Thermoplastic resin composition and molded article manufactured therefrom
By introducing components such as polysiloxane-polycarbonate copolymer resin, silicone modified polyester and syngastic polystyrene into the polycarbonate resin, combined with benzotriazole UV stabilizer, the solution is solved Polycarbonate resin has low scratch resistance and deterioration of optical properties in vehicle parts, achieving piano black color and good weather resistance and impact resistance.
Patent Information
- Application Number
- CN202380032360.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-15
AI Technical Summary
Polycarbonate resins have problems with low scratch resistance and deterioration of optical properties in vehicle parts applications. Existing improved methods such as the introduction of acrylate copolymers or silicone surface modifiers cannot be effectively solved, especially the difficulty in realizing pianos. Black color and good weather resistance.
Using thermoplastic resin compositions, including polycarbonate resins, polysiloxane-polycarbonate copolymer resins, silicone modified polyester and syngastic polystyrene, and benzotriazole-based UV stabilizers, The synergy of these components improves the compatibility and performance of the resin.
It achieves excellent scratch resistance, impact resistance and weather resistance, and achieves the tinting performance of piano black, ensuring the high-quality dark black appearance and mechanical properties of molded products.
Smart Images

Figure BDA0005069683340000021 
Figure BDA0005069683340000031 
Figure BDA0005069683340000041
Abstract
Description
Technical Field
[0001] Disclosed are a thermoplastic resin composition and a molded article produced therefrom. Background Art
[0002] Thermoplastic resins have a lower specific gravity than glass or metal, and also have advantages such as excellent plasticity and impact resistance. With the recent trend of low cost, large size, and light weight of electrical and electronic products, plastic products using thermoplastic resins have rapidly replaced traditional glass or metal products and are being used more widely from electrical and electronic products to automotive parts.
[0003] Among thermoplastic resins, polycarbonate (PC) resin has excellent impact resistance, heat resistance, strength, etc., and is therefore widely used in electrical and electronic products and vehicle parts. In addition, a colorant may be introduced into the polycarbonate resin to achieve the beauty of the vehicle.
[0004] However, since polycarbonate resins have basically low scratch resistance, in order to use them for vehicle parts, post-processing (such as surface treatment, coating, etc.) must be performed, which may cause additional problems (such as increased production costs and environmental pollution, etc.).
[0005] In order to improve the above-mentioned problems, attempts have been made to introduce an acrylate copolymer component therein to improve the scratch resistance of the polycarbonate resin, but due to the low compatibility between the polycarbonate resin and the acrylate copolymer component and the large refractive index difference between the polycarbonate resin and the acrylate copolymer component, there is a problem of deteriorating optical properties and mechanical properties.
[0006] In addition, there has been another attempt to introduce a silicone-based surface modifier therein to improve the scratch characteristics of polycarbonate resin, but due to the low compatibility between polycarbonate resin and the silicone-based surface modifier, this is still far from achieving colors that emphasize aesthetics, especially piano black.
[0007] To solve this problem, another attempt is to use a silicone-modified polycarbonate resin as the polycarbonate resin to ensure sufficient compatibility between the silicone-modified polycarbonate resin and the silicone-based surface modifier, which can achieve a piano black color and achieve satisfactory scratch resistance, but there is still another problem of deterioration of weather resistance due to the silicon (Si) component. Summary of the invention
[0008] To overcome this problem, the present invention provides a thermoplastic resin composition capable of achieving excellent coloring properties to the extent of achieving piano black and ensuring excellent scratch resistance, impact resistance and weather resistance, and a molded article produced therefrom.
[0009] According to an embodiment, a thermoplastic resin composition is provided, which includes: (A) a polycarbonate resin; (B) a polysiloxane-polycarbonate copolymer resin; (C) a siloxane-modified polyester; (D) syndiotactic polystyrene; and (E) a benzotriazole-based ultraviolet (UV) stabilizer.
[0010] The thermoplastic resin composition may include 100 parts by weight of a base resin (including 50 to 90 wt % of (A) a polycarbonate resin; and 10 to 50 wt % of (B) a polysiloxane-polycarbonate copolymer resin), 1 to 7 parts by weight of (C) a siloxane-modified polyester; 0.5 to 5 parts by weight of (D) a syndiotactic polystyrene; and 0.5 to 5 parts by weight of (E) a benzotriazole-based UV stabilizer.
[0011] The (A) polycarbonate resin may have a weight average molecular weight of about 10,000 g / mol to about 100,000 g / mol.
[0012] (A) The polycarbonate resin may be a bisphenol A-based polycarbonate resin.
[0013] The (B) polysiloxane-polycarbonate copolymer resin may include a polycarbonate block and a polysiloxane block, and the polysiloxane block may include a structural unit represented by Chemical Formula 2:
[0014] [Chemical formula 2]
[0015]
[0016] In the chemical formula 2, R 3 and R 4 R and R' are the same or different and are a hydrogen atom, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C1 to C20 alkoxy group, a substituted or unsubstituted C3 to C30 cycloalkyl group, a substituted or unsubstituted C3 to C30 cycloalkenyl group, a substituted or unsubstituted C3 to C30 cycloalkynyl group, a substituted or unsubstituted C6 to C30 aryl group, a substituted or unsubstituted C6 to C30 aryloxy group, a substituted or unsubstituted C6 to C30 aryl group, or NRR' (wherein R and R' are the same or different and are a hydrogen atom, or a substituted or unsubstituted C1 to C20 alkyl group).
[0017] The (B) polysiloxane-polycarbonate copolymer resin may include 1 wt % to 50 wt % of a polysiloxane block.
[0018] The (B) polysiloxane-polycarbonate copolymer resin may have a weight average molecular weight of about 15,000 g / mol to about 50,000 g / mol.
[0019] (C) The siloxane-modified polyester may include a structural unit represented by Chemical Formula 3:
[0020] [Chemical formula 3]
[0021]
[0022] In chemical formula 3, R 5 , R 6 , R 7 and R 8 Each independently is a C1 to C5 alkylene group, R 9 is C1 to C4 alkyl or phenyl, R 10 is hydrogen, hydroxy or methyl, and m and n are each independently an integer of 1 or greater.
[0023] In an embodiment, in Chemical Formula 3, R 5 and R 6 Each can be -(CH 2 ) 3 -, R 7 and R 8 Each can be -(CH 2 ) 5 -, R 9 A methyl group may be included, and m and n may be integers greater than or equal to 1 satisfying m:n=18:30.
[0024] (D) The syndiotactic degree of syndiotactic polystyrene may be 97% to 100%.
[0025] The thermoplastic resin composition may further include at least one additive selected from the group consisting of flame retardants, nucleating agents, coupling agents, glass fibers, plasticizers, lubricants, mineral fillers, antimicrobial agents, mold release agents, heat stabilizers, antioxidants, and antistatic agents.
[0026] Meanwhile, a molded article manufactured from the thermoplastic resin composition according to the embodiment may be provided.
[0027] The molded article may have a notched Izod impact strength of greater than or equal to 30 kgf·cm / cm at a thickness of 1 / 4 inch measured in accordance with ASTM D256.
[0028] The molded article may have a lightness change (ΔL) of less than or equal to 4.0 before and after the scratch resistance evaluation, as measured using a scratch hardness tester 430P-I from Erichsen Co., Ltd.
[0029] The molded article may have a color change (ΔE) of less than or equal to 3.0 before and after weathering evaluation as measured by irradiating the article with an energy of 2,500 KJ using a xenon arc accelerated weathering tester in accordance with SAE J 1960.
[0030] The thermoplastic resin composition according to the embodiment and the molded article manufactured therefrom have excellent scratch resistance, impact resistance, and weather resistance, as well as excellent coloring properties. DETAILED DESCRIPTION
[0031] Hereinafter, embodiments of the present invention are described in detail. However, these embodiments are exemplary, and the present disclosure is not limited thereto.
[0032] In the present specification, unless otherwise mentioned, "copolymerization" means block copolymerization, random copolymerization or graft copolymerization, and "copolymer" means block copolymer, random copolymer or graft copolymer.
[0033] In this specification, unless otherwise mentioned, the weight average molecular weight is measured using a 1200 series gel permeation chromatograph (GPC) manufactured by Agilent Technologies, Inc. after dissolving a powder sample in an appropriate solvent (the standard sample is Shodex polystyrene).
[0034] According to an embodiment, a thermoplastic resin composition is provided, which includes (A) a polycarbonate resin; (B) a polysiloxane-polycarbonate copolymer resin; (C) a siloxane-modified polyester; (D) syndiotactic polystyrene; and (E) a benzotriazole-based ultraviolet (UV) stabilizer.
[0035] Hereinafter, each component of the thermoplastic resin composition is described in detail.
[0036] (A) Polycarbonate resin
[0037] (A) The polycarbonate (PC) resin is a polyester having a carbonate bond, but is not particularly limited in type, and may include any polycarbonate resin that can be used in the field of resin compositions.
[0038] For example, the polycarbonate resin may be prepared by reacting a diphenol compound represented by Chemical Formula 1 with a compound selected from the group consisting of phosgene, halogen esters, carbonate esters, and combinations thereof.
[0039] [Chemical formula 1]
[0040]
[0041] In Chemical Formula 1,
[0042] A is a single bond, substituted or unsubstituted C1 to C30 alkylene, substituted or unsubstituted C2 to C5 alkenylene, substituted or unsubstituted C2 to C5 alkylene, substituted or unsubstituted C1 to C30 haloalkylene, substituted or unsubstituted C5 to C6 cycloalkylene, substituted or unsubstituted C5 to C6 cycloalkenylene, substituted or unsubstituted C5 to C10 cycloalkylene, substituted or unsubstituted C6 to C30 arylene, substituted or unsubstituted C1 to C20 alkyleneoxy, haloester, carbonate, selected from C═O, S and SO 2 The linking group in R 1 and R 2 Each is independently a substituted or unsubstituted C1 to C30 alkyl group or a substituted or unsubstituted C6 to C30 aryl group, and n1 and n2 are each independently an integer ranging from 0 to 4.
[0043] Two or more types of diphenols represented by Chemical Formula 1 may be combined to constitute a repeating unit of the polycarbonate resin.
[0044] Specific examples of diphenols may include hydroquinone, resorcinol, 4,4'-dihydroxybiphenyl, 2,2-bis(4-hydroxyphenyl)propane (also called "bisphenol A"), 2,4-bis(4-hydroxyphenyl)-2-methylbutane, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2-bis(3-chloro-4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane, 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane, bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)ketone, bis(4-hydroxyphenyl)ether, and the like. Among the diphenols, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane or 1,1-bis(4-hydroxyphenyl)cyclohexane may be desirably used. 2,2-bis(4-hydroxyphenyl)propane may be more desirably used.
[0045] (A) The polycarbonate resin may be a mixture of copolymers obtained using two or more types of diphenols. In addition, the polycarbonate resin may be a chain polycarbonate resin, a branched polycarbonate resin, a polyester carbonate copolymer resin, and the like.
[0046] A specific example of a chain polycarbonate resin may be a bisphenol A polycarbonate resin. A specific example of a branched polycarbonate resin may be a resin prepared by reacting a polyfunctional aromatic compound (such as trimellitic anhydride and trimellitic acid, etc.) with a diphenol and a carbonate. A polyester carbonate copolymer resin may be prepared by reacting a difunctional carboxylic acid with a diphenol and a carbonate, and the carbonate used here may be a diaryl carbonate (such as diphenyl carbonate) or ethylene carbonate.
[0047] The (A) polycarbonate resin may have a weight average molecular weight of about 10,000 g / mol to about 100,000 g / mol, for example, about 14,000 to about 50,000 g / mol. When the weight average molecular weight of the polycarbonate resin is within the above range, excellent impact resistance and fluidity may be obtained.
[0048] The (A) polycarbonate resin may be included in an amount of 50 wt % to 90 wt %, such as 50 wt % to 70 wt %, such as 60 wt % to 90 wt %, such as 70 wt % to 90 wt %, based on 100 wt % of the base resin including the (A) polycarbonate resin and the (B) polysiloxane-polycarbonate copolymer resin described later. Within the above weight range, the thermoplastic resin composition and the molded article manufactured therefrom may exhibit excellent appearance and mechanical strength.
[0049] The (A) polycarbonate resin may have a melt flow index of 5 to 80 g / 10 min, for example, 10 to 70 g / 10 min, as measured at 300° C. and a load of 1.2 kg according to ASTM D1238. When a polycarbonate resin having a melt flow index within the above range is used, the thermoplastic resin composition and a molded article made therefrom may exhibit excellent plasticity and excellent impact resistance.
[0050] Meanwhile, (A) polycarbonate resin can be used by mixing two or more polycarbonate resins having different weight average molecular weights or melt flow indexes. By using a mixture of polycarbonate resins having different weight average molecular weights or melt flow indexes, it is easy to adjust the thermoplastic resin composition to have desired fluidity.
[0051] (B) Polysiloxane-polycarbonate copolymer resin
[0052] The (B) polysiloxane-polycarbonate copolymer resin may be used together with the (A) polycarbonate resin and the (C) siloxane-modified polyester to be described later, in order to improve the compatibility of the components in the thermoplastic resin composition.
[0053] Conventionally, in order to improve the scratch resistance of a polycarbonate resin composition, a silicone surface modifier is added to the polycarbonate resin, which can improve the scratch resistance, but there is a problem of deteriorating mechanical properties or reducing coloring properties due to low compatibility between the polycarbonate resin and the silicone surface modifier, so that high black (such as piano black) cannot be achieved.
[0054] The present invention solves this problem by improving the compatibility between the polycarbonate resin (component (A)) and the siloxane-modified polyester (component (C)) by including (B) a polysiloxane-polycarbonate copolymer resin into a thermoplastic resin composition comprising a polycarbonate resin as a main component.
[0055] The (B) polysiloxane-polycarbonate copolymer resin may include a polycarbonate block and a polysiloxane block.
[0056] The polycarbonate block may include the same carbonate structural unit as that included in the aforementioned (A) polycarbonate resin.
[0057] The polysiloxane block may include a structural unit represented by Chemical Formula 2.
[0058] [Chemical formula 2]
[0059]
[0060] In chemical formula 2, R 3 and R 4 The same or different, and may be a hydrogen atom, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C1 to C20 alkoxy group, a substituted or unsubstituted C3 to C30 cycloalkyl group, a substituted or unsubstituted C3 to C30 cycloalkenyl group, a substituted or unsubstituted C3 to C30 cycloalkynyl group, a substituted or unsubstituted C6 to C30 aryl group, a substituted or unsubstituted C6 to C30 aryloxy group, a substituted or unsubstituted C6 to C30 aryl group, or NRR' (wherein R and R' are the same or different, and may be a hydrogen atom or a substituted or unsubstituted C1 to C20 alkyl group).
[0061] The polysiloxane block may be included in an amount of 1 wt % to 50 wt %, such as 1 wt % to 40 wt %, such as 1 wt % to 30 wt %, such as 1 wt % to 20 wt %, such as 1 wt % to 10 wt %, based on 100 wt % of the polysiloxane-polycarbonate copolymer resin, but is not limited thereto.
[0062] By including the polysiloxane block within the above weight range in the polysiloxane-polycarbonate copolymer resin, impact resistance of the thermoplastic resin composition and a molded article produced therefrom may be improved, and processing such as extrusion and injection molding may be easy.
[0063] The (B) polysiloxane-polycarbonate copolymer resin may have a weight average molecular weight of about 15,000 to about 50,000 g / mol, for example about 15,000 to about 30,000 g / mol. Within the above range, the thermoplastic resin composition and a molded article made therefrom may have excellent impact resistance.
[0064] The (B) polysiloxane-polycarbonate copolymer resin may be included in an amount of 10 wt % to 50 wt %, such as 30 wt % to 50 wt %, such as 10 wt % to 40 wt %, such as 10 wt % to 30 wt %, based on 100 wt % of the base resin. Within the above range, the thermoplastic resin composition and a molded article made therefrom may have excellent impact resistance and coloring properties.
[0065] (C) Siloxane-modified polyester
[0066] (C) The siloxane-modified polyester can improve the scratch resistance and coloring properties of the thermoplastic resin composition according to the present invention.
[0067] (C) The siloxane-modified polyester may include a structural unit represented by Chemical Formula 3:
[0068] [Chemical formula 3]
[0069]
[0070] In chemical formula 3, R 5 , R 6 , R 7 and R 8 Each independently is a C1 to C5 alkylene group, R 9 is C1 to C4 alkyl or phenyl, R 10 is hydrogen, hydroxy or methyl, and m and n are each independently an integer of 1 or greater.
[0071] In an embodiment, in Chemical Formula 3, R 5 and R 6 Each can be -(CH 2 ) 3 -, R 7 and R 8 Each can be -(CH 2 ) 5 -, R 9 A methyl group may be included, and m and n may be integers greater than or equal to 1 satisfying m:n=18:30.
[0072] Based on 100 parts by weight of the base resin including (A) and (B), the amount of the (C) siloxane-modified polyester included may be 1 to 7 parts by weight, for example, the amount of the (C) siloxane-modified polyester included may be 2 to 5 parts by weight. Within the above amount range, the scratch resistance and coloring properties of the thermoplastic resin composition and the molded article manufactured therefrom may be improved.
[0073] (D) Syndiotactic polystyrene
[0074] (D) Syndiotactic polystyrene can improve the impact resistance of the thermoplastic resin composition according to the present invention.
[0075] Polystyrene is generally classified into atactic, isotactic, and syndiotactic structures based on the position of the benzene rings. Atactic polystyrene has an irregular arrangement of benzene rings, while isotactic polystyrene has a structure in which the benzene rings are arranged on one side of the polymer backbone. In contrast, syndiotactic polystyrene has a structure in which the benzene rings are arranged in a regular, alternating pattern.
[0076] Wherein, syndiotactic polystyrene can be prepared using a catalytic system comprising styrene monomer, a metallocene catalyst and a cocatalyst. A metallocene catalyst has a structure in which one or two cycloalkadienyl groups (cyclopentadienyl, indenyl, fluorenyl and derivatives thereof) are attached to a Group IV transition metal (such as Ti, Zr or Hf) complex of the periodic table.
[0077] As the prior art of polystyrene with high stereoregularity, high melting point and excellent molecular weight distribution, U.S. Patent No. 6,010,974 discloses a novel alkyl-bridged binuclear metallocene catalyst, a silyl-bridged binuclear metallocene catalyst and a method for polymerizing styrene monomer using an alkyl-silyl-bridged binuclear metallocene catalyst, and U.S. Patent No. 6,284,700 discloses syndiotactic polystyrene using a catalyst system consisting of a metallocene catalyst and a cocatalyst. The disclosures in these patents are incorporated herein by reference in their entirety.
[0078] (D) The syndiotactic degree of syndiotactic polystyrene may be 97% to 100%.
[0079] Based on 100 parts by weight of the base resin, the amount of (D) syndiotactic polystyrene included may be 0.5 parts by weight to 5 parts by weight, for example 1 part by weight to 5 parts by weight, for example 1 part by weight to 3 parts by weight. Within the above weight range, the thermoplastic resin composition and the molded article manufactured therefrom may have excellent impact resistance.
[0080] (E) Benzotriazole UV stabilizer
[0081] (E) The benzotriazole-based UV stabilizer prevents the thermoplastic resin composition according to the present invention from being decomposed and discolored by ultraviolet rays, thereby improving weather resistance.
[0082] The type of the benzotriazole-based UV stabilizer is not particularly limited, and various commercially available benzotriazole-based UV stabilizers can be used.
[0083] The benzotriazole-based UV stabilizer may be included in an amount of 0.5 to 5 parts by weight, such as 1 to 5 parts by weight, such as 1 to 4 parts by weight, such as 2 to 4 parts by weight, based on 100 parts by weight of the base resin. Within the above weight range, the thermoplastic resin composition and the molded article manufactured therefrom may have excellent weather resistance.
[0084] (F) Other additives
[0085] In addition to components (A) to (E), the thermoplastic resin composition according to an embodiment may further include one or more additives required to balance the properties while maintaining excellent scratch resistance, weather resistance, impact resistance, and coloring properties or according to the final use of the thermoplastic resin composition.
[0086] Specifically, the additive may include at least one additive selected from flame retardants, nucleating agents, coupling agents, glass fibers, plasticizers, lubricants, mineral fillers, antimicrobial agents, mold release agents, thermal stabilizers, antioxidants, and antistatic agents.
[0087] These additives may be appropriately included within a range not to impair physical properties of the thermoplastic resin composition, and may be specifically included in an amount of 20 parts by weight or less based on 100 parts by weight of the base resin, but are not limited thereto.
[0088] The thermoplastic resin composition according to the present invention can be prepared by a known method for preparing a thermoplastic resin composition.
[0089] For example, the thermoplastic resin composition according to the present invention can be prepared in the form of pellets by mixing the components of the present invention and other additives and then melting and kneading the components of the present invention and other additives in an extruder.
[0090] The molded article according to the embodiment of the present invention may be manufactured from the aforementioned thermoplastic resin composition.
[0091] A molded article produced by appropriately adding a mixture of quinone-based dyes exhibiting black color to the above-mentioned thermoplastic resin composition can realize piano black, which is a high-quality deep black color, due to the synergistic effect of each component of the thermoplastic resin composition.
[0092] The molded article may have a notched Izod impact strength of greater than or equal to 30 kgf·cm / cm at a thickness of 1 / 4 inch measured in accordance with ASTM D256.
[0093] The molded article may have a lightness change (ΔL) of less than or equal to 4.0 before and after the scratch resistance evaluation, as measured using a scratch hardness tester 430P-I from Erichsen Co., Ltd.
[0094] The molded article may have a color change (ΔE) of less than or equal to 3.0 before and after weathering evaluation, as measured by irradiating the article with an energy of 2,500 KJ using a xenon arc accelerated weathering tester according to SAE J 1960.
[0095] Hereinafter, preferred embodiments of the present invention will be described. However, the following embodiments are merely preferred embodiments of the present invention, and the present invention is not limited to the following embodiments.
[0096] Examples 1 to 6 and Comparative Examples 1 to 6
[0097] According to the content ratio of each component shown in Table 1, thermoplastic resin compositions according to Examples 1 to 6 and Comparative Examples 1 to 6 were prepared, respectively.
[0098] Based on 100 parts by weight of base resin, black quinone dye mixture is added to the component shown in Table 1 with the amount of 0.5 parts by weight, and then dry blended, quantitatively and continuously fed into the feed section of a twin screw extruder (L / D=29, diameter=45mm), and melt / kneading. In this article, the barrel temperature of the twin screw extruder is set at about 280 ℃. Subsequently, each thermoplastic resin composition granulated from the twin screw extruder was dried at about 80 ℃ for about 4 hours, and then by using 6 ounces of injection molding machines at about 280 ℃ barrel temperature and about 60 ℃ mold temperature for injection molding for measuring the sample of physical properties.
[0099] In Table 1, (A) and (B) show the wt% of each component based on 100 wt% of the base resin, and (C), (D) and (E) show the weight parts of (C), (D) and (E) based on 100 parts by weight of the base resin ((A) + (B)).
[0100] (Table 1)
[0101]
[0102] Each component in Table 1 is described as follows.
[0103] (A) Polycarbonate resin
[0104] A bisphenol A chain polycarbonate resin having a weight average molecular weight of about 25,000 g / mol was used.
[0105] (B) Polysiloxane-polycarbonate copolymer resin
[0106] A polysiloxane-polycarbonate copolymer resin having a weight average molecular weight of about 24,000 g / mol and including about 97 wt % to 94 wt % of a polycarbonate block and about 3 wt % to 6 wt % of a polysiloxane block was used.
[0107] (C) Siloxane-modified polyester
[0108] H-Si 6441P from Evonik Industries was used.
[0109] (D) Syndiotactic polystyrene
[0110] 130ZC from Idemitsu Kosan Co., Ltd. was used.
[0111] (E) Benzotriazole UV stabilizer
[0112] Adeka's LA-300K was used.
[0113] Experimental Examples
[0114] The experimental results are shown in Table 2.
[0115] (1) Impact resistance (unit: kgf·cm / cm): The notched Izod impact strength of a 1 / 4 inch thick sample was measured according to ASTM D256.
[0116] (2) Coloring property: The lightness value (L) was measured by using CM-3700D (Konica Minolta Sensing Co., Ltd.) in the specular element free (SCE) mode. The lower the lightness, the better the black color, which confirmed that the coloring property was better.
[0117] (3) Weather resistance: According to SAE J 1960, the sample was irradiated with an energy of 2,500 KJ by using a xenon arc accelerated weathering tester, and the color change (ΔE) on the glossy surface before and after the evaluation was measured by using CM-3700D of Konica Minolta Sensing Co., Ltd. in the specular component free (SCE) mode.
[0118] (4) Scratch resistance
[0119] By using a scratch hardness tester 430P-I manufactured by Erichsen Co., Ltd., under the conditions that the test cutter has a diameter of 1 mm and a load of 10 N, at a cutting speed of 1 m / min, after applying scratches to the sample 20 times in a grid pattern at intervals of 2 mm, the lightness change (ΔL) of the sample before and after the scratch evaluation was measured in the specular reflection component-free (SCE) mode by using a CM-3700D of Konica Minolta Sensing Co., Ltd. Since the applied scratches generate microcracks on the sample surface, generating flaws, which increases the lightness of the sample, the higher the lightness change (ΔL), the more damage is caused by the scratches, which is judged to be low in scratch resistance.
[0120] (Table 2)
[0121]
[0122] Referring to Tables 1 and 2, when a thermoplastic resin composition is prepared by using a polycarbonate resin, a polysiloxane-polycarbonate copolymer resin, a siloxane-modified polyester, a syndiotactic polystyrene, and a benzotriazole-based ultraviolet (UV) stabilizer in optimal amounts, it is confirmed that a thermoplastic resin composition having excellent impact resistance, weather resistance, scratch resistance, and coloring properties is achieved, and a molded article manufactured therefrom is confirmed.
[0123] In particular, the molded articles manufactured from the thermoplastic resin compositions of Examples 1 to 6 maintained excellent properties and simultaneously had a lightness (L) of 2.0 or less, thus exhibiting excellent coloring properties to the extent of achieving piano black.
[0124] While the invention has been described in conjunction with what are presently considered to be practical example embodiments, it should be understood that the invention is not limited to the disclosed embodiments, but is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the claims.
Claims
1. A thermoplastic resin composition comprising: (A) polycarbonate resin; (B) polysiloxane-polycarbonate copolymer resin; (C) siloxane-modified polyester; (D) syndiotactic polystyrene; and (E) Benzotriazole ultraviolet (UV) stabilizer.
2. The thermoplastic resin composition according to claim 1, wherein The thermoplastic resin composition comprises: 100 parts by weight of a base resin, comprising: 50 wt % to 90 wt % of the (A) polycarbonate resin; and 10 wt % to 50 wt % of the (B) polysiloxane-polycarbonate copolymer resin, 1 to 7 parts by weight of the (C) siloxane-modified polyester; 0.5 to 5 parts by weight of the (D) syndiotactic polystyrene; and 0.5 to 5 parts by weight of the (E) benzotriazole UV stabilizer.
3. The thermoplastic resin composition according to claim 1, wherein The (A) polycarbonate resin has a weight average molecular weight of about 10,000 g / mol to about 100,000 g / mol.
4. The thermoplastic resin composition according to claim 1, wherein The (A) polycarbonate resin is a bisphenol A polycarbonate resin.
5. The thermoplastic resin composition according to claim 1, wherein The (B) polysiloxane-polycarbonate copolymer resin includes a polycarbonate block and a polysiloxane block, and the polysiloxane block includes a structural unit represented by Chemical Formula 2: [Chemical formula 2] in, In chemical formula 2, R 3 and R 4 R and R' are the same or different and are a hydrogen atom, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C1 to C20 alkoxy group, a substituted or unsubstituted C3 to C30 cycloalkyl group, a substituted or unsubstituted C3 to C30 cycloalkenyl group, a substituted or unsubstituted C3 to C30 cycloalkynyl group, a substituted or unsubstituted C6 to C30 aryl group, a substituted or unsubstituted C6 to C30 aryloxy group, a substituted or unsubstituted C6 to C30 aryl group, or NRR' (wherein R and R' are the same or different and are a hydrogen atom or a substituted or unsubstituted C1 to C20 alkyl group).
6. The thermoplastic resin composition according to claim 5, wherein The (B) polysiloxane-polycarbonate copolymer resin includes 1 wt % to 50 wt % of the polysiloxane block.
7. The thermoplastic resin composition according to claim 1, wherein The (B) polysiloxane-polycarbonate copolymer resin has a weight average molecular weight of about 15,000 g / mol to about 50,000 g / mol.
8. The thermoplastic resin composition according to claim 1, wherein The (C) siloxane-modified polyester is represented by Chemical Formula 3: [Chemical formula 3] in, In chemical formula 3, R 5 , R 6 , R 7 and R 8 Each independently is a C1 to C5 alkylene group, R 9 is C1 to C4 alkyl or phenyl, R 10 is hydrogen, hydroxy or methyl, and m and n are each independently an integer of 1 or greater.
9. The thermoplastic resin composition according to claim 8, wherein In chemical formula 3, R 5 and R 6 Each is -(CH2)3-, R 7 and R 8 Each is -(CH2)5-, R 9 is a methyl group, and m and n are integers greater than or equal to 1 satisfying m:n=18:
30.
10. The thermoplastic resin composition according to claim 1, wherein The syndiotactic degree of the (D) syndiotactic polystyrene is 97% to 100%.
11. The thermoplastic resin composition according to claim 1, wherein The thermoplastic resin composition comprises at least one additive selected from the group consisting of flame retardants, nucleating agents, coupling agents, glass fibers, plasticizers, lubricants, mineral fillers, antibacterial agents, mold release agents, thermal stabilizers, antioxidants, and antistatic agents.
12. A molded article produced from the thermoplastic resin composition according to any one of claims 1 to 11.
13. The molded article according to claim 12, wherein The molded article has a notched Izod impact strength of greater than or equal to 30 kgf·cm / cm at a thickness of 1 / 4 inch measured in accordance with ASTM D256.
14. The molded article according to claim 12, wherein The molded article has a lightness change (ΔL) of less than or equal to 4.0 before and after the scratch resistance evaluation, as measured using a scratch hardness tester 430P-I from Erichsen Co., Ltd.
15. The molded article according to claim 12, wherein The molded article has a color change (ΔE) of less than or equal to 3.0 before and after the weatherability evaluation as measured by irradiating the article with an energy of 2,500 KJ using a xenon arc accelerated weatherability tester in accordance with SAE J 1960.