcing layer being less than 6 hours, for example after 2 hours (corresponding to the time required for the first screed to be walkable),
[0141] - applying a reinforcing fabric or glass fiber fabric, fixing it with a calcium sulfate coating (e.g. a solid calcium sulfate coating),
[0142] - Applying a calcium sulfate spread as a leveling material for the second leveling layer (eg a fast-curing fine spread) - preferably with a layer thickness of between 6 and 50 mm, but in particular between 6 and 10 mm; the final floor covering can be laid after 48 hours at the latest.
[0143] A preferred embodiment of the method of the present invention for a ground structure with a floating screed comprises:
[0144] - Lay a PE membrane 100 μm (PE = polyethylene) on the underlying ground structure,
[0145] - application of the mortar composition according to the invention as a first levelling layer (lightweight filling layer) - preferably with a layer thickness between 25 and 100 mm, the drying time required for application of the reinforcing layer being less than 6 hours, for example after 2 hours,
[0146] - Apply reinforcement fabric or glass fiber fabric (e.g. PZG), which is fixed with a calcium sulfate coating (e.g. a solid calcium sulfate coating),
[0147] - Applying a calcium sulfate spread as a leveling material for the second leveling layer (eg a fast-curing fine spread) - preferably with a layer thickness of between 6 and 50 mm, but in particular between 6 and 10 mm; the final floor covering can be laid after 48 hours at the latest.
[0148] The floor structure according to the invention is preferably a floor structure, in particular for indoor areas. The floor structure is particularly suitable for the floor of a living room or the sales area of a store, or also for commercial areas.
[0149] Due to the low weight of the floor structure according to the invention, it is particularly suitable for sub-floor structures or substrates with low load-bearing capacity. Preferred fields of application are floor renovation and / or floor structures on wooden substrates or substrates containing a wooden layer.
[0150] The present invention also relates to the use of the one-component or two-component mortar composition of the present invention as described above as a leveling layer, in particular as a lightweight filler.
[0151] The above contents about the mortar composition of the present invention and the method of the present invention are also applicable to the use of the present invention, in particular the design of the mortar composition, the floor structure and the substrate, and reference can be made to the relevant contents.
[0152] The use of the present invention is preferably suitable for producing a floor structure on a substrate, which comprises in sequence a first screed layer made of the one-component or two-component mortar composition of the present invention, a reinforcing layer and a second screed layer, wherein a floor covering is optionally arranged on the second screed layer.
[0153] The use according to the invention is preferably suitable for floor renovation or floor renovation, since in that case the weight of the spread or screed is usually limited due to the load-bearing capacity of the underlying floor structure.
[0154] The use according to the invention is preferably applicable to sub-floor structures made of a wood substrate or to multi-layer substrates comprising a wood layer.
[0155] The use of the invention is particularly suitable for a ground structure according to the invention as described above.
[0156] The present invention also relates to a floor structure on a substrate, which comprises in sequence a first screed layer made of the mortar composition of the present invention as described above, a reinforcing layer and a second screed layer, wherein a floor covering is optionally provided on the second screed layer.
[0157] The above contents about the mortar composition of the present invention, the method of the present invention and the use of the present invention are also applicable to the floor structure of the present invention, in particular the design of the mortar composition, the reinforcing layer, the first and second leveling layers, the floor covering and the substrate, so reference can be made to the relevant contents.
[0158] The ground structure is preferably obtained according to the method of the invention as described above.
[0159] The present invention is explained in detail below by way of examples. The examples are for illustrative purposes and are not intended to limit the present invention in any way.
[0160] Example
[0161] Example 1
[0162] Mortar composition
[0163] A two-component mortar composition consisting of components A and B was prepared according to the following formulation.
[0164] Component A:
[0165]
[0166] Component B:
[0167] <![CDATA[Expanded glass, particle size 2 - 4 mm, apparent density: approximately 0.32 g / cm 3 > 100
[0168] Component A and component B were mixed in a ratio of 50 wt % of component A and 50 wt % of component B. The obtained mortar composition had the following composition.
[0169] Mortar composition
[0170]
[0171] Example 2 and Comparative Example 1
[0172] The mortar composition of Example 1 was used to manufacture a floor structure on a gypsum board (or concrete substrate) as a substrate in the following manner (Example 2):
[0173] -Mix the mortar composition of Example 1 with water (ratio 100 kg mortar composition / 16.4 l water)
[0174] - Apply the mixture to the substrate in the layer thickness indicated in Table 1
[0175] - Approximately 2 hours after the mixture is applied, the reinforcing fabric (fiberglass fabric) is laid and fixed with a calcium sulfate spreader
[0176] - After about 2 hours, apply a levelling agent (calcium sulfate coating) to the fabric with a layer thickness of about 8 mm
[0177] A floor structure was produced on a gypsum board as a substrate using a commercially available cement-based dry mortar for lightweight fillers (including lightweight admixtures of expanded polystyrene) in the following manner (Comparative Example 1):
[0178] - Mix dry mortar with water (ratio 100kg dry mortar / 47.6-52.4l water)
[0179] - Apply the mixture to the substrate in the layer thickness indicated in Table 1
[0180] - Lay the glass fiber nonwoven fabric about 4 hours after applying the mixture
[0181] - After about 48 hours a thin coating of cement was applied to the nonwoven with a layer thickness of about 8 mm.
[0182] The properties of the floor structures according to Example 2 and Comparative Example 1 were tested. The results are listed in Table 1. The tests were carried out on the mortar composition of the invention ("filling layer" in Table 1) or the entire floor structure ("system" in Table 1).
[0183] The following test methods were used:
[0184] Apparent density: According to DIN EN 1015-10
[0185] Flexural strength / compressive strength: According to DIN EN 13892-2
[0186] Chair Roll Tester: According to ASTM C627
[0187] Bond tensile strength: According to DIN EN 13892-8
[0188] Pot life 2: After mixing the mortar composition of Example 2 or the dry mortar of Comparative Example 1 with water for 20 minutes, a small surface was formed with the mixture every 5 minutes and tested with a hammer on the next day. When the surface is broken: the pot life ends (TZ end point)
[0189]
[0190]
Claims
1. A one-component or two-component mortar composition, comprising: i) an aluminate binder selected from calcium aluminate cement and / or calcium sulphoaluminate cement, ii) a calcium sulfate binder selected from calcium sulfate hemihydrate and / or anhydrous calcium sulfate, iii) one or more apparent densities of at least 2.0 g / cm 3 of fillers, and iv) One or more apparent densities less than 1.5 g / cm 3 Lightweight fillers, especially inorganic lightweight fillers, The apparent density is less than 1.5g / cm 3 The amount of lightweight filler, in particular inorganic lightweight filler, is 30 wt % to 70 wt %, and the total amount of aluminate binder and calcium sulfate binder is 20 wt % to 65 wt %, wherein the weight ratio of aluminate binder to calcium sulfate binder is in the range of 1:1 to 1:10, wherein the weight data are based on the dry weight of the mortar composition.
2. The one-component or two-component mortar composition according to claim 1, wherein the apparent density is less than 1.5 g / cm 3 The content of lightweight fillers, especially inorganic lightweight fillers, is 35 to 65 wt %, preferably 40 to 60 wt %, based on the dry weight of the mortar composition.
3. A one-component or two-component mortar composition according to any one of the preceding claims, wherein the apparent density is less than 1.5 g / cm 3 The one or more lightweight fillers are selected from expanded glass, hollow glass balls, foamed glass slag, hollow aluminum silicate balls, pumice, expanded clay, expanded shale, expanded perlite, regenerated stone particles, non-expanded perlite, hollow silicate microspheres, recycled plastics, rubber powder, bio-based lightweight fillers, especially based on hemp, rice husk, wood or cork, or a combination thereof, wherein expanded glass, pumice, expanded perlite, expanded clay, expanded shale or a combination thereof is preferred.
4. The one-component or two-component mortar composition according to any one of the preceding claims, wherein the apparent density is less than 1.5 g / cm 3 The one or more lightweight fillers, in particular expansion glass, have an average particle size in the range of 0.05 to 16 mm, preferably 0.5 to 10 mm, more preferably 1 to 7 mm, particularly preferably 2 to 4 mm.
5. A one-component or two-component mortar composition according to any one of the preceding claims, wherein the apparent density is at least 2.0 g / cm 3 The content of the filler is 2 to 20 wt %, preferably 4 to 15 wt %, based on the dry weight of the mortar composition.
6. A one-component or two-component mortar composition according to any one of the preceding claims, wherein the apparent density is at least 2.0 g / cm 3 The one or more fillers include sand and / or calcium carbonate, wherein the calcium carbonate is preferably chalk and / or limestone powder.
7. A one-component or two-component mortar composition according to any one of the preceding claims, wherein the total amount of aluminate binder and calcium sulfate binder is 20 to 60 wt. %, preferably 35 to 55 wt. %, based on the dry weight of the mortar composition, and / or The mortar composition further comprises at least one additive selected from lithium salts, at least one retarder selected from tartaric acid or tartrates, gluconates, in particular sodium gluconate, and citric acid or citrates, a plasticizer, preferably a polycarboxylate ether, or a combination thereof.
8. Use of the one-component or two-component mortar composition according to any one of claims 1 to 7 as a leveling layer, in particular as a lightweight filler.
9. Use of the one-component or two-component mortar composition according to any one of claims 1 to 7 for preparing a ground structure, the ground structure comprising, in sequence, a first leveling layer, in particular a lightweight filling layer, a reinforcement layer and a second leveling layer made of the one-component or two-component mortar composition according to any one of claims 1 to 7, wherein a ground covering is optionally arranged on the second leveling layer.
10. Use of the one-component or two-component mortar composition according to any one of claims 1 to 7 in floor renovation and / or on a wooden substrate or a multi-layer substrate comprising a wooden layer.
11. A method for producing a ground structure on a substrate, include: a) applying a mixture of the mortar composition according to any one of claims 1 to 7 and water to the substrate to form a first leveling layer, b) applying a reinforcement layer onto said first screed layer, c) applying a mixture of leveling material and water onto the reinforcement layer to form a second leveling layer, and d) Optionally applying a floor covering to the second screed.
12. The method according to claim 11, wherein The reinforcing layer comprises a sheet-like textile carrier, in particular a sheet-like textile carrier made of glass fibers, particularly preferably a glass fiber fabric, and / or The leveling material is a calcium sulfate coating material, wherein the calcium sulfate coating material comprises a calcium sulfate binder, preferably a calcium sulfate binder and an aluminate binder.
13. The method according to claim 11 or 12, wherein The layer thickness of the first levelling layer is in the range of 15 to 100 mm, preferably 20 to 100 mm, and / or The layer thickness of the second leveling layer is in the range from 6 to 50 mm, preferably from 6 to 10 mm.
14. A floor structure on a substrate, the floor structure comprising, in sequence, a first screed layer made of the mortar composition according to any one of claims 1 to 7, a reinforcing layer and a second screed layer, wherein a floor covering is optionally arranged on the second screed layer.
15. Ground structure according to claim 14, obtained by a method according to any one of claims 11 to 13.
Citation Information
Cited By
Gypsum-based plastering mortar material, preparation method thereof and gypsum-based plastering mortar
CN119751006A