Emulsion polymerization with acetone acetal (meth) acrylate

By using free radical emulsion polymerization technology to adjust pH value using alkaline compounds under acidic reaction conditions, aqueous polymer latex was successfully prepared, solving the problems of polymer latex performance and application in acidic environments, and improving product stability and application potential.

CN118974113APending Publication Date: 2024-11-15BASF SE
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202380031172.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-21
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, when preparing aqueous polymer latex containing acetonitrile (meth)acrylate as monomer, it is difficult to maintain an appropriate pH value in an acidic environment, affecting the performance and application of the polymer.

Method used

In the presence of an acidic radical polymerization initiator in the aqueous polymerization medium, radical emulsion polymerization is selectively carried out with the help of basic compounds, maintaining a pH between 6 and 8, ensuring the neutral environment of the polymerization process.

Benefits of technology

The successful preparation of aqueous polymer latex under acidic reaction conditions has been achieved, and the stability and application potential of the product have been improved, especially in the fields of coatings, films, paints and adhesives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005063747150000191
    Figure BDA0005063747150000191
Patent Text Reader

Abstract

A process for preparing an aqueous polymer latex by polymerizing a monomer composition containing acetone acetal (meth) acrylate, optionally in the presence of a seed latex, in an aqueous polymerization medium in the presence of an acidic reactive free radical polymerization initiator, wherein the monomer composition comprises a) from 0.1% to 100% by weight of acetone acetal (meth) acrylate, b) from 0% to 99.9% by weight of one or more additional ethylenically unsaturated monomers, characterized in that the monomer composition comprises a) from 0.1% to 100% by weight of acetone acetal (meth) acrylate, b) from 0% to 99.9% by weight of one or more additional ethylenically unsaturated monomers, by the presence of a basic compound, a substantially neutral pH in the range of 6 to 8 is maintained in the aqueous polymerization medium during the free radical emulsion polymerization reaction.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for preparing an aqueous polymer latex containing solketal (meth)acrylate as a monomer by free radical emulsion polymerization, and the aqueous polymer latex obtained thereby and its use.

[0002] Acrylic acid glyceryl acetonate (also known as methyl acrylate (2,2-dimethyl-1,3-dioxolan-4-yl) ester, IPGA) is known as a reactive diluent in curable compositions such as printing inks, preferably inkjet printing inks. Acrylic acid glyceryl acetonate can be prepared by transesterification of ethyl acrylate with glyceryl acetonate as described in WO2018 / 146258.

[0003] Glyceryl (meth)acrylate acetonide has become increasingly interesting as a monomer for the preparation of aqueous polymer latexes for various applications such as aqueous coatings, films and paints and also various adhesives by free radical emulsion polymerization. Further fields of application of polymer latexes are, for example, pigment printing, road markings, ground or oil drilling fluids.

[0004] Zhen et al., Atom Transfer Radical Polymerization of Solketal Acrylate Using Cyclohexanone as the Solvent, Macromolecular Chemistry and Physics 206(5), pp. 607-612, describes homopolymerization of glyceryl acrylate by atom transfer radical polymerization (ATRP) using CuBr / pentamethyldiethylenetriamine as catalyst and cyclohexanone as solvent. The prepared bromine-terminated homopolymer was used as a macroinitiator to initiate polymerization of tert-butyl acrylate under similar ATRP conditions, resulting in a diblock copolymer with controlled molecular weight and low polydispersity.

[0005] Pham et al., Glycerol-based co-oligomers by free-radical chain transfer polymerization: Towards reactive polymers bearing acetal and / or carbonate groups with enhanced properties, European Polymer Journal 95 (2017), pp. 491-502, reported the synthesis of solvent-soluble oligomers from glycerol acrylate carbonate and glyceryl acrylate acetonide by free radical chain transfer polymerization using 2-mercaptoethanol as a chain transfer agent.

[0006] WO 2017 / 191167 discloses an aqueous polymer latex used as a binder in an aqueous coating composition containing titanium dioxide pigment. The aqueous polymer latex is obtained by polymerizing a monomer composition M by free radical emulsion polymerization using a specific feeding method, wherein the monomer composition M consists of:

[0007] a) 80% to 99.95% by weight, based on the total weight of the monomer composition M, of an ethylenically unsaturated monomer M1 selected from a mixture of at least one C1-C1-4-hydroxy-2-nitropropene selected from acrylic acid; 20 Alkyl esters and C5-C methacrylate 20 alkyl ester monomers M1a; and at least one monomer M1b selected from vinyl aromatic monomers and C1-C4 alkyl esters of methacrylic acid;

[0008] b) 0.05 to 5% by weight, based on the total weight of the monomer composition M, of one or more monoethylenically unsaturated monomers M2 selected from monoethylenically unsaturated monocarboxylic acids having 3 to 6 carbon atoms and monoethylenically unsaturated dicarboxylic acids having 4 to 6 carbon atoms;

[0009] c) 0 to 20% by weight of nonionic monomers M3 which are different from the monomers M1, such as hydroxy-C2-C4-alkyl esters of acrylic acid and methacrylic acid.

[0010] The waterborne polymer latex is used as a binder in the waterborne coating composition containing titanium dioxide pigment.

[0011] The free radical initiated aqueous emulsion polymerization is triggered by a free radical polymerization initiator (free radical initiator). These are in principle peroxides, persulfates, azo compounds and redox initiator systems. The peroxides can be inorganic peroxides or organic peroxides. Some free radical polymerization initiators, especially inorganic persulfates, make the reaction acidic when they come into contact with water: when dissolved in an aqueous reaction medium, especially at elevated temperatures, they produce an acidic pH below 6.

[0012] An object of the present invention is to provide a method for preparing an aqueous polymer latex containing glyceryl (meth)acrylate acetonide as a monomer by free radical emulsion polymerization using an acidic reaction polymerization initiator such as persulfate.

[0013] The problem is solved by a method for preparing an aqueous polymer latex by polymerizing a monomer composition containing glyceryl (meth)acrylate acetonide by free radical emulsion polymerization in an aqueous polymerization medium in the presence of an acidic reactive free radical polymerization initiator, optionally in the presence of a seed latex, wherein the monomer composition comprises

[0014] a) 0.1 to 100% by weight of glyceryl (meth)acrylate acetonide,

[0015] b) 0 to 99.9% by weight of one or more further ethylenically unsaturated monomers,

[0016] Characterized in that a substantially neutral pH in the range of 6 to 8 is maintained in the aqueous polymerization medium during the free radical emulsion polymerization by the presence of a basic compound.

[0017] Glyceryl (meth)acrylate is an abbreviation of glyceryl acrylate and glyceryl methacrylate. Glyceryl acrylate is preferred.

[0018] The additional ethylenically unsaturated monomers may be selected from the group consisting of C1-C1 20 The alkyl esters form group b1).

[0019] Terminology C1-C 20The alkyl group represents a group of linear or branched or cyclic saturated hydrocarbon groups having 1 to 20 carbon atoms. Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, pentyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, 2,2-dimethylpropyl, 1-ethylpropyl, hexyl, 1,1-dimethylpropyl, 1,2-dimethylpropyl, 1-methylpentyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, 1,1-dimethylbutyl, 1,2-dimethylbutyl, 1,3-dimethylbutyl, 2,2-dimethylbutyl, 2,3-dimethylbutyl, 3,3-dimethylbutyl, 1-ethylbutyl, 2-ethylbutyl, 1,1,2-trimethylpropyl, 1,2,2-trimethylpropyl, 1-ethyl-1-methylpropyl, 1-ethyl-2-methylpropyl, n-heptyl, 2-heptyl, n-octyl cyclopentyl, cyclohexyl, methylcyclohexyl, dimethylcyclohexyl, cycloheptyl, cyclooctyl, cyclododecyl, cyclohexadecyl, norbornyl (= bicyclo[2.2.1]heptyl) and isobornyl (= 1,7,7-trimethylbicyclo[2.2.1]heptyl).

[0020] In particular, tert-butyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-propylheptyl (meth)acrylate, cyclohexyl (meth)acrylate, n-octyl (meth)acrylate, 2-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, methyl (meth)acrylate are used as monomer b1). (Meth)acrylate is an abbreviation for acrylate and methacrylate.

[0021] The further ethylenically unsaturated monomers may be selected from the group b2) consisting of vinyl esters, in particular vinyl acetate, vinyl propionate, vinyl laurate, vinyl neodecanoate, vinyl versatate and vinyl 2-ethylhexanoate.

[0022] Further ethylenically unsaturated monomers may be selected from group b3) consisting of vinyl aromatic monomers, in particular styrene.

[0023] The additional ethylenically unsaturated monomers may be selected from the group b4) consisting of:

[0024] - monoethylenically unsaturated monocarboxylic acids having 3 to 6 carbon atoms, such as acrylic acid, methacrylic acid, crotonic acid, 2-ethylacrylic acid, 2-propylacrylic acid, 2-acryloyloxyacetic acid and 2-methacryloyloxyacetic acid;

[0025] - monoethylenically unsaturated dicarboxylic acids having 4 to 6 carbon atoms, such as itaconic acid, citraconic acid, maleic acid and fumaric acid;

[0026] - half esters of monoethylenically unsaturated dicarboxylic acids having 4 to 6 carbon atoms with C1-C4-alkanols, such as methanol or ethanol, such as half esters of itaconic acid, citraconic acid, maleic acid or fumaric acid with methanol or ethanol;

[0027] - monoethylenically unsaturated sulfonic acids, such as vinylsulfonic acid, allylsulfonic acid, styrenesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid;

[0028] - monoethylenically unsaturated phosphonic acids, such as vinylphosphonic acid, allylphosphonic acid, styrenephosphonic acid and 2-acrylamido-2-methylpropanephosphonic acid; and

[0029] - monoethylenically unsaturated phosphoric acids, such as the monophosphates of hydroxyalkyl acrylates, the monophosphates of hydroxyalkyl methacrylates, the monophosphates of alkoxylated hydroxyalkyl acrylates and the monophosphates of alkoxylated hydroxyalkyl methacrylates, in particular the monophosphates of hydroxyethyl acrylate, hydroxypropyl acrylate or hydroxybutyl acrylate, the monophosphates of hydroxyethyl methacrylate, hydroxypropyl methacrylate or hydroxybutyl methacrylate, the monophosphates of ethoxylated hydroxy-C2-C4-alkyl acrylates, the monophosphates of propoxylated hydroxy-C2-C4-alkyl acrylates, the monophosphates of ethoxylated hydroxy-C2-C4-alkyl methacrylates and the monophosphates of propoxylated hydroxy-C2-C4-alkyl methacrylates.

[0030] Preferred monomers b4) are acrylic acid, methacrylic acid, maleic acid, half-methyl maleate, half-ethyl maleate, citraconic acid, half-methyl citraconic acid, itaconic acid, half-methyl itaconic acid, fumaric acid, half-methyl fumarate and half-ethyl fumarate.

[0031] The additional ethylenically unsaturated monomers may be selected from the group b5) consisting of:

[0032] - primary amides of monoethylenically unsaturated monocarboxylic acids having 3 to 8 carbon atoms, such as acrylamide and methacrylamide;

[0033] - an N-C1-C2-carboxylic acid of a monoethylenically unsaturated monocarboxylic acid having 3 to 6 carbon atoms 10 Alkylamides, especially acrylic or methacrylic acid N-C1-C 10Alkylamides such as N-methylacrylamide, N-ethylacrylamide, N-propylacrylamide, N-isopropylacrylamide, N-butylacrylamide, N-methylmethacrylamide, N-ethylmethacrylamide, N-propylmethacrylamide, N-isopropylmethacrylamide and N-butylmethacrylamide;

[0034] -N-hydroxy-C1-C2-hydroxy-monoethylenically unsaturated monocarboxylic acid having 3 to 6 carbon atoms 10 Alkylamides, especially N-hydroxy-C1-C2- 10 Alkylamides, such as N-hydroxymethyl acrylamide, monoethylenically unsaturated monomers with urea or keto groups, such as 2-(2-oxo-imidazolidin-1-yl)ethyl (meth)acrylate, 2-ureido (meth)acrylate, N-[2-(2-oxooxazolidin-3-yl)ethyl]methacrylate, acetoacetoxyethyl acrylate, acetoacetoxypropyl methacrylate, acetoacetoxybutyl methacrylate, 2-(acetoacetoxy)ethyl methacrylate, diacetone acrylamide (DAAM) and diacetone methacrylamide;

[0035] - hydroxyalkyl esters of monoethylenically unsaturated C3-C6-monocarboxylic acids, in particular hydroxyalkyl acrylates and methacrylates (hereinafter also referred to as hydroxyalkyl (meth)acrylates), in particular hydroxy-C2-C4-alkyl acrylates and hydroxy-C2-C4-alkyl methacrylates, such as 2-hydroxyethyl acrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl methacrylate and 4-hydroxybutyl methacrylate; and

[0036] - Monoethylenically unsaturated monomers carrying at least one tri-C1-C4-alkoxysilane group, such as vinyltrimethoxysilane, vinyltriethoxysilane, methacryloxyethyltrimethoxysilane, methacryloxyethyltriethoxysilane.

[0037] Preferred monomers b5) are acrylamide, methacrylamide, N-methylolacrylamide, 2-hydroxyethyl acrylate, ureido methacrylate and 4-hydroxybutyl acrylate.

[0038] The additional ethylenically unsaturated monomers may be selected from the group b6) consisting of:

[0039] - diesters of monoethylenically unsaturated C3-C6-monocarboxylic acids with saturated aliphatic or cycloaliphatic diols, in particular diesters of acrylic acid or methacrylic acid, such as the diacrylates and dimethacrylates of ethylene glycol (1,2-ethanediol), propylene glycol (1,2-propylene glycol), 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol (2,2-dimethyl-1,3-propanediol) and 1,2-cyclohexanediol;

[0040] - monoesters of monoethylenically unsaturated C3-C6 monocarboxylic acids with monoethylenically unsaturated aliphatic or alicyclic monohydroxy compounds, such as acrylic and methacrylic esters of vinyl alcohol (ethenol), allyl alcohol (2-propen-1-ol), 2-cyclohexen-1-ol or norbornene alcohol; and

[0041] - divinylaromatic compounds, such as 1,3-divinylbenzene and 1,4-divinylbenzene.

[0042] In some embodiments, the monomer composition comprises

[0043] a) 1 to 99% by weight of glyceryl (meth)acrylate acetonide,

[0044] b) 1 to 99% by weight of one or more additional ethylenically unsaturated monomers.

[0045] In some specific embodiments, the monomer composition comprises

[0046] a) 5 to 50% by weight of glyceryl (meth)acrylate acetonide,

[0047] b) 50 to 95% by weight of one or more additional ethylenically unsaturated monomers.

[0048] In some other specific embodiments, the monomer composition comprises

[0049] a) 1 to 20% by weight of glyceryl (meth)acrylate acetonide,

[0050] b) 80 to 99% by weight of one or more additional ethylenically unsaturated monomers.

[0051] In some other specific embodiments, the monomer composition comprises

[0052] a) 50 to 95% by weight of glyceryl (meth)acrylate acetonide,

[0053] b) 5 to 50% by weight of one or more additional ethylenically unsaturated monomers.

[0054] In some other specific embodiments, the monomer composition comprises

[0055] a) 80 to 99% by weight of glyceryl (meth)acrylate acetonide,

[0056] b) 1 to 20% by weight of one or more additional ethylenically unsaturated monomers.

[0057] In some embodiments, the additional ethylenically unsaturated monomer is selected from one or more of the groups b1), b2), b3), b4), b5), and b6).

[0058] The process for preparing the polymer latex is carried out according to the well-known free radical emulsion polymerization technique. The conditions required for carrying out the free-radical emulsion polymerization of the monomers are sufficiently familiar to the person skilled in the art, for example from the prior art cited at the outset and from the following documents: "Emulsions-polymerisation" [Emulsion Polymerization] in Encyclopedia of Polymer Science and Engineering, Vol. 8, pp. 659 ff. (1987); DC Blackley, High Polymer Latices, Vol. 1, pp. 35 ff. (1966); H.Warson, The Applications of Synthetic Resin Emulsions [Applications of Synthetic Resin Emulsions], Chapter 5, pp. 246 ff. (1972); D.Diederich, Chemie in unserer Zeit [Current Chemistry] 24, pp. 135 to 142 (1990); Emulsion Polymerisation [Emulsion Polymerization], Interscience Publishers, New York (1965); DE-A 40 03 422 and Dispersionen synthetischer Hochpolymere [Dispersions of Synthetic High Polymers], F. Holscher, Springer-Verlag, Berlin (1969).

[0059] However, according to the present invention, the free radical emulsion polymerization must be carried out by maintaining a substantially neutral pH of pH 6 to 8, preferably pH 6.5 to 7.5, in the aqueous polymerization medium during the polymerization reaction by the presence of a basic compound in the aqueous polymerization medium.

[0060] The free-radically initiated aqueous emulsion polymerization is initiated by free-radical polymerization initiators (free-radical initiators). These are in principle peroxides, persulfates, azo compounds and redox initiator systems.

[0061] According to the invention, the free radical polymerization initiator is an acidic reaction polymerization initiator which, when dissolved in water, generally leads to an acidic pH of <6, preferably ≤4, for example 2 to 4. The free radical polymerization initiator renders the reaction acidic, in particular at elevated temperatures.

[0062] Preferred acidic reacting free radical polymerization initiators for use according to the present invention are persulfates. Preferred persulfates are sodium persulfate, potassium persulfate and ammonium persulfate. They are inexpensive and commonly used in industrial processes.

[0063] Typically, the substantially neutral pH of the aqueous polymerization medium is maintained by adding a basic compound to the aqueous polymerization medium during the polymerization reaction.In some embodiments of the present methods, a partial or full amount of the basic compound is initially charged to the reaction vessel with the aqueous polymerization medium.

[0064] Preferably, the basic compound is selected from water-soluble hydroxides, oxides, carbonates, hydrogen carbonates (bicarbonates), acetates, citrates, borates, phosphates, hydrogen phosphates of alkali or alkaline earth metals or ammonium. Other basic compounds are also possible, like ammonia or water-soluble organic amines such as lower aliphatic amines.

[0065] Preferred alkaline compounds are sodium, potassium and ammonium hydroxides, sodium and potassium carbonates and sodium and potassium bicarbonates (bicarbonates).

[0066] The basic compound is preferably dissolved in water.

[0067] In the embodiment, the polymerization vessel is initially fully charged with the amount of free radical initiator used for the emulsion polymerization. However, it is preferred that no or only a portion (e.g. not more than 40%, especially not more than 15%, by weight based on the total amount of free radical initiator required in the aqueous polymerization medium) of the acidic reaction free radical initiator is charged.

[0068] If necessary, the polymerization vessel may also be initially charged with a basic compound or a portion of the basic compound to achieve a substantially neutral pH in the aqueous reaction mixture of between 6 and 8. This is generally not necessary if no free radical initiator is charged and the pH of the reaction mixture initially charged is already between pH 6 and 8. The entire amount or any remaining amount of the basic component is then added in one or more portions, depending on consumption, or continuously at a constant or varying flow rate during the free radical emulsion polymerization of the monomers under polymerization conditions to maintain a substantially neutral pH in the aqueous polymerization medium of between 6 and 8.

[0069] Preferably, the basic compound is dissolved in water and added as an aqueous solution as described above.

[0070] In another preferred embodiment, the free radical aqueous emulsion polymerization of the present invention is carried out at a temperature in the range of 0° C. to 170° C., more preferably in the range of 50° C. to 100° C., most preferably in the range of 60° C. to 100° C., and in particular, the free radical aqueous emulsion polymerization of the present invention is carried out at a temperature in the range of 70° C. to 100° C. The free radical aqueous emulsion polymerization may be carried out at a pressure less than, equal to or greater than 1 atm (101325 Pa).

[0071] In certain embodiments, the polymerization is carried out in the presence of a chain transfer agent. The chain transfer agent is selected from the group consisting of aliphatic and / or aromatic aliphatic halogen compounds, such as n-butyl chloride, n-butyl bromide, n-butyl iodide, dichloromethane, dichloroethane, chloroform, bromoform, bromotrichloromethane, dibromodichloromethane, carbon tetrachloride, carbon tetrabromide, benzyl chloride, benzyl bromide; organic thio compounds, such as primary, secondary or tertiary aliphatic mercaptans, such as ethanethiol, n-propyl mercaptan, 2-propyl mercaptan, n-butyl mercaptan, 2-butyl mercaptan, 2-methyl-2-propyl mercaptan, n-pentyl mercaptan, 2-pentyl mercaptan, 3-pentyl mercaptan, 2-methyl-2-butyl mercaptan, 3-methyl-2-butyl mercaptan, n-hexyl mercaptan, 2-hexyl mercaptan, 3-hexyl mercaptan, 2-methyl-2-pentyl mercaptan, 3-methyl-2-pentyl mercaptan, 4-methyl -2-pentanethiol, 2-methyl-3-pentanethiol, 3-methyl-3-pentanethiol, 2-ethylbutanethiol, 2-ethyl-2-butanethiol, n-heptanethiol and isomeric compounds thereof, n-octanethiol and isomeric compounds thereof, n-nonanethiol and isomeric compounds thereof, n-decanethiol and isomeric compounds thereof, n-undecanethiol and isomeric compounds thereof, n-dodecanethiol and isomeric compounds thereof, n-tridecanethiol and isomeric compounds thereof; substituted thiols, for example 2-hydroxyethanethiol; aromatic thiols, for example benzenethiol, o-, m- or p-methylbenzenethiol; alkyl esters of thioglycolic acid (thioglycolic acid), for example 2-ethylhexyl thioglycolate; alkyl esters of mercaptopropionic acid, for example octyl mercaptopropionate; and also Polymer Handbook [Polymer Handbook], 3rd edition, 1989, J. Brandrup and EH Immergut, John Wiley & Sons [John Wiley & Sons Publishing Company], Section II, pages 133 to 141; and aliphatic and / or aromatic aldehydes, such as acetaldehyde, propionaldehyde and / or benzaldehyde; unsaturated fatty acids, such as oleic acid; dienes with non-conjugated double bonds, such as divinylmethane or vinylcyclohexane; or hydrocarbons with easily abstractable hydrogen atoms, for example toluene.

[0072] Typically, the total amount of chain transfer agent (if present) does not exceed 1% by weight, based on the total amount of monomers.

[0073] Typically, free radical emulsion polymerization is carried out in the presence of a surfactant. The surfactant can be selected from emulsifiers and protective colloids. Relative to emulsifiers, protective colloids are understood to mean polymeric compounds with a molecular weight higher than 2000 daltons, while emulsifiers typically have lower molecular weights. The surfactant can be an anionic or nonionic surfactant or a mixture of a nonionic and anionic surfactant.

[0074] Anionic surfactants usually carry at least one anionic group selected from phosphate, phosphonate, sulfate and sulfonate groups. Anionic surfactants carrying at least one anionic group are typically used in the form of their alkali metal salts (especially their sodium salts) or in the form of their ammonium salts.

[0075] In a preferred embodiment, the anionic surfactant is an anionic emulsifier, in particular with at least one sulfate or sulfonate group. Likewise, an anionic emulsifier with at least one phosphate or phosphonate group can be used as the sole anionic emulsifier or in combination with one or more anionic emulsifiers with at least one sulfate or sulfonate group. Examples of anionic emulsifiers with at least one sulfate or sulfonate group are, for example, alkyl sulfates, in particular C8-C12 sulfates. 22 Salts of alkyl esters, especially alkali metal salts and ammonium salts; sulfuric acid monoesters of ethoxylated alkanols, especially ethoxylated C8-C 22 Salts of sulfuric acid monoesters of alkanols, preferably with an ethoxylation level (EO level) in the range of 2 to 40, especially alkali metal salts and ammonium salts; sulfuric acid monoesters of ethoxylated alkylphenols, especially ethoxylated C4-C 18 Salts of sulfuric acid monoesters of alkylphenols (EO level: preferably 3 to 40), especially alkali metal salts and ammonium salts; alkylsulfonic acids, especially C8-C 22 Salts of alkylsulfonic acids, especially alkali metal and ammonium salts; dialkyl esters of sulfosuccinic acid, especially di-C1-C 18 Salts of alkyl esters, especially alkali metal and ammonium salts; alkylbenzenesulfonic acids, especially C4-C 22 Salts of alkylbenzenesulfonic acids, especially the alkali metal and ammonium salts; and mono- or di-sulfonated alkyl-substituted diphenyl ethers, for example with C4-C 24 Salts of alkyl bis(benzenesulfonic acid) ethers, especially alkali metal and ammonium salts. Examples are described in US Pat. No. 4,269,749 and are 2A1 (Dow Chemical Company).

[0076] In a particularly preferred embodiment, the anionic surfactant is an anionic emulsifier selected from the following group:

[0077] Alkyl sulfate, especially C8-C 22 Salts of alkyl esters, especially alkali metal and ammonium salts,

[0078] Sulfate monoesters of ethoxylated alkanols, especially ethoxylated C8-C 22 Salts, especially alkali metal salts, of sulfuric acid monoesters of alkanols, preferably having an ethoxylation level (EO level) in the range of 2 to 40,

[0079] Sulfate monoesters of ethoxylated alkylphenols, especially ethoxylated C4-C 18 Sulfate monoesters of alkylphenols (EO level: preferably 3 to 40), alkylbenzenesulfonic acids, especially C4-C 22 Alkylbenzene sulfonic acid, and

[0080] Mono- or di-sulfonated alkyl-substituted diphenyl ethers, e.g., with C4-C 24 Alkyl bis(benzenesulfonic acid) ethers.

[0081] Examples of anionic emulsifiers with phosphate or phosphonate groups include, but are not limited to, the following salts selected from the group consisting of:

[0082] Mono- and di-alkyl phosphates, especially C8-C 22 Salts of alkyl phosphates, especially alkali metal and ammonium salts,

[0083] Phosphoric acid monoesters of C2-C3 alkoxylated alkanols (preferably having an alkoxylation level in the range of 2 to 40, especially in the range of 3 to 30), for example ethoxylated C8-C 22 Phosphoric acid monoesters of alkanols (preferably having an ethoxylation level (EO level) in the range of 2 to 40), propoxylated C8-C 22 Phosphoric acid monoesters of alkanols, preferably having a propoxylation level (PO level) in the range of 2 to 40, and ethoxylated-co-propoxylated C8-C 22 Salts, especially alkali metal and ammonium salts, of phosphoric acid monoesters of alkanols, preferably with an ethoxylation level (EO level) in the range of 1 to 20 and a propoxylation level of 1 to 20,

[0084] Phosphoric acid monoesters of ethoxylated alkylphenols, especially ethoxylated C4-C 18 Salts of phosphoric acid monoesters of alkylphenols (EO level: preferably 3 to 40), especially alkali metal and ammonium salts,

[0085] Alkylphosphonic acid, especially C8-C 22 Salts of alkylphosphonic acids, especially alkali metal and ammonium salts, and

[0086] Alkylbenzenephosphonic acid, especially C4-C 22 Salts of alkylbenzenephosphonic acids, especially the alkali metal and ammonium salts.

[0087] Further suitable anionic surfactants can be found in Houben-Weyl, Methoden der organischen Chemie [Methods of Organic Chemistry], Volume XIV / 1, Makromolekulare Stoffe [Macromolecular Substances], Georg-Thieme-Verlag, Stuttgart, 1961, pages 192-208.

[0088] In other preferred embodiments, the surfactant comprises at least one anionic emulsifier with at least one sulfate or sulfonate group. At least one anionic emulsifier with at least one sulfate or sulfonate group can be the only type of anionic emulsifier. However, a mixture of at least one anionic emulsifier with at least one sulfate or sulfonate group and at least one anionic emulsifier with at least one phosphate or phosphonate group can also be used. In such a mixture, the amount of at least one anionic emulsifier with at least one sulfate or sulfonate group is preferably at least 50% by weight, based on the total weight of the anionic surfactant used in the method of the present invention. In particular, the amount of anionic emulsifier with at least one phosphate or phosphonate group does not exceed 20% by weight, based on the total weight of the anionic surfactant used in the method of the present invention.

[0089] In other preferred embodiments, the surfactant may also comprise one or more nonionic surface-active substances, in particular selected from nonionic emulsifiers. Suitable nonionic emulsifiers are, for example, aromatic aliphatic or aliphatic nonionic emulsifiers, such as ethoxylated mono-, di- and tri-alkylphenols (EO level: 3 to 50, alkyl chain: C4-C 10 ), long chain alcohol ethoxylates (EO level: 3 to 100, alkyl chain: C8-C 36 ) and polyethylene oxide / polypropylene oxide homopolymers and copolymers. These may contain alkylene oxide units copolymerized in random distribution or in block form. Very suitable examples are EO / PO block copolymers. Preference is given to ethoxylates of long-chain alkanols (alkyl chain: C1-C 30 , average ethoxylation level: 5 to 100), and among these, particularly preferred are those having C 12 -C 20 Those having an alkyl chain and an average ethoxylation level of 5 to 20, and also ethoxylated monoalkylphenols. Preferably, the surfactant used in the process of the invention comprises less than 60% by weight, especially not more than 50% by weight, of nonionic surfactants, based on the total amount of surfactants used in the process of the invention.

[0090] In other embodiments, the surfactant used in the method of the present invention comprises at least one anionic surfactant and at least one nonionic surfactant, and the ratio of the anionic surfactant to the nonionic surfactant is generally in the range of 0.5:1 to 10:1, in particular 1:1 to 5:1.

[0091] In other preferred embodiments, the surfactant(s) are used in such an amount that the amount of surfactant(s) is in the range of 0.2 to 5% by weight, especially in the range of 0.5 to 3% by weight, based on the monomers to be polymerized.

[0092] The aqueous reaction medium in the polymerization may in principle also contain small amounts (≤5% by weight) of water-soluble organic solvents, such as methanol, ethanol, isopropanol, butanol, pentanol, and also acetone, etc. Preferably, however, the process according to the invention is carried out in the absence of such solvents.

[0093] Typically, the aqueous polymer dispersion obtained has a polymer solids content in the range from 10 to 70% by weight, preferably from 20 to 65% by weight, more preferably from 30 to 60% by weight and most preferably from 40 to 60% by weight, based in each case on the total weight of the aqueous polymer dispersion.

[0094] It has been found to be advantageous to carry out the free radical emulsion polymerization in the presence of a seed latex. The seed latex is a polymer latex present in the aqueous polymerization medium before the metering of glyceryl (meth)acrylate acetonide and optionally further monomers begins. The seed latex can help to better adjust the particle size of the final polymer latex obtained in the free radical emulsion polymerization of the present invention.

[0095] In principle, every polymer latex can be used as seed latex. For the purpose of the present invention, seed latexes in which the particle size of the polymer particles is relatively small are preferred. The Z average particle size of the polymer particles of the seed latex (as measured by dynamic light scattering at 20° C.) is preferably in the range of 10 to 80 nm, in particular 10 to 50 nm. Preferably, the polymer particles of the seed latex are formed from ethylenically unsaturated monomers, which contain at least 95% by weight, based on the total weight of the monomers forming the seed latex, of one or more monomers selected from the group consisting of: C2-C 10 Alkyl esters, in particular ethyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate; C1-C4-alkyl methacrylic acid esters, in particular methyl methacrylate; and vinyl aromatic monomers, in particular styrene.

[0096] For this purpose, the seed latex is usually charged to the polymerization reactor before the metering of glyceryl (meth)acrylate acetonate and optionally further monomers is started. In particular, the seed latex is charged to the polymerization vessel before the metering of glyceryl (meth)acrylate acetonate and optionally further monomers is started, after which the polymerization conditions are established and at least a portion of the free radical initiator is charged to the polymerization vessel.

[0097] The amount of the seed latex may generally be in the range of 0.1 to 10% by weight, specifically 0.5 to 5% by weight, calculated as solid, based on the total weight of the monomers to be polymerized.

[0098] Typically, no free radical initiator, part or all of the amount of free radical initiator, no basic compound, part or all of the amount of basic compound, optionally part or all of the amount of surfactant and optionally part or all of the amount of glyceryl (meth)acrylate acetonide and optionally one or more additional ethylenically unsaturated monomers are initially charged to the reaction vessel.

[0099] In a preferred embodiment, free radical emulsion polymerization is carried out by adding one or more feeds containing glyceryl (meth)acrylate acetonide, optionally one or more additional ethylenically unsaturated monomers and optionally a surfactant, one feed containing an acidic reacting polymerization initiator and one feed containing a basic compound to a reaction vessel containing an aqueous reaction medium.

[0100] In a more preferred embodiment, a portion of the free radical initiator, a portion of the basic compound, optionally a portion of the surfactant and optionally a certain amount of glyceryl (meth)acrylate acetonide and optionally one or more additional ethylenically unsaturated monomers are initially charged to the reaction vessel.

[0101] Therefore, in a more preferred embodiment, the free radical emulsion polymerization is carried out by initially charging part of the free radical initiator, part of the basic compound, optionally part of the surfactant and optionally part of the glyceryl (meth)acrylate acetonate and optionally one or more additional ethylenically unsaturated monomers into a reaction vessel, and adding one or more feeds containing (the remaining glyceryl (meth)acrylate acetonate, optionally (the remaining) one or more additional ethylenically unsaturated monomers and optionally (the remaining) surfactant, one feed containing the remaining acidic reaction polymerization initiator and one feed containing the basic compound.

[0102] The invention also relates to polymer latexes obtained by the method of the invention and their use. Preferred uses of the polymer latexes are uses in coatings, films, paints and various adhesives. Other application areas of the polymer latexes are, for example, pigment printing, road markings, ground or oil drilling fluids.

[0103] The present invention is explained in more detail by the following examples.

[0104] Examples

[0105] Example E1

[0106] Test on the hydrolysis of glyceryl acetonide acrylate under acidic conditions

[0107] 5 g of glyceryl acetonate, 0.4 g of sodium dodecyl sulfate, 0.025 g of methylhydroquinone (MeHQ) and 0.025 g of phenothiazine (PTZ) were mixed with 45 g of deionized water and stirred. The pH value was adjusted to

[0108] a)2.5

[0109] b)3.8

[0110] c)7.0,

[0111] In the case of a) and b), aqueous HCl solution (5 wt.% solution) and in the case of c), aqueous sodium bicarbonate solution (10 wt.%) were used. The mixture was stirred at 90° C. for 3 h. In the case of c), the pH was maintained at pH 7 by continuous addition of drops of aqueous sodium bicarbonate solution (10 wt.%). The mixture was then cooled to room temperature. In the case of a) and b), the pH was adjusted to pH 7 with aqueous sodium hydroxide solution (10 wt.% solution).

[0112] Determination of the degree of hydrolysis of glyceryl acetonide by GC analysis:

[0113] Degree of Hydrolysis:

[0114] a)>99.8%

[0115] b)>99.8%

[0116] c) < 0.01%

[0117] Example E2

[0118] Emulsion Polymerization of Acrylic Acid with Acrylic Acid Glyceryl under Neutral Conditions

[0119] A reactor equipped with a stirrer, a temperature controller, a nitrogen inlet and several injection possibilities is charged with 500 g of deionized water, 11 g of sodium dodecyl sulfate and 0,4 g of potassium persulfate. The reaction mixture is purged with nitrogen, heated to 85° C. and adjusted to pH 7 with feed 3. At 85° C., feed 1 is added within 80 min and feed 2 is added within 90 min. The pH is maintained between pH 6.5 and 7.5 by continuous addition of drops of feed 3 (feed 3 does not necessarily have to be added completely). Feed 1: 350 g of deionized water, 5 g of sodium dodecyl sulfate, 196.25 g of methyl methacrylate, 196.25 g of n-butyl acrylate, 392.5 g of glyceryl acetonate. Feed 2: 3 g of potassium persulfate in 60 g of deionized water. Feed 3: 10 g of sodium bicarbonate in 70 g of deionized water. The reaction mixture is post-polymerized at 85° C. for 60 min. The reaction mixture was then cooled to ambient temperature.

[0120] No condensation was observed.

[0121] Examples E3 to E5

[0122] Emulsion Polymerization of Acrylic Acid with Acrylic Acid Glyceryl under Neutral Conditions

[0123] Emulsion polymerizations of E3-E5 were prepared by a protocol similar to that of E2 replacing the monomers with the corresponding relative amounts (based on total monomers, BOTM) given in wt. % and summarized in Table 1 .

[0124] No condensation was observed.

[0125] Comparative Example C1

[0126] Emulsion polymerization with glyceryl acetonide under acidic conditions without pH adjustment

[0127] A reactor equipped with a stirrer, a temperature controller, a nitrogen inlet and several injection possibilities is charged with 500 g of deionized water, 11 g of sodium dodecyl sulfate and 0,4 g of potassium persulfate. The reaction mixture is purged with nitrogen and heated to 85° C. At 85° C., feed 1 is added within 80 min and feed 2 within 90 min. Feed 1: 350 g of deionized water, 5 g of sodium dodecyl sulfate, 196.25 g of methyl methacrylate, 196.25 g of n-butyl acrylate, 392.5 g of glyceryl acetonate. Feed 2: 3 g of potassium persulfate in 60 g of deionized water. The reaction mixture is post-polymerized at 85° C. for 60 min. The reaction mixture is then cooled to ambient temperature.

[0128] Complete coagulant was observed. No dispersion was formed.

[0129] Comparative Example C2

[0130] Emulsion polymerization of glyceryl acetonide without acrylate under neutral conditions

[0131] The emulsion polymerization of C2 was prepared by a protocol similar to that of E2 replacing the monomers with the corresponding relative amounts (based on total monomers, BOTM) given in wt. % and summarized in Table 1 .

[0132] No condensation was observed.

[0133] The results of the experiment are summarized in Table 1.

[0134] Table 1

[0135]

[0136] BOTM: Based on Total Monomers

[0137] Residual monomer content: Determined by headspace gas chromatography

[0138] Particle size: determined by dynamic light scattering.

Claims

1. A method for preparing an aqueous polymer latex by polymerizing a monomer composition containing glyceryl (meth)acrylate acetonide by free radical emulsion polymerization in an aqueous polymerization medium in the presence of an acidic reactive free radical polymerization initiator, optionally in the presence of a seed latex, wherein the monomer composition comprises a) 0.1 to 100% by weight of glyceryl (meth)acrylate acetonide, b) 0 to 99.9% by weight of one or more further ethylenically unsaturated monomers, It is characterized in that A substantially neutral pH in the range of 6 to 8 is maintained in the aqueous polymerization medium during the free radical emulsion polymerization reaction by the presence of a basic compound.

2. The method of claim 1, wherein: The acidic reacting free radical polymerization initiator is a persulfate.

3. The method according to claim 1 or 2, wherein: The substantially neutral pH in the aqueous polymerization medium is maintained by adding a basic compound to the aqueous polymerization medium during the polymerization reaction.

4. The method of claim 3, wherein: The basic compound is selected from the group consisting of water-soluble hydroxides, oxides, carbonates, bicarbonates (bicarbonates), acetates, citrates, borates, phosphates, hydrogen phosphates of alkali metals or alkaline earth metals or ammonium, ammonia or water-soluble organic amines.

5. The method of claim 4, wherein: These alkaline compounds are selected from the group consisting of sodium, potassium and ammonium hydroxides, sodium and potassium carbonates and sodium and potassium bicarbonates (bicarbonates).

6. The method according to any one of claims 1 to 5, wherein: The free radical emulsion polymerization is carried out in the presence of a surfactant.

7. The method according to any one of claims 1 to 6, wherein: The free radical emulsion polymerization is carried out by adding one or more feeds containing glyceryl (meth)acrylate acetonide, optionally one or more additional ethylenically unsaturated monomers and optionally a surfactant, one feed containing the acidic reacting polymerization initiator and one feed containing the basic compound to a reaction vessel containing the aqueous reaction medium.

8. The method of claim 7, wherein: The reaction vessel is initially charged with a portion of the free radical initiator, a portion of the basic compound, optionally a portion of the surfactant and optionally a portion of glyceryl acetonide (meth)acrylate and optionally the one or more additional ethylenically unsaturated monomers.

9. A polymer latex obtainable by the method according to any one of claims 1 to 8.

10. Use of the polymer latex according to claim 9 in coatings, films, paints, adhesives and for pigment printing, road markings, flooring or oil drilling.

Citation Information

Cited By

  • Water-based ink acrylate emulsion for PVC (polyvinyl chloride) and preparation method of water-based ink acrylate emulsion

    CN120442105A

  • Water-based ink acrylate emulsion for PVC and its preparation method

    CN120442105B