Titanium (IV) oxide powder comprising particles having peanut gemini shape, and cosmetic containing same

By using peanut-shaped twin titanium dioxide particles of specific shapes and sizes, the problem of insufficient extensibility and dispersibility of titanium dioxide particles in cosmetics has been solved, achieving lightweight extensibility, soft focus and moderate coverage in cosmetics, creating a natural bare skin feel.

CN118974178APending Publication Date: 2024-11-15TITAN IND INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380030659.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The titanium dioxide particles in existing cosmetics lack sufficient extensibility, smoothness, and dispersibility, resulting in an unpleasant feel when applying makeup, a tendency to leave a white cast, insufficient coverage, and an inability to naturally conceal skin imperfections.

Method used

Titanium oxide (IV) particles with a peanut-shaped twin shape are used, with a major axis diameter of 300 nm or more and 700 nm or less, a minor axis diameter of 100 nm or more and 400 nm or less, a narrow portion diameter of 80 nm or more and 200 nm or less, and a narrow portion diameter/minor axis diameter ratio of 0.9 or less. They are formed by the aggregation of fine rod-shaped particles, and the particle surface can be covered with an inorganic and/or organic layer.

Benefits of technology

It achieves lightweight spreadability, soft-focus effect, and moderate coverage in cosmetics, forming an even makeup film, avoiding whitening, and showing a natural bare skin look, while also exhibiting excellent dispersion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974178A_ABST
    Figure CN118974178A_ABST
Patent Text Reader

Abstract

Provided is a titanium oxide capable of providing a cosmetic capable of exhibiting a natural nude muscle feeling by having light ductility, flexibility, and moderate covering power, thereby achieving a uniform cosmetic film. Provided are: titanium oxide (IV) comprising particles characterized by having a peanut-type gemini shape; and a cosmetic containing the titanium oxide (IV). The longest portion of one of the peanut gemini-shaped particles has a major axis diameter of 300-700 nm inclusive, the largest portion in the direction perpendicular to the major axis has a minor axis diameter of 100-400 nm inclusive, and the diameter of a narrowed portion of the length in the direction perpendicular to the major axis at the center of the major axis is 80-200 nm inclusive. The ratio of the narrowed portion diameter / minor axis diameter is 0.9 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a titanium (IV) oxide powder consisting of particles characterized by a peanut-shaped twin shape and a method for producing the same.

[0002] The present invention also relates to a cosmetic containing the titanium (IV) oxide powder. The cosmetic containing the titanium (IV) oxide has light spreadability, soft focus properties, and moderate covering power, so that the uniformity of the cosmetic film is excellent and a natural bare skin feeling can be expressed. Background Art

[0003] Conventionally, makeup cosmetics such as foundations have been used as cosmetics that change the color of the skin by adding pigments with high coloring power such as titanium (IV) oxide and other inorganic pigments, organic pigments and other colorants in order to cover redness, dullness, spots, freckles and the like caused by the skin and give the skin an even and beautiful appearance.

[0004] Titanium oxide is generally used as a pigment with high coloring and hiding power, such as titanium (IV) oxide, to cover redness, dullness, etc. and eliminate skin unevenness. Japanese Patent Application Laid-Open No. 61-118311 (Patent Document 1) uses spherical titanium oxide with a particle size of 0.1 μm to 50 μm.

[0005] However, when applying makeup using a foundation containing titanium oxide, the skin may feel astringent or lose its smooth touch. In addition, under sunlight, due to a phenomenon generally known as whitening caused by the high reflectivity of blue-toned colors, there is a problem that the finished makeup looks unnaturally bluish-white. In order to solve this problem, attempts have been made to set the primary particle size to a smaller side.

[0006] For example, Japanese Patent Application Laid-Open No. 9-221411 (Patent Document 2) discloses a cosmetic product containing titanium dioxide having an average particle size of more than 0.10 μm and less than 0.14 μm. Japanese Patent Application Laid-Open No. 11-158035 (Patent Document 3) discloses a cosmetic product containing titanium dioxide having a primary particle size of more than 0.001 μm and less than 0.15 μm and a secondary particle size of more than 0.6 μm and less than 2.0 μm, and having an anatase crystal form.

[0007] In addition, in Japanese Patent Gazette No. 2000-191325 (Patent Document 4), it is proposed to use spherical titanium dioxide aggregates with an apparent average particle size of 0.1 μm to 3 μm, which are formed by small spherical particles of titanium dioxide with an average primary particle size of 0.01 μm to 0.07 μm as measured by X-ray diffraction, in cosmetics, and it is disclosed that the cosmetics can be expected to have good sliding properties and excellent light stability that previous titanium dioxide did not have.

[0008] In addition, the applicant proposed in Japanese Patent Application Laid-Open No. 2008-56535 (Patent Document 5) a rutile titanium oxide aggregate particle having a particle size of 0.1 μm or more and 5.0 μm or less, wherein the rod-shaped titanium oxide primary particles are aggregated to form a fan-shaped titanium oxide, and the fan-shaped titanium oxide is further aggregated to form a cosmetic using the aggregated particles. In addition, it is reported that the cosmetic can be applied smoothly to the skin without astringent or rough feeling on the skin, and with appropriate coloring power and covering power, it can show a natural bare skin feeling without whitening.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 61-118311

[0012] Patent Document 2: Japanese Patent Application Laid-Open No. 9-221411

[0013] Patent Document 3: Japanese Patent Application Laid-Open No. 11-158035

[0014] Patent Document 4: Japanese Patent Application Publication No. 2000-191325

[0015] Patent Document 5: Japanese Patent Application Publication No. 2008-56535 Summary of the invention

[0016] Problem that the invention aims to solve

[0017] However, the cosmetic described in Patent Document 2 is not sufficient in terms of spreadability and smoothness during makeup.

[0018] In addition, the cosmetic disclosed in Patent Document 3 has a high activity and a strong blue hue because the crystal form is anatase type. In addition, the dispersion when added to the cosmetic cannot be said to be sufficient.

[0019] Furthermore, the cosmetic described in Patent Document 4 requires the use of hydrogen peroxide and an autoclave in its production, which is not necessarily satisfactory in terms of production safety and production efficiency.

[0020] The cosmetics described in Patent Document 5 leave a slightly bluish-white impression, and there is still room for improvement in terms of hiding power. The present inventors have determined that it is important to have appropriate hiding power in order to stably obtain cosmetics that are free of bluish tint and do not cause whitening.

[0021] In addition, the inventors of the present invention have focused on the fact that, in addition to relying on hiding power, there is also a method of lightening (Japanese: ぼかす) as a means of making spots on the skin less noticeable. In other words, it is believed that if a titanium oxide pigment with soft focus properties is used, it is not necessary to excessively increase hiding power and a natural impression that is less likely to cause whitening can be provided.

[0022] Therefore, an object of the present invention is to provide titanium (IV) oxide particles and cosmetics containing the particles, wherein the titanium (IV) oxide particles have soft focus and appropriate covering power in addition to light ductility, and when used in cosmetics, form a uniform cosmetic film, and further, due to the soft focus and appropriate covering power, can show a natural bare skin feeling.

[0023] Solutions for solving problems

[0024] As a result of conducting in-depth research on the above-mentioned subject, the present inventors have found that by using titanium (IV) oxide powder composed of peanut-shaped particles, the longest part of one particle of the peanut-shaped particles has a major axis diameter of 300 nm to 700 nm, the short axis diameter of the largest part in the direction perpendicular to the long axis is 100 nm to 400 nm, the diameter of the narrowed part in the direction perpendicular to the long axis at the center of the long axis is 80 nm to 200 nm, and the ratio of the narrowed part diameter to the short axis diameter is 0.9 or less. The present invention includes the following, but is not limited to them.

[0025] [1] A titanium (IV) oxide powder, which is composed of particles having a peanut-shaped twin shape, wherein the diameter of the longest part of one of the particles of the peanut-shaped twin shape is greater than 300 nm and less than 700 nm, the diameter of the short axis of the largest part in the direction perpendicular to the long axis is greater than 100 nm and less than 400 nm, the diameter of the narrowed portion in the direction perpendicular to the long axis at the center of the long axis is greater than 80 nm and less than 200 nm, and the ratio of the narrowed portion diameter / short axis diameter is less than 0.9.

[0026] [2] The titanium (IV) oxide powder according to [1], wherein the titanium (IV) oxide is rutile titanium oxide.

[0027] [3] A titanium (IV) oxide powder according to [1] or [2], wherein the aforementioned one particle is formed by aggregating fine rod-shaped particles in a peanut-like twin shape, and the fine rod-shaped particles have a major axis diameter of greater than 30 nm and less than 350 nm and a minor axis diameter of greater than 3 nm and less than 12 nm.

[0028] [4] A titanium (IV) oxide powder according to any one of [1] to [3], wherein a mixed solution of trimethylsiloxysilicate and cyclopentasiloxane in a mass ratio of 1:1 is used as a medium, and the mixture is stirred at 2000 rpm to prepare a coating having a powder concentration of 100 g / kg, and the coating is formed into a coating film using a rod coater with a film thickness of 18.4 μm, and the coating film is irradiated with light having a color temperature of 6774 K, i.e., C light, in a double-beam manner for measurement. The total light transmittance of the coating film is 45.0% or more and 60.0% or less, and the haze value is 90.0% or more.

[0029] [5] The titanium (IV) oxide powder according to any one of [1] to [4], wherein at least a portion of the surface of particles constituting the powder is covered with a layer of an inorganic substance and / or an organic substance.

[0030] [6] A powder of titanium (IV) oxide according to [5], wherein at least a portion of the surface of the particles constituting the powder is covered with a layer of an inorganic substance, and the layer of the inorganic substance comprises one or more of aluminum, silicon, zinc, titanium, zirconium, iron, cerium and tin.

[0031] [7] A titanium (IV) oxide powder according to [5], wherein at least a portion of the surface of the particles constituting the powder is covered with a layer of organic matter, and the layer of organic matter contains one or more of an organosilicon compound, a coupling agent, a fluorine compound and a fatty acid.

[0032] [8] A cosmetic comprising the titanium (IV) oxide powder according to any one of [1] to [7].

[0033] [9] A method for producing a titanium (IV) oxide powder as described in any one of [1] to [7], comprising step 1: adding hydrochloric acid to a slurry containing an acid-soluble titanium compound, adjusting the hydrochloric acid concentration to at least 60 g / L and at most 130 g / L, and adjusting the temperature to at least 25°C and at most 60°C and maintaining the temperature for at least 1 hour.

[0034]

[10] The production method according to [9], wherein in the aforementioned step 1, the steps of adjusting the aforementioned hydrochloric acid concentration to 80 g / L or more and 130 g / L or less and adjusting the aforementioned temperature to 35°C or more and 45°C or less are included.

[0035]

[11] The manufacturing method according to [9] or

[10] , wherein step 2 is further included after step 1: adjusting the hydrochloric acid concentration and / or temperature to a value higher than step 1 within the range of hydrochloric acid concentration below 180 g / L and temperature below 100°C and maintaining the concentration for more than 1 hour.

[0036]

[12] The production method according to

[11] , further comprising step 3 of calcining after step 2.

[0037] Effects of the Invention

[0038] The titanium (IV) oxide powder of the present invention, when added to cosmetics, especially color cosmetics, can form a uniform makeup film and show a natural bare skin feeling. In addition, the coating film containing the titanium (IV) oxide powder of the present invention has soft focus properties and appropriate hiding power. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a transmission electron microscope photograph showing peanut-shaped titanium (IV) oxide particles obtained in Example 1.

[0040] Figure 2 This is a transmission electron microscope photograph showing peanut-shaped titanium (IV) oxide particles obtained in Example 2.

[0041] Figure 3 This is a transmission electron microscope photograph showing peanut-shaped titanium (IV) oxide particles obtained in Example 3.

[0042] Figure 4 This is a transmission electron microscope photograph showing peanut-shaped titanium (IV) oxide particles obtained in Example 4.

[0043] Figure 5 This is a transmission electron microscope photograph showing peanut-shaped titanium (IV) oxide particles obtained in Example 5.

[0044] Figure 6 This is a transmission electron microscope photograph showing peanut-shaped titanium (IV) oxide particles obtained in Example 6.

[0045] Figure 7 This is a transmission electron microscope photograph showing titanium (IV) oxide particles obtained in Comparative Example 1.

[0046] Figure 8 This is a transmission electron microscope photograph showing titanium (IV) oxide particles obtained in Comparative Example 2. DETAILED DESCRIPTION

[0047] The present invention provides a powder composed of titanium (IV) oxide particles, wherein the titanium (IV) oxide particles have a peanut-shaped particle shape having a major axis diameter and a minor axis diameter within a specific range and a narrowed portion at the center. By making the particles have an appropriate size, it is possible to impart a good ductile touch to the cosmetics when they are mixed with cosmetics. In addition, by using this shape, it is possible to produce cosmetics that have smoothness, soft focus, and appropriate covering power, and have excellent uniformity when forming a cosmetic film, and that show a natural bare skin feel. In addition, the dispersibility when mixed with cosmetics is also excellent, and cosmetics with good touch can be provided.

[0048] For the titanium (IV) oxide particles constituting the powder of the present invention, the diameter of the longest part of the particles is 300 nm to 700 nm, the diameter of the short axis of the part that is the largest in the direction perpendicular to the long axis is 100 nm to 400 nm, and the diameter of the narrowed portion of the length in the direction perpendicular to the long axis at the center of the long axis is 80 nm to 200 nm. In addition, the ratio of the narrowed portion diameter / short axis diameter obtained by dividing the narrowed portion diameter by the short axis diameter is 0.9 or less. In this way, the particles constituting the powder of the present invention have a peanut-like twin shape with a narrowed portion at the center. In order to form a peanut-like twin shape, the diameter of the second largest part in the direction perpendicular to the long axis direction is preferably larger than the narrowed portion diameter. The larger the long axis diameter within the above range, the higher the transparency, and the more natural bare skin feeling cosmetics are obtained. However, when the long axis diameter is greater than 700 nm, the covering power becomes too small, and spots cannot be hidden. In addition, when the ratio of the narrowed portion diameter / short axis diameter is greater than 0.9, the soft focus property decreases. The lower limit of the major axis diameter is more preferably 350 nm or more, more preferably 400 nm or more, and the upper limit is more preferably 650 nm or less. The lower limit of the minor axis diameter is more preferably 110 nm or more, more preferably 150 nm or more, and the upper limit is more preferably 360 nm or less. The lower limit of the diameter of the narrowing portion is more preferably 85 nm or more, more preferably 100 nm or more, and the upper limit is more preferably 195 nm or less, and more preferably 180 nm or less. The ratio of the diameter of the narrowing portion / the minor axis diameter is more preferably 0.80 or less, and more preferably 0.60 or less. The lower limit of the ratio of the diameter of the narrowing portion / the minor axis diameter is not particularly limited, and is considered to be about 0.40.

[0049] The major axis diameter, minor axis diameter and constriction diameter of the particles can be measured by the following method:

[0050] About 300 particles were observed using a transmission electron microscope, and the major axis diameter, minor axis diameter, and constricted portion diameter defined above were measured, and their respective average values ​​were calculated.

[0051] In addition, the ratio of the narrowing diameter / minor axis diameter of the particle can be obtained by the following method:

[0052] About 300 particles were observed using a transmission electron microscope. For each particle, the value of the narrowed portion diameter / minor axis diameter ratio was calculated from the values ​​of the minor axis diameter and the narrowed portion diameter defined above, and the values ​​were averaged to obtain the narrowed portion diameter / minor axis diameter ratio of the particle.

[0053] As described above, the titanium (IV) oxide powder of the present invention has light ductility, soft focus and moderate hiding power when combined with cosmetics. The reason is not clear, but it is considered as follows. The particles constituting the titanium (IV) oxide powder of the present invention are in a shape formed by connecting two particles with a particle size of 100nm to 400nm, so the optical properties as an aggregate are close to those of particles with a particle size of 100nm to 400nm. However, the number of times the incident light passes through the surface of the particles itself is reduced, so scattering and reflection are suppressed. On the other hand, the titanium (IV) oxide powder of the present invention has many spaces left inside the powder due to the shape of the particles constituting the powder, and the light incident on the powder is scattered at the boundary surface of the particles in the space. It is believed that these effects counteract each other, resulting in soft focus and moderate hiding power. In addition, it is believed that the powder of the present invention has a smaller specific surface area than an aggregate of particles with a particle size of 100nm to 400nm, and there are fewer contact points between the particles, so the ductility becomes good.

[0054] The titanium oxide (IV) in the powder of the present invention is preferably rutile titanium oxide (IV). Compared with anatase titanium oxide, rutile titanium oxide has a weaker blue hue and less activity. In addition, compared with titanium oxide (IV) of crystalline phases other than rutile and anatase, it is excellent in manufacturability and stability. The crystalline phase of titanium oxide (IV) can be determined by confirming the main peaks of each crystalline phase (e.g., the diffraction intensity of the (110) plane of rutile titanium oxide (IV)) using an X-ray diffraction device.

[0055] Each particle constituting the powder of titanium (IV) oxide of the present invention can be formed by aggregating fine rod-shaped particles in a peanut-like twin shape, wherein the major axis diameter of the fine rod-shaped particles is 30 nm or more and 350 nm or less, and the minor axis diameter is 3 nm or more and 12 nm or less. In the case where a peanut-like twin shape is formed by aggregating fine rod-shaped particles, the lasting property of the cosmetic can be improved when combined with cosmetics. The reason is not clear, but it is believed that when individual particles of a peanut-like twin shape are formed by aggregating rod-shaped particles, many fine gaps are generated on the surface of the particles, so that excess sebum and sweat are gradually absorbed by the fine gaps, thereby improving the lasting property of the cosmetic. The lower limit of the major axis of the fine rod-shaped particles is preferably 150 nm or more, more preferably 200 nm or more, the upper limit is preferably 325 nm, more preferably 300 nm or less, and the lower limit of the minor axis of the fine rod-shaped particles is preferably 8 nm or more, and the upper limit is 11 nm or less.

[0056] The major axis diameter and the minor axis diameter of the fine rod-shaped particles are average values ​​of the major axis diameters and the minor axis diameters of about 300 fine rod-shaped particles observed using a transmission electron microscope.

[0057] It should be noted that by calcining particles in which fine rod-like particles are assembled in a peanut-like twin shape so as to fuse the fine rod-like particles to each other, a single particle having a peanut-like twin shape can be produced. The particles constituting the powder of the present invention include particles in which fine rod-like particles (not fused) are assembled to form one particle on the surface and particles in which fine rod-like particles are fused to form one particle. In the former case, as described above, when combined with cosmetics, the effect of improving the lasting makeup is obtained. In addition, in the latter case, cosmetics with better covering power can be obtained.

[0058] The powder of titanium (IV) oxide of the present invention preferably has a total light transmittance of 45.0% or more and 60.0% or less, and a haze value of 90.0% or more. When a powder having such a total light transmittance and haze value is combined with cosmetics, it has soft focus and moderate covering power, and can show a natural bare skin feel. Preferably, the lower limit of the total light transmittance is 50.0% or more, the upper limit is 60.0% or less, and the lower limit of the haze value is 91.0% or more. The upper limit of the haze value is not particularly limited and can be 100.0%. The method for determining the total light transmittance and the haze value is as follows:

[0059] The powder was added to a 1:1 mixture of trimethylsiloxysilicate and cyclopentasiloxane, and the mixture was stirred at 2000 rpm to prepare a coating having a powder concentration of 100 g / kg. The coating was formed into a coating film using a rod coater with a film thickness of 18.4 μm, and irradiated with light having a color temperature of 6774 K, i.e., C light, in a double-beam method, and the total light transmittance and haze value of the coating film were measured.

[0060] The entirety or at least a portion of the surface of the particles constituting the powder of the present invention may be covered by an inorganic and / or organic layer. As an inorganic substance, one or more of aluminum, silicon, zinc, titanium, zirconium, iron, cerium and tin may be included, preferably their oxides, hydroxides or oxyhydroxides. In addition, as an organic substance, one or more of organic silicon compounds such as dimethylpolysiloxane, methylhydrogenpolysiloxane, coupling agents such as silane, aluminum, titanium and zirconium, fluorine compounds such as perfluoroalkyl phosphoric acid compounds and fatty acids such as lauric acid and stearic acid may be preferably used. In addition, hydrocarbons, lecithin, amino acids, polyethylene, waxes, etc. may also be used.

[0061] The titanium (IV) oxide powder of the present invention can be contained in cosmetics. The amount of titanium (IV) oxide powder in cosmetics varies depending on the form of the cosmetics, but is generally preferably 1 g / kg to 500 g / kg, and more preferably 10 g / kg to 450 g / kg.

[0062] (Manufacturing method)

[0063] The peanut-shaped titanium (IV) oxide particles constituting the powder of the present invention can be obtained by a method comprising the following steps: step 1, adding hydrochloric acid to a slurry containing an acid-soluble titanium compound so that the hydrochloric acid concentration is 60 g / L or more and 130 g / L or less, and heating and hydrolyzing the slurry at a temperature of 25°C or more and 60°C or less for more than one hour; and step 2, heating and hydrolyzing the slurry at a higher hydrochloric acid concentration and / or temperature than that in step 1 for more than one hour.

[0064] The acid-soluble titanium compound used in the present invention may be any titanium compound soluble in hydrochloric acid, such as titanium hydroxide and sodium titanate. As such an acid-soluble titanium compound, sodium titanate is particularly preferred.

[0065] In the hydrolysis reaction of step 1, as described above, the hydrochloric acid concentration is adjusted to 60 g / L or more and 130 g / L or less, and the temperature is adjusted to 25° C. or more and 60° C. or less and maintained. The lower limit of the hydrochloric acid concentration is more preferably 70 g / L or more, and more preferably 80 g / L or more. The lower limit of the temperature is more preferably 30° C. or more, and more preferably 35° C. or more, and the upper limit is more preferably 50° C. or less, and more preferably 45° C. or less. The holding time is not particularly limited as long as it is more than 1 hour. From the perspective of energy efficiency, it is preferably shorter, preferably 1 hour or more and 10 hours or less, and more preferably 2 hours or more and 5 hours or less.

[0066] In the hydrolysis reaction of step 2, at least one of the hydrochloric acid concentration and the temperature is made higher than that of step 1. In step 2, it is more preferred to adjust both the hydrochloric acid concentration and the temperature to be higher than that of step 1. In addition, in step 2, the upper limit of the hydrochloric acid concentration is set to 180 g / L or less, and the upper limit of the temperature is set to 100°C or less. The upper limit of the hydrochloric acid concentration is preferably 170 g / L or less, more preferably 160 g / L or less, and the temperature is preferably 70°C or less, and more preferably 65°C or less. The lower limits of the hydrochloric acid concentration and the temperature are not particularly limited, and are preferably not lower than step 1, so they are preferably 60 g / L or more and 25°C or more, respectively. The retention time in step 2 is not particularly limited as long as it is more than 1 hour, and is preferably more than 1 hour and less than 30 hours, and more preferably more than 10 hours and less than 20 hours.

[0067] The hydrolysis reaction may be carried out three or more times. The conditions for the third and subsequent times are not particularly limited, but in consideration of the equipment required for the hydrolysis, it can be said that it is preferably carried out under conditions close to those of the first and second times.

[0068] The sample after hydrolysis is preferably cooled, filtered, cleaned and recovered by keeping the solution at a certain temperature to precipitate titanium (IV) oxide. The precipitation conditions are not limited, preferably kept at 60°C or more and 100°C or less for more than 1 hour. The upper limit of the holding time during precipitation is not particularly limited, preferably less than 8 hours. The method of cooling, filtering and cleaning is not particularly limited. It is preferably carried out according to the usual steps in the art.

[0069] The titanium (IV) oxide obtained through the above-mentioned steps 1 and 2 can be further calcined (step 3). The titanium (IV) oxide particles having a peanut-shaped twin shape of the present invention can further improve the covering power of the cosmetics when mixed with cosmetics by calcining as needed. The calcination temperature is preferably 700°C or less. When calcining is performed at a temperature higher than 700°C, excessive sintering proceeds, so it is possible that peanut-shaped twin particles that meet the scope of the present invention cannot be obtained, and the natural bare skin feeling when the particles are used in cosmetics may be lost. The lower limit of the calcination temperature is not particularly limited, but as a reference, it is preferably 300°C or more. When the calcination temperature is lower than 300°C, the performance change is small compared to the case where calcination is not performed, so the value of industrial calcination is small. The holding time is preferably 10 minutes or more and 60 minutes or less. If it is kept for more than 60 minutes, excessive sintering proceeds, and it is possible that peanut-shaped twin particles that meet the scope of the present invention cannot be obtained. When the holding time is shorter than 10 minutes, heat unevenness may occur in the powder and the quality becomes uneven, which is not preferred in industry. More preferably, the time is 20 minutes to 50 minutes.

[0070] The particles of titanium oxide (IV) obtained above (including calcined products and non-calcined products) can cover at least a portion of the particle surface with a layer of inorganic and / or organic matter. The method of imparting the covering is not particularly limited, and a commonly used method can be used. By covering at least a portion of the particle surface with a layer of inorganic matter, for example, the dispersion stability and durability in the dispersion medium can be improved. As the inorganic matter that can be used, for example, one or more of metals such as aluminum, silicon, zinc, titanium, zirconium, iron, cerium and tin can be used. Preferably, their oxides, hydroxides or oxyhydroxides. The type of the metal salt is not limited in any way.

[0071] In addition, according to the purpose of cosmetics, by covering at least a part of the particle surface with an organic layer, the particles can be subjected to water-repellent and / or oil-repellent treatment. As organic matter, organic silicon compounds such as dimethylpolysiloxane, methylhydrogenpolysiloxane, coupling agents such as silane, aluminum, titanium and zirconium, fluorine compounds such as perfluoroalkyl phosphoric acid compounds, hydrocarbons, lecithin, amino acids, polyethylene, waxes, fatty acids such as lauric acid and stearic acid, etc. can be listed.

[0072] (use)

[0073] The titanium (IV) oxide powder of the present invention is not particularly limited in its use, but is particularly suitable for use in cosmetics. The powder of the present invention can impart soft-focus properties and appropriate covering power to cosmetics without sticking.

[0074] When the titanium (IV) oxide powder of the present invention is used in cosmetics, other cosmetic raw materials can be mixed with the powder according to a known method. The powder is preferably pre-covered with the aforementioned surface. When mixed with other cosmetic raw materials, the powder can be directly mixed with the other raw materials, or the powder can be dispersed in a dispersion medium to form a dispersion, and then the dispersion is mixed with the other raw materials. In the present invention, the term "cosmetics containing titanium (IV) oxide powder" includes not only cosmetics containing titanium (IV) oxide powder directly (in the form of powder), but also cosmetics obtained by dispersing the powder in a dispersion medium to form a dispersion and then adding it to cosmetics. The content of the titanium (IV) oxide powder of the present invention in cosmetics can be arbitrarily set according to the required characteristics of various cosmetics, preferably more than 1 g / kg and less than 500 g / kg, more preferably more than 10 g / kg and less than 450 g / kg. Two or more titanium (IV) oxide powders of the present invention composed of peanut-shaped particles having different major axis diameters, minor axis diameters, and narrowed portion diameters may be mixed and used, and titanium oxide of different particle sizes and / or shapes may be further formulated into cosmetics containing the powders of the present invention as needed.

[0075] In the case of obtaining a cosmetic containing the titanium (IV) oxide powder of the present invention, various components such as inorganic pigments and organic pigments used in general cosmetics can be used in combination as needed. As inorganic pigments that can be used in combination, titanium oxide, zinc oxide, red iron oxide, yellow iron oxide, black iron oxide, brown iron oxide, ultramarine, Prussian blue, cerium oxide, talc, muscovite, synthetic mica, phlogopite, biotite, synthetic fluorphlogopite, mica titanium, mica-like iron oxide, sericite, zeolite, kaolin, bentonite, clay, silicic acid, anhydrous silicic acid, magnesium silicate, aluminum silicate, calcium silicate, barium sulfate, magnesium sulfate, calcium sulfate, calcium carbonate, magnesium carbonate, boron nitride, bismuth oxychloride, aluminum oxide, zirconium oxide, magnesium oxide, chromium oxide, calamine, hydroxyapatite, and complexes thereof can be used. As for the organic pigments that can be used in combination, silicone powder, silicone elastic powder, polyurethane powder, cellulose powder, nylon powder, urethane powder, silk powder, polymethyl methacrylate (PMMA) powder, starch, polyethylene powder, polystyrene powder, carbon black, tar pigment, natural pigment, metal soaps such as zinc stearate, and their complexes can be used.

[0076] The cosmetics containing the titanium (IV) oxide powder of the present invention may contain other ingredients as required in addition to the above-mentioned ingredients within the range of quantity and quality that do not impair the effects of the present invention. For example, oily ingredients, pigments, pH adjusters, moisturizers, thickeners, surfactants, dispersants, stabilizers, colorants, preservatives, antioxidants, metal chelating agents, astringents, anti-inflammatory agents, ultraviolet absorbers, fragrances, etc. may be appropriately mixed within the range that does not impair the effects of the present invention.

[0077] Cosmetics containing the powder of titanium (IV) oxide of the present invention can be manufactured by a known method. As the dosage form of the cosmetics, it can be in any state of powder, powder solid, cream, emulsion, lotion, oily liquid, oily solid, paste, etc. For example, it can be made into makeup base, foundation, concealer, face powder, toner, sunscreen, lipstick, lip balm, eye shadow, eyeliner, mascara, blush, nail polish, talcum powder, perfume powder, baby powder and other color cosmetics, skin care cosmetics, hair care cosmetics, etc.

[0078] The titanium (IV) oxide powder of the present invention can be used in various fields where titanium oxide is usually used in addition to cosmetics. Specifically, it can be used in resin compositions, coatings, inks, toner additives, photocatalysts, electrical / electronic materials, ultraviolet shielding materials, thermal insulation materials, radio wave shielding materials, ultraviolet shielding materials, etc., but is not limited thereto.

[0079] For example, it is believed that the powder of titanium oxide (IV) of the present invention has the characteristic of being easy to generate gaps between particles due to its particle shape, and when added to a resin, the effect of preventing the generation of so-called dough is obtained. In addition, since there are few contact points between the particles, it is believed that fluidity can be maintained when used for ink and coating. In addition, it is believed that the powder of titanium oxide (IV) of the present invention has electrical and mechanical characteristics that titanium oxide (IV) has not had so far due to its special shape, and it is believed that its new characteristics can be applied to the field of electrical / electronic materials. That is, cosmetics, resin compositions, coatings, inks or electrical / electronic materials containing the powder of titanium oxide (IV) of the present invention are one mode of the present invention. In addition, from other viewpoints, the use of the powder of titanium oxide (IV) of the present invention in cosmetics, resin compositions, coatings, inks or electrical / electronic materials is also a mode of the present invention. In addition, for example, the use of the powder of titanium oxide (IV) of the present invention in the manufacture of cosmetics, resin compositions, coatings, inks, or electrical / electronic materials can also be said to be a mode of the present invention.

[0080] Before describing the examples, the test methods used in the present invention will be described.

[0081] [Evaluation items and evaluation methods]

[0082] (major axis diameter, minor axis diameter, constriction diameter and ratio of constriction diameter to minor axis diameter)

[0083] The measurement was performed using a transmission electron microscope JEM-1400plus manufactured by JEOL Ltd. The observation magnification was set to 50,000 times (10,000 times the observation magnification of the transmission electron microscope × 5 times the printing). The length of the longest part of each particle was set to the major axis diameter, the maximum length in the direction perpendicular to the major axis was set to the minor axis diameter, and the length in the direction perpendicular to the major axis at the center of the major axis was set to the constriction diameter. The image analysis software ImageJ was used to evaluate the major axis diameter, minor axis diameter and constriction diameter of about 300 particles in the observation field of view. The average value of the length of the diameter of each of about 300 particles was used as the major axis diameter, minor axis diameter and constriction diameter in the present invention. In addition, for about 300 particles, the constriction diameter was divided by the minor axis diameter, and the value of the constriction diameter / minor axis diameter was calculated, and the average value was calculated, which was used as the "constriction diameter / minor axis diameter ratio".

[0084] (Crystalline Phase)

[0085] Using an X-ray diffraction apparatus RINT-TTRIII manufactured by Rigaku Corporation, with a copper (Cu) target, a tube voltage of 50 kV, a tube current of 300 mA, a divergence slit of 1 / 2°, a divergence longitudinal slit of 10 mm, a scattering slit of 1 / 2°, a receiving slit of 0.15 mm, and a scanning speed of 0.5° / min, the diffraction intensities of the (110) plane of rutile titanium dioxide (IV) and the (101) plane of anatase titanium dioxide (IV) were measured at a 2θ scan range of 20° to 35°.

[0086] (Coverage)

[0087] 30.0 g of commercially available acrylic clear paint for automobile repair, 5.0 g of butyl acetate, and 10.0 g of titanium (IV) oxide powder were weighed in a 140 mL mayonnaise bottle, and a 30 mm diameter impeller was installed on a DISPERMAT FE / S manufactured by VMA-GETZMANN, and the mixture was dispersed at a rotation speed of 5000 rpm for 20 minutes to obtain a dispersion. 0.5 g of the dispersion was collected, and the mixture was dispersed by rotating 50 times with a load of 150 Lbs using a Hoover Muller, and then applied to a hiding test paper Lot. NA220022 manufactured by MotoFuji Co., Ltd. using a 3 mil applicator, and then dried. The color tone was measured using an SM-7 color computer manufactured by Suga Test Instruments Co., Ltd., and the ratio of the L value of the black background / the L value of the white background was taken as the hiding rate.

[0088] (Total transmittance and haze value)

[0089] 1 g of the sample was added to 9.0 times the mass of trimethylsiloxysilicate KF-7312J (a mixture of trimethylsiloxysilicate and cyclopentasiloxane in a mass ratio of 1:1) manufactured by Shin-Etsu Chemical Industry, and stirred at 2000 rpm using LABOLUTION (registered trademark) manufactured by PRIMIX Corporation to prepare a coating having a powder concentration of 100 g / kg. The coating was made into a coating film using a rod coater having a film thickness of 18.4 μm. The obtained coating film was air-dried with cold air from a dryer until the surface was dry, and a haze meter HZ-V3 manufactured by Suga Test Instruments Co., Ltd. was used to irradiate light, i.e., C light, with a color temperature of 6774 K in a double-beam manner to measure the diffuse transmittance and total light transmittance. The haze value was calculated by (diffuse transmittance / total light transmittance) × 100.

[0090] Example

[0091] The present invention will be described in more detail with reference to the following examples. The following examples are provided for illustration only and the scope of the invention is not limited thereto.

[0092] It should be noted that, in the stirring operation recorded in the embodiments and comparative examples, the properties related to the behavior of the liquid during stirring, such as the amount of liquid, the viscosity of the liquid, the shape of the container, etc., are considered, and the rotating speed is appropriately adjusted so that the liquid as a whole is uniformly mixed and the foam does not scatter around. In addition, in the case where sodium hydroxide, etc., as long as it is a general commercial product, the product of whichever enterprise is used can obtain the same effect, the enterprise name of the manufacturer and the distributor is omitted.

[0093] [Example 1]

[0094] Commercially available sodium titanate was dissolved in a mixture of water and 400 g / L of hydrochloric acid to prepare a sodium titanate slurry with a TiO2 concentration of 80 g / L and a hydrochloric acid concentration of 130 g / L. Next, the slurry was stirred and heated using HEIDON (registered trademark) 600G (hereinafter referred to as "mixer") manufactured by Shinto Science Co., Ltd., and stirred and maintained at a liquid temperature of 40°C for 3 hours, thereby performing the first hydrolysis. Next, 400 g / L of hydrochloric acid was added to the solution, and the hydrochloric acid concentration was adjusted to 150 g / L while heating the solution to a liquid temperature of 45°C and stirring and maintaining for 17 hours, thereby performing the second hydrolysis. Then, the liquid temperature was increased and maintained at 80°C for 8 hours, thereby precipitating titanium oxide (IV), and the solution was cooled, filtered, and washed to obtain a white powder.

[0095] Figure 1 A transmission electron microscope photograph of the obtained titanium (IV) oxide powder is shown. The obtained titanium (IV) oxide powder is a peanut twin-shaped particle formed by a collection of fine rod-shaped particles with a long axis of 280 nm and a short axis of 10 nm. The long axis diameter measured by the above method is 560 nm, the short axis diameter is 310 nm, the narrowing diameter is 170 nm, and the ratio of the narrowing diameter to the short axis diameter is 0.55. In addition, the crystalline phase was confirmed by an X-ray diffraction device, and the main peak came from rutile titanium (IV) oxide. The coverage is 0.83, the total transmittance is 52.0%, the diffuse transmittance is 48.4%, and the haze value is 93.0%.

[0096] [Example 2]

[0097] In the first hydrolysis, except that the concentration of hydrochloric acid was adjusted to 120 g / L, the same procedure as in Example 1 was carried out to obtain a white powder of titanium (IV) oxide. Figure 2The transmission electron microscope photograph of the obtained titanium oxide (IV) powder is shown. The obtained titanium oxide (IV) powder is a peanut twin-shaped particle formed by a collection of fine rod-shaped particles with a long axis of 265nm and a short axis of 10nm, with a long axis diameter of 530nm, a short axis diameter of 260nm, a narrowing diameter of 150nm, and a ratio of narrowing diameter to short axis diameter of 0.58. The main peak comes from rutile titanium oxide (IV). The measured values ​​of the hiding power, total light transmittance, diffuse transmittance and haze value are shown in Table 3.

[0098] [Example 3]

[0099] In the first hydrolysis, except that the concentration of hydrochloric acid was adjusted to 110 g / L, the same procedure as in Example 1 was carried out to obtain a white powder of titanium (IV) oxide. Figure 3 The transmission electron microscope photograph of the obtained titanium oxide (IV) powder is shown. The obtained titanium oxide (IV) powder is a peanut twin-shaped particle formed by a collection of fine rod-shaped particles with a long axis of 210nm and a short axis of 10nm, with a long axis diameter of 420nm, a short axis diameter of 180nm, a narrowing diameter of 110nm, and a ratio of narrowing diameter to short axis diameter of 0.61. The main peak comes from rutile titanium oxide (IV). The measured values ​​of the hiding power, total light transmittance, diffuse transmittance and haze value are shown in Table 3.

[0100] [Example 4]

[0101] In the first hydrolysis, except that the concentration of hydrochloric acid was adjusted to 80 g / L, the same procedure as in Example 1 was carried out to obtain a white powder of titanium (IV) oxide. Figure 4 The transmission electron microscope photograph of the obtained titanium oxide (IV) powder is shown. The obtained titanium oxide (IV) powder is a peanut twin-shaped particle formed by a collection of fine rod-shaped particles with a long axis of 185nm and a short axis of 10nm, with a long axis diameter of 370nm, a short axis diameter of 110nm, a narrowing diameter of 85nm, and a ratio of narrowing diameter to short axis diameter of 0.77. The main peak comes from rutile titanium oxide (IV). The measured values ​​of the hiding power, total light transmittance, diffuse transmittance and haze value are shown in Table 3.

[0102] [Example 5]

[0103] In the second hydrolysis, except that the hydrochloric acid concentration was adjusted to 160 g / L, the same procedure as in Example 1 was carried out to obtain a white powder of titanium (IV) oxide. Figure 5The transmission electron microscope photograph of the obtained titanium oxide (IV) powder is shown. The obtained titanium oxide (IV) powder is a peanut twin-shaped particle formed by a collection of fine rod-shaped particles with a long axis of 320nm and a short axis of 10nm, with a long axis diameter of 640nm, a short axis diameter of 360nm, a narrowing diameter of 180nm, and a ratio of narrowing diameter to short axis diameter of 0.50. The main peak comes from rutile titanium oxide (IV). The measured values ​​of the hiding power, total light transmittance, diffuse transmittance and haze value are shown in Table 3.

[0104] [Example 6]

[0105] The titanium (IV) oxide powder obtained in Example 5 was calcined at 650° C. for 30 minutes using SUPER-C C-2035D manufactured by MOTOYAMA CO., LTD., and then cooled to room temperature to obtain a white powder. Figure 6 A transmission electron microscope photograph of the obtained titanium (IV) oxide powder is shown. The obtained titanium (IV) oxide powder consists of particles having a peanut-shaped twin shape, with a major axis diameter of 610 nm, a minor axis diameter of 355 nm, a narrowed portion diameter of 195 nm, and a narrowed portion diameter / minor axis diameter ratio of 0.55. The fine rod-shaped particles observed in Examples 1 to 5 could not be observed. The main peak comes from rutile titanium (IV) oxide. The measured values ​​of the hiding power, total transmittance, diffuse transmittance and haze value are shown in Table 3.

[0106] [Comparative Example 1]

[0107] In the first hydrolysis, except that the concentration of hydrochloric acid was adjusted to 50 g / L, the same procedure as in Example 1 was carried out to obtain a white powder of titanium (IV) oxide. Figure 7 The transmission electron microscope photograph of the obtained titanium oxide (IV) powder is shown. The obtained titanium oxide (IV) powder is a particle with a strip shape formed by a collection of fine rod-shaped particles with a long axis of 120nm and a short axis of 10nm, with a long axis diameter of 240nm, a short axis diameter of 55nm, a narrowing diameter of 50nm, and a ratio of narrowing diameter to short axis diameter of 0.91. The main peak comes from rutile titanium oxide (IV). The measured values ​​of the hiding power, total light transmittance, diffuse transmittance and haze value are shown in Table 3.

[0108] [Comparative Example 2]

[0109] In the first hydrolysis, the same procedure as in Example 5 was carried out except that the hydrochloric acid concentration was adjusted to 140 g / L to obtain a white powder of titanium (IV) oxide. Figure 8The transmission electron microscope photo of the obtained titanium oxide (IV) powder is shown. The obtained titanium oxide (IV) powder is an aggregated particle without a narrowing portion formed by a collection of fine rod-shaped particles with a long axis of 410nm and a short axis of 10nm. The long axis diameter is 820nm, the short axis diameter is 490nm, the narrowing portion diameter (the diameter perpendicular to the long axis at the center of the long axis) is 540nm, and the ratio of the narrowing portion diameter to the short axis diameter is 1.10. The main peak comes from rutile titanium oxide (IV). The measured values ​​of the hiding power, total light transmittance, diffuse transmittance and haze value are shown in Table 3.

[0110] [Comparative Example 3]

[0111] A powder of commercially available rutile titanium (IV) oxide used in cosmetics was prepared. The powder of titanium oxide was composed of amorphous particles, with a major axis diameter of 340 nm, a minor axis diameter of 240 nm, a narrowed portion diameter of 240 nm, and a narrowed portion diameter / minor axis diameter ratio of 1.00. The measured values ​​of the hiding power, total light transmittance, diffuse transmittance, and haze value are shown in Table 3.

[0112] Table 1 shows the production conditions of the titanium (IV) oxide powders of Examples and Comparative Examples, Table 2 shows the properties of the particles constituting the titanium (IV) oxide powders obtained in Examples and Comparative Examples, and Table 3 shows the properties of the titanium (IV) oxide powders of Examples and Comparative Examples.

[0113] [Table 1]

[0114]

[0115] [Table 2]

[0116]

[0117] [Table 3]

[0118]

[0119] As can be seen from Table 3, the covering power of the titanium (IV) oxide powder obtained in Examples 1 to 6 is greater than that of Comparative Examples 1 and 2. It is expected that the titanium (IV) oxide powder of Examples 1 to 6 will impart appropriate covering power to the cosmetics when formulated in cosmetics. In addition, the haze value of the powder obtained in Examples 1 to 6 is as large as that of the titanium oxide of Comparative Example 3, which is commercially available, and the total light transmittance is greater than that of Comparative Example 3. Therefore, it is expected that the cosmetics formulated with the powder of Examples 1 to 6 will have excellent soft focus properties in addition to covering power.

[0120] (cosmetic)

[0121] The cosmetics containing the titanium (IV) oxide powder of the present invention will be described below.

[0122] [Formula Example 1: Powder Foundation]

[0123] The powders (titanium oxide samples) obtained in Examples and Comparative Examples were blended to prepare powder foundations.

[0124]

[0125]

[0126] (Note 1) Rheopearl (registered trademark) manufactured by Chiba Flour Milling Co., Ltd.) ISK

[0127] (Note 2) The surface was treated with KF-9909 manufactured by Shin-Etsu Chemical Co., Ltd.

[0128] (Manufacturing method)

[0129] A: Components 11 to 13 were stirred and mixed using LAB. MIXER LM-110T (hereinafter referred to as "Henschel mixer") manufactured by HANIL Electric Co., Ltd.

[0130] B: Add A to components 1 to 10 and disperse evenly using a Henschel mixer.

[0131] C: In another container, heat and dissolve components 14 to 18.

[0132] D: Add C to B and emulsify, then cool to room temperature to obtain a powder foundation.

[0133] (Sensory Evaluation)

[0134] The obtained powder foundation was subjected to sensory tests on ductility, smoothness, hiding power, whitening and makeup lastingness.

[0135] [Evaluation and evaluation criteria]

[0136] Ten panelists were asked to use the powder foundations prepared using the powders of Examples 1 to 6 and Comparative Examples 1 to 3, and to perform sensory evaluation on the sensory test items in Table 4 in five grades, and the evaluation was made based on the average score.

[0137] (Evaluation Criteria)

[0138] Very good: 5 points Good: 4 points Average: 3 points Slightly poor: 2 points Poor: 1 point

[0139] (Judgment Criteria)

[0140] Average score of 4.0 or higher and 5.0 or lower: A

[0141] 3.0 or more and less than 4.0: B

[0142] 2.0 or more and less than 3.0: C

[0143] 1.0 or more and less than 2.0: D.

[0144] The results are shown in Table 4.

[0145] [Table 4]

[0146] Ductility Smoothness Covering power Whitening Long-lasting makeup Example 1 A A A B B Example 2 A B B B B Example 3 B B B B B Example 4 B B C A B Example 5 A A B B B Example 6 A A A B B Comparative Example 1 C C C A C Comparative Example 2 B B C B B Comparative Example 3 D D A D C

[0147] The results of the sensory test showed that the powder foundations containing the powders obtained in Examples 1 to 6 had excellent spreadability, smoothness, hiding power, and long-lasting makeup, and were not prone to whitening. By incorporating the titanium (IV) oxide powder composed of peanut-shaped particles of the present invention into cosmetics, light spreadability, soft focus, and moderate hiding power were imparted to the cosmetics. As a result, a cosmetic with excellent uniformity of the makeup film, reduced spots and pores, and a natural bare skin feeling can be provided.

[0148] [Formula Example 2: W / O emulsified foundation]

[0149] A W / O emulsified foundation was prepared using the powder obtained in Example.

[0150]

[0151] (Note 1) KSG-210 manufactured by Shin-Etsu Chemical Co., Ltd.

[0152] (Note 2) KSG-15 manufactured by Shin-Etsu Chemical Co., Ltd.

[0153] (Note 3) The surface was treated with KF-9909 manufactured by Shin-Etsu Chemical Co., Ltd.

[0154] (Manufacturing method)

[0155] A: Components 1 to 5 were uniformly mixed using LABOLUTION (registered trademark) manufactured by PRIMIX Corporation (hereinafter referred to as a "mixer"), and component 6 was further uniformly dispersed using a Henschel mixer.

[0156] B: Components 7 to 11 are uniformly mixed using a mixer.

[0157] C: B is slowly added to A under stirring to emulsify and obtain a W / O emulsified foundation.

[0158] The obtained W / O emulsion foundation has excellent spreadability, and even after application, it has soft focus and moderate coverage without causing whitening, and it reduces spots and pores, giving a natural bare skin finish.

[0159] [Formulation Example 3: W / O Cream]

[0160] The powder obtained in the example was used to prepare a W / O cream.

[0161]

[0162] (Note 1) KSG-210 manufactured by Shin-Etsu Chemical Co., Ltd.

[0163] (Note 2) KSG-15 manufactured by Shin-Etsu Chemical Co., Ltd.

[0164] (Note 3) KF-6028 manufactured by Shin-Etsu Chemical Co., Ltd.

[0165] (Note 4) KP-575 manufactured by Shin-Etsu Chemical Co., Ltd.

[0166] (Note 5) The surface was treated with KF-9909 manufactured by Shin-Etsu Chemical Co., Ltd. (manufacturing method)

[0167] A: Mix ingredients 1 to 8 and disperse them uniformly.

[0168] B: Mix and dissolve components 10 to 12.

[0169] C: Add B to A and mix well.

[0170] D: Add ingredient 9 to C and mix well to obtain a W / O cream.

[0171] The obtained W / O cream has light ductility, no astringency, and excellent adhesion. [Formulation Example 4: W / O emulsion type sunscreen]

[0172] The powder obtained in the example was used to prepare a W / O emulsion type sunscreen.

[0173]

[0174] (Note 1) Surface treatment with AES-3083 manufactured by Shin-Etsu Chemical Co., Ltd. (Note 2) Surface treatment with KF-9909 manufactured by Shin-Etsu Chemical Co., Ltd. (Note 3) KSP-300 manufactured by Shin-Etsu Chemical Co., Ltd.

[0175] (Note 4) KMP-590 manufactured by Shin-Etsu Chemical Co., Ltd.

[0176] (Note 5) KSG-16 manufactured by Shin-Etsu Chemical Co., Ltd.

[0177] (Manufacturing method)

[0178] A: Components 1 to 13 are mixed and pulverized uniformly.

[0179] B: Components 15 to 17 are uniformly mixed using a mixer, and added to A to make the entire mixture uniform.

[0180] C: Component 14 is added to B and the mixture is press-formed in a mold to obtain a W / O emulsion type sunscreen.

[0181] The obtained W / O emulsion type sunscreen has very light spreadability, no stickiness, and excellent adhesion.

[0182] [Formula Example 5: Pressed Powder Foundation 1]

[0183] The powder obtained in the example was used to prepare a pressed powder foundation.

[0184]

[0185] (Note 1) Matsumoto Microsphere M-100 manufactured by Matsumoto Oil & Fats Co., Ltd.

[0186] (Note 2) SUNLOVELY (registered trademark) manufactured by AGC Si-Tech Co., Ltd.

[0187] (Manufacturing method)

[0188] A: Components 1 to 7 are mixed and ground.

[0189] B: Transfer A to a Henschel mixer, add ingredients 8 to 12 and stir until uniform.

[0190] C: B was pulverized using a sample mill TASM-1 manufactured by TOKYO ATOMIZER MFG.CO., LTD. (hereinafter referred to as "atomizer"), and the pulverized powder was pressed into an aluminum dish to obtain a pressed powder foundation.

[0191] The resulting pressed powder foundation has excellent spreadability, and even after application, it has soft focus properties and moderate coverage without causing whitening, and it reduces spots and pores, giving a natural bare skin finish.

[0192] [Formula Example 6: Pressed Powder Foundation 2]

[0193] The powder obtained in the example was used to prepare a pressed powder foundation.

[0194]

[0195] (Note 1) BBR-213HP made by Titan Kogyo, Ltd.

[0196] (Note 2) COSMOL (registered trademark) manufactured by The Nisshin OilliO Group, Ltd.) 168ARV

[0197] (Manufacturing method)

[0198] A: Components 1 to 6 are mixed and ground.

[0199] B: Transfer A to a Henschel mixer, add ingredients 8 to 12 and stir until uniform.

[0200] C: B was crushed with an atomizer and pressed into an aluminum dish to obtain a pressed powder foundation.

[0201] The resulting pressed powder foundation has excellent spreadability, and even after application, it has soft focus properties and moderate coverage without causing whitening, and it reduces spots and pores, giving a natural bare skin finish.

[0202] [Formula Example 7: Dual-Purpose Pressed Powder]

[0203] The powder obtained in the example was used to prepare a dual-purpose pressed powder.

[0204]

[0205]

[0206] (Note 1) The surface was treated with KF-99P manufactured by Shin-Etsu Chemical Co., Ltd.

[0207] (Manufacturing method)

[0208] A: Heat to dissolve ingredients 9 to 13.

[0209] B: Components 1 to 8 were mixed using a Henschel mixer, and A was added thereto.

[0210] C: Crush B with an atomizer and press into shape in an aluminum dish to obtain a dual-purpose powder.

[0211] The obtained two-purpose pressed powder has excellent ductility, and even after application, it has soft focus properties and moderate coverage without causing whitening, and it can fade spots and pores, giving a natural bare skin finish.

[0212] [Formula Example 8: Oily Pressed Powder]

[0213] The powder obtained in the example was used to prepare an oil-based pressed powder.

[0214]

[0215]

[0216] (Note 1) The surface was treated with KF-9901 manufactured by Shin-Etsu Chemical Co., Ltd.

[0217] (Manufacturing method)

[0218] A: Components 1 to 6 were mixed with a Henschel mixer and pulverized uniformly.

[0219] B: Heat and dissolve ingredients 7 to 16, add A and stir evenly.

[0220] C: After degassing, pour B into a tray and slowly cool to room temperature to obtain an oil-based pressed powder.

[0221] The obtained oil-based pressed powder has excellent ductility, and even after application, it has soft focus properties and moderate coverage without causing whitening, and it reduces spots and pores, giving a natural bare skin finish.

[0222] [Formula Example 9: Foundation Stick]

[0223] A foundation stick was prepared using the powder obtained in the example.

[0224]

[0225]

[0226] (Note 1) The surface was treated with KF-99P manufactured by Shin-Etsu Chemical Co., Ltd.

[0227] (Manufacturing method)

[0228] A: Components 12 to 16 were mixed using a Henschel mixer.

[0229] B: Ingredients 1 to 11 are weighed in a container containing the entire amount and heated to dissolve.

[0230] C: In another container, weigh ingredients 17 to 21 and heat to dissolve.

[0231] D: Add A to B to evenly disperse it, and then add C to emulsify it.

[0232] E: After degassing, pour D into a mold and slowly cool to room temperature to obtain a foundation stick.

[0233] The obtained foundation stick has excellent ductility. In addition, even after application, it has soft focus and moderate coverage without causing whitening, and it can fade spots and pores, giving a natural bare skin finish.

[0234] [Formulation Example 10: O / W emulsified foundation]

[0235] An O / W emulsified foundation was prepared using the powder obtained in Example.

[0236]

[0237] (Manufacturing method)

[0238] A: Components 1 to 7 were heated and dissolved at 85°C.

[0239] B: Components 8 to 10 are mixed and ground.

[0240] C: Components 11 to 15 are heated to 85°C and dissolved and mixed.

[0241] D: Add B to A and disperse evenly, slowly add C thereto and emulsify, and stir and cool to room temperature. Next, fill in a suitable container to obtain an O / W emulsified foundation.

[0242] The obtained O / W emulsified foundation has excellent spreadability, and even after application, it does not cause whitening due to its soft focus and moderate coverage, and it reduces spots and pores, giving a natural bare skin finish.

[0243] [Formula Example 11: Moisturizing O / W Cream]

[0244] The powder obtained in the example was used to prepare a moisturizing O / W cream.

[0245]

[0246] (Note 1) KSG-15 manufactured by Shin-Etsu Chemical Co., Ltd.

[0247] (Note 2) KSG-16 manufactured by Shin-Etsu Chemical Co., Ltd.

[0248] (Note 3) KF-6104 manufactured by Shin-Etsu Chemical Co., Ltd.

[0249] (Note 4) KF-6100 manufactured by Shin-Etsu Chemical Co., Ltd.

[0250] (Note 5) SIMULGEL 600 manufactured by SEPPIC

[0251] (Note 6) Aristoflex (registered trademark) AVC manufactured by Clariant Japan KK

[0252] (Manufacturing method)

[0253] A: Mix components 3 to 5 and disperse them uniformly.

[0254] B: Components 1, 2 and A are mixed and uniformly blended using a mixer.

[0255] C: Components 6 to 12 are uniformly mixed using a mixer.

[0256] D: B was slowly added to C under stirring for emulsification to obtain a moisturizing O / W cream.

[0257] The obtained moisturizing O / W cream has light ductility, no stickiness or oiliness, is dry and has no astringency, has a refreshing feeling during use, and has excellent stability.

[0258] [Formulation Example 12: O / W cream]

[0259] The powder obtained in the example was used to prepare an O / W cream.

[0260]

[0261] (Note 1) KSG-15 manufactured by Shin-Etsu Chemical Co., Ltd.

[0262] (Manufacturing method)

[0263] A: Heat and mix components 1 to 8 until they are uniform.

[0264] B: Components 9 to 13 and 15 are mixed and heated.

[0265] C: B is slowly added to A under stirring to emulsify, and after cooling, ingredient 14 is added to obtain an O / W cream.

[0266] The obtained O / W cream has light ductility, no stickiness or oiliness, is dry and has no astringency, has a refreshing feeling during use, and has excellent stability.

[0267] [Formula Example 13: Body Lotion]

[0268] The powder obtained in the example was used to prepare a body lotion.

[0269]

[0270] (Note 1) KF-6100 manufactured by Shin-Etsu Chemical Co., Ltd.

[0271] (Note 2) KSP-100 manufactured by Shin-Etsu Chemical Co., Ltd.

[0272] (Manufacturing method)

[0273] A: Components 1 to 6 are uniformly mixed using a mixer.

[0274] B: Components 7 to 10 are uniformly mixed using a mixer.

[0275] C: Slowly add A to B while stirring and mix to obtain a body lotion.

[0276] The obtained body lotion has light ductility, no stickiness or oiliness, is dry and has no astringency, has a refreshing feeling when used, and has excellent stability.

[0277] [Formula Example 14: Sunscreen]

[0278] The powder obtained in the example was used to prepare a sunscreen.

[0279]

[0280]

[0281] (Note 1) KSG-240 manufactured by Shin-Etsu Chemical Co., Ltd.

[0282] (Note 2) KSG-15 manufactured by Shin-Etsu Chemical Co., Ltd.

[0283] (Note 3) KF-6038 manufactured by Shin-Etsu Chemical Co., Ltd.

[0284] (Note 4) KP-575 manufactured by Shin-Etsu Chemical Co., Ltd.

[0285] (Note 5) The surface was treated with AES-3083 manufactured by Shin-Etsu Chemical Co., Ltd.

[0286] (Manufacturing method)

[0287] A: Component 7 was added to a portion of component 5 to make it uniform, and then components 8 and 9 were added and dispersed using an Easy Nano RMB type bead mill manufactured by AIMEX CO., LTD.

[0288] B: Components 1 to 4, the remainder of component 5, and 6 are uniformly mixed using a mixer.

[0289] C: Components 10 to 12 and component 14 are mixed and made uniform.

[0290] D: C is added to B for emulsification, and A and ingredient 13 are added to obtain a sunscreen.

[0291] The resulting sunscreen has very light spreadability, no stickiness, and excellent adhesion.

[0292] [Formula Example 15: Embossed Blush]

[0293] The powder obtained in the example was used to make relief blush.

[0294]

[0295] (Note 1) The surface was treated with KP-574 manufactured by Shin-Etsu Chemical Co., Ltd.

[0296] (Note 2) The surface was treated with KF-9909 manufactured by Shin-Etsu Chemical Co., Ltd.

[0297] (Note 3) KSP-300 manufactured by Shin-Etsu Chemical Co., Ltd.

[0298] (Manufacturing method)

[0299] A: Components 1 to 8 are uniformly dispersed.

[0300] B: Mix components 9 to 11 by heating.

[0301] C: Add B to A, mix evenly using a mixer, and press into shape in a metal dish to obtain a relief blush.

[0302] The resulting relief blush has light ductility, no oily or powdery feel, excellent adhesion to the skin, and a natural finish.

[0303] [Formula Example 16: Loose Powder]

[0304] The powder obtained in the example was used to prepare loose powder.

[0305]

[0306]

[0307] (Note 1) Matsumoto Microsphere S-100 manufactured by Matsumoto Oil & Fats Co., Ltd.

[0308] (Manufacturing method)

[0309] A: Components 1 to 7 are mixed and ground.

[0310] B: Transfer A to a Henschel mixer, add ingredients 8 to 10, and stir until uniform.

[0311] C: B is crushed with an atomizer and filled to obtain loose powder.

[0312] The obtained loose powder has excellent ductility and excellent transparency even after application, and has a moderate covering power without causing whitening, giving a natural bare skin finish.

[0313] [Formula Example 17: Eyeliner]

[0314] Eyeliner was produced using the powder obtained in Example.

[0315]

[0316]

[0317] (Manufacturing method)

[0318] A: A part of component 5 and component 6 were added to component 7, and components 1 to 3, a part of component 4, and the remainder of component 5 were added thereto, and the mixture was processed using a colloid mill CM-1 manufactured by Mitsui Electric Seiki Co., Ltd.

[0319] B: The remaining portion of component 4, component 8, and component 9 are mixed, and A is added at 70° C. and uniformly dispersed, followed by cooling and filling to obtain an eyeliner.

[0320] The obtained eyeliner has a uniform color tone, excellent spreadability, and excellent adhesion.

[0321] [Example 18: Mascara]

[0322] The powder obtained in the example was used to prepare mascara.

[0323]

[0324]

[0325] (Manufacturing method)

[0326] A: Components 7 to 11 were stirred and mixed using a Henschel mixer.

[0327] B: Add A to components 1 to 6 and disperse evenly using a stirrer.

[0328] C: Heat and dissolve ingredients 12 to 20 in another container.

[0329] D: C was added to B and emulsified, then cooled to 40°C, component 21 was added, and the mixture was cooled to room temperature to obtain a mascara.

[0330] The obtained mascara had a uniform color tone, moderate glossiness, and excellent adhesion to eyebrows.

[0331] [Formula Example 19: Eyeshadow Cream]

[0332] The powder obtained in the example was used to prepare eye shadow cream.

[0333]

[0334]

[0335] (Note 1) KP-545 manufactured by Shin-Etsu Chemical Co., Ltd.

[0336] (Note 2) KP-561P manufactured by Shin-Etsu Chemical Co., Ltd.

[0337] (Note 3) KF-6028P manufactured by Shin-Etsu Chemical Co., Ltd.

[0338] (Note 4) The surface was treated with KP-574 manufactured by Shin-Etsu Chemical Co., Ltd.

[0339] (Manufacturing method)

[0340] A: Components 1 to 6 are mixed, and components 7 to 10 are further added, and the mixture is uniformly mixed and dispersed using a mixer.

[0341] B: Mix components 11 and 12.

[0342] C: Add B to A and emulsify to obtain eye shadow cream.

[0343] The resulting eyeshadow cream has light ductility, no oily or powdery feel, and excellent adhesion to the skin.

[0344] [Formula Example 20: Eye Shadow]

[0345] Eye shadow was prepared using the powder obtained in Example.

[0346]

[0347] (Note 1) The surface was treated with KF-99P manufactured by Shin-Etsu Chemical Co., Ltd.

[0348] (Manufacturing method)

[0349] A: Components 1 to 5 are mixed and ground.

[0350] B: Transfer A to a Henschel mixer, add the additional mixed ingredients 6 to 10, and stir until uniform.

[0351] C: B was crushed with an atomizer and pressed into an aluminum dish to obtain an eye shadow.

[0352] The obtained eye shadow has a uniform color tone, excellent spreadability, and excellent adhesion to the skin.

[0353] [Formula Example 21: Nail Polish]

[0354] The powder obtained in the example was used to prepare nail polish.

[0355]

[0356] (Manufacturing method)

[0357] A: Components 8 and 9 are dissolved in a part of component 2 and component 3, and the mixture is fully kneaded.

[0358] B: Component 2, the remaining portion of component 3, component 1, components 4 to 7, and component 10 are added to and mixed in A, and the mixture is filled in a container to obtain a nail polish.

[0359] The applied color of the obtained nail polish was equivalent to the appearance color, the color tone was uniform, and the ductility was excellent.

[0360] [Formulation Example 22: Solid Oil-in-Polyol Emulsified Blush]

[0361] The powder obtained in the example was used to prepare a solid oil-in-polyol emulsified blush.

[0362]

[0363]

[0364] (Note 1) KSG-710 manufactured by Shin-Etsu Chemical Co., Ltd.

[0365] (Note 2) KSG-15 manufactured by Shin-Etsu Chemical Co., Ltd.

[0366] (Note 3) The surface was treated with KP-562P manufactured by Shin-Etsu Chemical Co., Ltd.

[0367] (Manufacturing method)

[0368] A: Components 1 to 8 were heated to 80° C. and uniformly mixed using a mixer.

[0369] B: Components 9 to 12 are uniformly mixed using a mixer, added to A, and uniformly dispersed.

[0370] C: Mix ingredients 13 and 15 and heat to 80°C.

[0371] D: C was added to B for emulsification, and ingredient 14 was added and poured into a metal dish for cooling to obtain a solid oil-in-polyol emulsified blush.

[0372] The obtained solid polyol-in-oil emulsified blush has light ductility, no stickiness or oiliness, excellent adhesion to the skin, and a natural finish.

[0373] [Formula Example 23: Blush]

[0374] The powder obtained in the example was used to prepare blush.

[0375]

[0376] (Manufacturing method)

[0377] A: Heat and dissolve components 6 to 9.

[0378] B: Components 1 to 5 were mixed using a Henschel mixer, and A was added thereto.

[0379] C: B was crushed with a sprayer and molded in a medium dish to obtain blush.

[0380] The resulting blush has light ductility, no oily or powdery feel, excellent adhesion to the skin, and a natural finish.

[0381] [Formula Example 24: Creamy lipstick]

[0382] The powder obtained in the example was used to prepare a creamy lipstick.

[0383]

[0384]

[0385] (Note 1) Rheopearl (registered trademark) manufactured by Chiba Flour Milling Co., Ltd.

[0386] (Note 2) KSG-43 manufactured by Shin-Etsu Chemical Co., Ltd.

[0387] (Note 3) KF-6105 manufactured by Shin-Etsu Chemical Co., Ltd.

[0388] (Manufacturing method)

[0389] A: Components 9 to 12 were mixed with a portion of component 2, and the mixture was dispersed using a three-roll mill BR-100VIII manufactured by AIMEX CO., LTD.

[0390] B: Component 1, the remaining portion of component 2, and components 3 to 6 are heated and uniformly mixed using a mixer.

[0391] C: Add A to B and mix evenly using a mixer.

[0392] D: Mix ingredients 7 and 8, heat, and add to C to emulsify.

[0393] E: Add ingredients 13 and 14 to D to obtain a creamy lipstick.

[0394] The resulting creamy lipstick is light on spread, has no stickiness or oiliness, and is moist without feeling dry.

[0395] [Formula Example 25: Facial Cleansing Foam]

[0396] The powder obtained in the example was used to prepare a facial cleanser foam.

[0397]

[0398]

[0399] (Manufacturing method)

[0400] A: Mix ingredients 1 to 9 and heat to dissolve.

[0401] B: Weigh ingredients 10 and 11 in another container, add them to A, and saponify.

[0402] C: Components 12 to 15 were added to B, stirred and mixed uniformly, and then cooled to room temperature. Then, the mixture was filled into a suitable container to obtain a facial cleanser foam.

[0403] The obtained facial cleansing foam has a beautiful white appearance, has excellent foaming properties and foam retention without impairing the cleansing properties.

[0404] [Formula Example 26: Lipstick]

[0405] The powder obtained in the example was used to make lipstick.

[0406]

[0407]

[0408] (Manufacturing method)

[0409] A: Heat and mix ingredients 1 to 12, and stir evenly.

[0410] B: After degassing, A is poured into a mold and rapidly cooled to obtain a lipstick.

[0411] The obtained lipstick had the same coating color and appearance color and was also excellent in spreadability.

[0412] [Formula Example 27: Lip Gloss]

[0413] The powder obtained in the example was used to prepare lip gloss.

[0414]

[0415] (Manufacturing method)

[0416] A: Components 1 to 5 are heated to 85°C and uniformly dissolved.

[0417] B: Add components 6 to 8 to A and disperse evenly.

[0418] C: Fill B into a container at high temperature and cool it to room temperature to obtain lip gloss.

[0419] The obtained lip gloss had an applied color that was equivalent to an external color, was excellent in spreadability, and also had excellent adhesion.

Claims

1. A titanium (IV) oxide powder, comprising particles having a peanut-shaped twin shape, wherein the diameter of the longest part of one of the particles of the peanut-shaped twin shape is 300 nm to 700 nm, the diameter of the short axis of the largest part in a direction perpendicular to the long axis is 100 nm to 400 nm, the diameter of a narrowed portion in a direction perpendicular to the long axis at the center of the long axis is 80 nm to 200 nm, and the ratio of the narrowed portion diameter to the short axis diameter is 0.9 or less.

2. The titanium (IV) oxide powder according to claim 1, wherein The titanium (IV) oxide is rutile titanium oxide.

3. The titanium (IV) oxide powder according to claim 1 or 2, wherein The single particle is formed by fine rod-shaped particles aggregated in a peanut-shaped twin shape, wherein the fine rod-shaped particles have a major axis diameter of 30 nm to 350 nm and a minor axis diameter of 3 nm to 12 nm.

4. The titanium (IV) oxide powder according to claim 1 or 2, wherein A mixed liquid of trimethylsiloxysilicate and cyclopentasiloxane in a mass ratio of 1:1 was used as a medium and stirred at 2000 rpm to prepare a coating with a powder concentration of 100 g / kg. The coating was formed into a coating film using a rod coater with a film thickness of 18.4 μm. When the coating film was irradiated with light having a color temperature of 6774 K, i.e., C light, in a double-beam manner and measured, the total light transmittance of the coating film was 45.0% or more and 60.0% or less, and the haze value was 90.0% or more.

5. The titanium (IV) oxide powder according to claim 1 or 2, wherein At least a part of the surface of particles constituting the powder is covered with a layer of an inorganic substance and / or an organic substance.

6. The titanium (IV) oxide powder according to claim 5, wherein At least a part of the surface of the particles constituting the powder is covered with an inorganic layer, and the inorganic layer contains one or two or more of aluminum, silicon, zinc, titanium, zirconium, iron, cerium and tin.

7. The titanium (IV) oxide powder according to claim 5, wherein At least a part of the surface of particles constituting the powder is covered with an organic layer, and the organic layer contains one or more of an organic silicon compound, a coupling agent, a fluorine compound, and a fatty acid.

8. A cosmetic comprising the titanium (IV) oxide powder according to claim 1 or 2.

9. A method for producing a titanium (IV) oxide powder as described in claim 1, comprising step 1: adding hydrochloric acid to a slurry containing an acid-soluble titanium compound, adjusting the hydrochloric acid concentration to be greater than 60 g / L and less than 130 g / L, and adjusting the temperature to be greater than 25°C and less than 60°C and maintaining the temperature for more than 1 hour.

10. The manufacturing method according to claim 9, wherein: The step 1 includes adjusting the concentration of the hydrochloric acid to 80 g / L or more and 130 g / L or less, and adjusting the temperature to 35° C. or more and 45° C. or less.

11. The manufacturing method according to claim 9 or 10, wherein: After the step 1, the method further includes a step 2 of adjusting the hydrochloric acid concentration and / or the temperature to a value higher than that in the step 1 within the range of a hydrochloric acid concentration of 180 g / L or less and a temperature of 100° C. or less and maintaining the concentration for 1 hour or more.

12. The manufacturing method according to claim 11, wherein: After step 2, step 3 is further included: calcination.

Citation Information

Patent Citations

  • Titanium dioxide and composition containing the same

    JP1997221411A

  • Cosmetic

    JP1999158035A

  • Spherical titanium dioxide aggregate formed from fine spherical particles of titanium dioxide and its production

    JP2000191325A

  • Rutile type titanium oxide particle aggregate and cosmetic material containing the same

    JP2008056535A