Battery positive electrode material, processing method thereof and battery
Patent Information
- Application Number
- CN202380008984.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-11-15
AI Technical Summary
The slow lithium/sodium ion diffusion rate of existing lithium-ion or sodium-ion battery cathode materials results in low energy and power density, limiting battery performance and cycle life.
By subjecting the surface of the battery cathode material to cold plasma treatment, active particles are doped to increase its surface energy and interface affinity with the electrolyte, forming a rod-like morphology and a NaF layer to enhance the sodium ion transport rate and electronic conductivity.
The energy density, cycle life and rate capability of lithium-ion or sodium-ion batteries are improved, and the occurrence of side reactions is reduced. The processing process is simple, the energy consumption is low, and it is suitable for large-scale production.
Smart Images

Figure CN118974974A_ABST
Abstract
Description
Battery positive electrode material, processing method thereof, and battery Technical Field
[0001] The present invention relates to the field of battery materials, and more particularly to a battery positive electrode material, a processing method thereof, and a battery. Background Art
[0002] In recent years, industries such as mobile consumer electronics and electric vehicles have developed rapidly, and there is an urgent need to develop new energy batteries with high energy density, high safety and stability to improve the long-term endurance and long-term stable operation of these devices. Therefore, lithium-ion or sodium-ion batteries are generally considered to be one of the most promising candidate batteries for large-scale energy storage applications. However, since the currently known positive electrode materials all have the bottleneck of slow lithium / sodium ion diffusion rate, the energy and power density of lithium-ion or sodium-ion batteries are low. High-performance positive electrode materials can improve the energy density, cycle life and rate capability of lithium-ion or sodium-ion batteries. Therefore, the development of high-performance positive electrode materials is particularly important.
[0003] Summary of the Invention
[0004] In response to the shortcomings of the prior art, one of the objectives of the present invention is to address one or more of the problems existing in the prior art. For example, one of the objectives of the present invention is to provide a treatment method that can enhance the surface energy of battery positive electrode particles and improve their interfacial affinity with the electrolyte.
[0005] In order to achieve the above-mentioned purpose, one aspect of the present invention provides a method for processing battery positive electrode materials, which may include the following steps: subjecting a battery positive electrode material having a carbon layer on at least a portion of its surface to be treated to cold plasma treatment to dope the carbon layer with active particles, wherein the active particle doping amount is not less than 50 ppm (molar fraction or volume fraction, parts per billion, ppm).
[0006] In an exemplary embodiment of the method for treating a battery cathode material according to the present invention, the power of the cold plasma treatment may be 100W to 500W.
[0007] In an exemplary embodiment of the method for treating a battery positive electrode material according to the present invention, the voltage of the cold plasma treatment may be 50V to 150V, and the treatment current may be 0.4A to 2A.
[0008] In an exemplary embodiment of the method for treating a battery positive electrode material according to the present invention, the cold plasma treatment time may be 1 min to 60 min.
[0009] In an exemplary embodiment of the method for processing a battery cathode material of the present invention, the discharge for generating cold plasma may be selected from one or a combination of radio frequency plasma discharge, corona discharge, dielectric barrier discharge, and sliding arc discharge.
[0010] In an exemplary embodiment of the method for processing a positive electrode material of a battery according to the present invention, the doping may be oxygen doping, nitrogen doping, or a combination thereof.
[0011] In an exemplary embodiment of the method for processing battery positive electrode materials of the present invention, cold plasma treatment may include inputting one or a combination of precursor gases of oxygen, nitrogen into a cold plasma generator to generate active particles to dope the carbon layer, wherein the precursor gas flow rate may be 1 ml / s to 15 ml / s.
[0012] In an exemplary embodiment of the method for processing a battery cathode material according to the present invention, the battery cathode material may be a polyanionic compound, a layered oxide, a spinel compound, Prussian blue, or a ternary lithium battery cathode material. For example, the battery cathode material may be sodium vanadium phosphate, lithium iron phosphate, sodium titanium phosphate, sodium fluoride phosphate, LiMO2, NaMO2, LiN2O4, lithium nickel cobalt manganese oxide, or lithium nickel cobalt aluminum oxide, wherein M may be Co, Ni, Mn, V, or Fe, and N may be Co, Nix, Mn, or V.
[0013] In an exemplary embodiment of the method for processing a battery cathode material of the present invention, at least a portion of the surface of the doped battery cathode material has a rod-like morphology.
[0014] In an exemplary embodiment of the method for processing a positive electrode material for a battery according to the present invention, the average length of the rod-shaped morphology may be 1.5 μm to 3 μm.
[0015] In an exemplary embodiment of the method for processing a battery positive electrode material of the present invention, a NaF layer is formed on at least a portion of the surface of the doped battery positive electrode material, and the average thickness of the NaF layer may be 6 nm to 10 nm.
[0016] In an exemplary embodiment of the method for treating a positive electrode material for a battery according to the present invention, the content of the NaF layer is not less than 500 ppm.
[0017] Another aspect of the present invention provides a battery positive electrode material, at least a portion of its surface contains a carbon layer and at least a portion of the surface has a rod-like morphology, wherein the carbon layer is a carbon layer doped with active particles after cold plasma treatment; the doping amount is not less than 50 ppm.
[0018] In an exemplary embodiment of a battery positive electrode material of the present invention, the active particles may be oxygen, nitrogen, or a combination thereof.
[0019] In an exemplary embodiment of a battery positive electrode material of the present invention, the average length of the rod-shaped morphology is 1.5 μm to 3 μm.
[0020] Another aspect of the present invention provides a positive electrode sheet, which may include the positive electrode material processed by the above-mentioned method for processing the battery positive electrode material or the above-mentioned battery positive electrode material.
[0021] Another aspect of the present invention provides a battery, which may include the positive electrode sheet described above.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] (1) The treatment method of the present invention can enhance the surface energy of the battery positive electrode material particles, improve their interfacial affinity with the electrolyte, and obtain a positive electrode material with uniform texture, low porosity, high ionic conductivity and electronic conductivity.
[0024] (2) The positive electrode material of the present invention has high electronic conductivity, good interfacial compatibility with the electrolyte, and a "rod-like" surface morphology, which makes the interface contact between the battery positive electrode material and the current collector stable and can improve the rate of sodium ion transmission and electronic conductivity.
[0025] (3) The treatment method of the present invention can produce a NaF layer on the surface of the battery positive electrode material. This layer has ultra-high sodium ion conductivity, limits the occurrence of side reactions between the positive electrode material and the electrolyte, and increases the transmission rate of sodium ions at the solid-liquid interface.
[0026] (4) The lithium-ion batteries and sodium-ion batteries prepared using the battery positive electrode materials treated by the present invention have high energy density, cycle life and rate capability.
[0027] (5) The treatment method of the present invention has a simple process flow, low energy consumption, small equipment investment, no generation of "three wastes", is environmentally friendly, and is suitable for large-scale production applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The above and other objects and features of the present invention will become more apparent from the following description in conjunction with the accompanying drawings, in which:
[0029] FIG. 1 shows a comparison diagram of XRD (X-ray diffraction, XRD) of the sodium vanadium phosphate positive electrode material before and after treatment in Example 1. FIG.
[0030] FIG2 shows a comparison of the XPS (X-ray photoelectron spectroscopy, XPS) of the sodium vanadium phosphate cathode material before and after treatment in Example 1. FIG.
[0031] FIG3 shows a SEM (scanning electron microscope, SEM) image of the untreated sodium vanadium phosphate positive electrode material in Example 2.
[0032] FIG4 shows an SEM image of the sodium vanadium phosphate positive electrode material after treatment in Example 2.
[0033] FIG5 shows a voltage-capacity graph of the battery in Example 2.
[0034] FIG6 shows the contact angle of the untreated sodium vanadium phosphate positive electrode material to the electrolyte in Example 3.
[0035] FIG7 shows the contact angle of the sodium vanadium phosphate positive electrode material after treatment in Example 3 to the electrolyte.
[0036] FIG8 shows an EIS (Electrochemical Impedance Spectroscopy, EIS) graph of the sodium vanadium phosphate positive electrode material after treatment in Example 3.
[0037] FIG9 shows the XPS of the untreated sodium vanadium phosphate cathode material in Example 4.
[0038] FIG10 shows the XPS of the sodium vanadium phosphate cathode material after treatment in Example 4.
[0039] FIG. 11 shows a voltage-capacity graph of the battery in Example 6. FIG.
[0040] FIG. 12 shows a long cycle diagram of sodium vanadium phosphate after treatment in Example 6.
[0041] FIG13 shows a voltage-capacity graph of the battery in Example 8.
[0042] FIG14 shows a long cycle diagram of lithium iron phosphate after treatment in Example 8.
[0043] FIG. 15 shows EIS graphs of lithium iron phosphate before and after treatment in Example 9. FIG. DETAILED DESCRIPTION
[0044] Hereinafter, a battery positive electrode material, a processing method thereof, and a battery according to the present invention will be described in detail with reference to the accompanying drawings and exemplary embodiments.
[0045] One aspect of the present invention provides a method for processing battery positive electrode materials, which may include the following steps: subjecting the battery positive electrode material having a carbon layer on at least a portion of its surface to be processed to cold plasma treatment to dope the carbon layer, wherein the doping amount is not less than 50 ppm.
[0046] The battery positive electrode material is doped with highly active particles generated by cold plasma on the carbon layer attached to or coated on the surface of the positive electrode material, which can form more defects on the surface of the carbon layer, improve the stability of the interface contact between the positive electrode material and the current collector, and thus increase the rate of sodium ion or lithium ion transmission and electronic conductivity. It also improves the affinity between the positive electrode material and the electrolyte, alleviates the serious volume effect caused by the large radius of sodium ions or lithium ions, and makes the active material have good structural stability during long cycles. Compared with untreated positive electrode materials, batteries using treated positive electrode materials have lower polarization voltage, lower interfacial impedance, more stable charge and discharge platform and higher specific capacity.
[0047] In some embodiments, at least a portion of the battery positive electrode material to be processed has a carbon layer to achieve doping of the carbon layer. The carbon layer can be fully or partially coated on the surface of the positive electrode material to be processed. That is, the carbon layer described herein can form all or only a portion of the surface of the positive electrode material, and in some embodiments, the carbon layer can be one or more layers, for example, the carbon layer can be 2 layers, or 3 layers, or 4 layers, or more than 5 layers, or more than 6 layers. It should be understood that the surface of the positive electrode material may not only include a carbon layer, but may also contain other coating layers or adhesion layers on the surface of the positive electrode material that can improve the performance of the positive electrode material.
[0048] In some embodiments, the doping amount affects the electronic conductivity of the carbon layer on the surface of the positive electrode material. If the doping amount is less than 50ppm, the electronic conductivity of the carbon layer on the surface of the positive electrode material is not significantly improved. Therefore, the doping amount may be not less than 50ppm, not less than 70ppm, not less than 85ppm, not less than 105ppm, not less than 123ppm, not less than 152ppm, or 160ppm to 246ppmm, or 214ppm to 318ppmm, or 259ppm to 413ppmm, or 586ppm to 793ppmm, or 803ppm to 1050ppm. In addition, a doping amount greater than 600ppm may cause damage to the surface carbon layer and reduce the cycle stability of the active particles. Therefore, preferably, the doping amount is between 50ppm and 600ppm.
[0049] In some embodiments, the thickness of the cathode material to be treated can be adjusted. As described herein, cathode materials of any thickness can be treated using the treatment methods herein. In certain embodiments, the thickness of the cathode material to be treated can be 30 μm to 100 μm, for example, the thickness can be less than 28 μm or greater than 110 μm, or 15 μm, or 45 μm, or 84 μm, or 141 μm.
[0050] In some embodiments, the power of the cold plasma treatment can be between 100W and 500W. Within this range, doping can be achieved while ensuring the stability of the carbon layer on the surface of the cathode material. If the power is lower than 100W, the energy required to break carbon-carbon bonds will not be reached, preventing the active particles from being doped. If the power is higher than 500W, the carbon layer structure on the surface of the cathode material will be destroyed, resulting in a decrease in electrochemical performance. Furthermore, within this power range, the cathode material can achieve a high surface energy and improve its affinity with the electrolyte interface. For example, cold plasma can be generated by delivering a source gas such as oxygen, nitrogen, or a mixed gas into a cold plasma generator to generate active particles. Regarding the applied power mentioned above, it should be noted that this power refers to the power directly acting on the precursor gas, that is, the power directly received by the source gas. In certain embodiments, the power of the cold plasma treatment can be no less than 150W, or no less than 245W, or no less than 289W, or no less than 423W.
[0051] In some embodiments, the voltage of the cold plasma treatment can be 50V to 150V, and the treatment current can be 0.4A to 2A. Applying the voltage and current within the above range can make the power of the cold plasma treatment reach 100W to 500W, which can break the carbon-carbon bonds while ensuring the stability of the carbon layer on the surface of the positive electrode material. It should be understood in the art that the voltage and current here are the voltage and current applied to the cold plasma generator. In certain embodiments, the voltage of the cold plasma treatment can be not less than 60V, or not less than 72V, or not less than 83V, or not less than 114V, or not less than 127V, or not less than 142V or a combination of the above ranges. The current of the cold plasma treatment can be 0.5A to 1.8A, 0.7A to 1.6A, 0.9A to 1.4A, 1.1A to 1.3A or a combination of the above ranges. Under the above-mentioned applied voltage, current and power, the surface of the positive electrode material can have a rod-like morphology (rod-like structure), so that the positive electrode material has the properties described herein.
[0052] In some embodiments, the cold plasma treatment time can be 1 min to 60 min. During the above-mentioned cold plasma treatment time, the treatment voltage and treatment current applied in coordination can ensure that the carbon layer on the surface of the positive electrode material is doped so that its doping amount reaches 50 ppm or more. For example, the treatment time can be not less than 2 min, not less than 15 min, not less than 23 min, not less than 38 min, not less than 47 min, not less than 52 min. In some cases, the cold plasma treatment time can be greater than about 30 s, or greater than about 45 s. However, it should be understood that the treatment time can be adjusted arbitrarily as long as the doping amount described herein can be achieved.
[0053] In some embodiments, the content of NaF will affect the electrochemical properties of the electrode surface. If the content of NaF is less than 50ppm, the ionic conductivity of the positive electrode material surface is not significantly improved. Therefore, the content of NaF is not less than 50ppm, not less than 70ppm, not less than 85ppm, not less than 105ppm, not less than 123ppm, not less than 152ppm, or 160ppm to 246ppmm, or 214ppm to 318ppmm, or 259ppm to 413ppmm, or 586ppm to 793ppmm, or 803ppm to 1050ppm. In addition, a doping amount greater than 50ppm may cause damage to the electrode surface binder and reduce the bonding force between the active materials. Therefore, preferably, the doping amount is between 50ppm and 500ppm.
[0054] In some embodiments, the discharge for generating the cold plasma is selected from one or a combination of radio frequency plasma discharge (RF), corona discharge (CD), dielectric barrier discharge (DBD), and glide arc discharge (GAD). The above-mentioned cold plasma equipment can stably discharge at high pressure, is simple to operate, and can form a large area of plasma discharge area, so that the active particles in the discharge area have a larger range of action, providing a basis for efficient doping treatment. Of course, it should be understood that any other discharge suitable for generating cold plasma is also applicable to the treatment method described herein.
[0055] In some embodiments, the doped active particles or doped active materials may be one or a combination of oxygen doping and nitrogen doping. For example, in certain embodiments, oxygen doping, nitrogen doping, or oxygen-nitrogen doping may be independent. Doping the carbon layer with highly active particles generated by cold plasma can enable the positive electrode material to obtain better electrochemical properties. Of course, it should be understood in the art that the doping of the above-mentioned active particles may include inputting one or a combination of precursor gases, such as oxygen and nitrogen, into a cold plasma generator to generate active particles and then doping the carbon layer on the surface of the positive electrode material. However, in certain embodiments, the doping of the active particles may also be achieved by other forms of cold plasma generators.
[0056] In some embodiments, the flow rate of the precursor gas introduced into the cold plasma generator can be 1 ml / s to 15 ml / s. At the above-mentioned precursor gas flow rate, the voltage and current applied in coordination can ensure the realization of carbon layer doping. In one group of embodiments, the positive electrode material to be treated can be placed in a cold plasma generator, and the precursor gas can be introduced at the rate described in this article, and the cold plasma generator can be adjusted to the voltage and current described in this article to treat the positive electrode material to be treated. Of course, it should be understood that when oxygen doping is achieved, oxygen doping needs to be completed in a short time under an oxygen atmosphere to ensure that oxygen-containing functional groups are introduced while very little oxidation occurs, and to avoid oxidation caused by too long a time or too high a power. For oxygen-containing mixed gases, since the oxygen content is low, the oxidation effect can be ignored.
[0057] In some embodiments, the treated cathode materials described herein exhibit distinct morphological characteristics compared to existing cathode materials. The treatment of the cathode material can result in at least a portion of the cathode material's surface exhibiting a rod-like morphology. For example, a sodium vanadium phosphate cathode material can exhibit numerous rod-like, rod-like, or flaky structures on its surface after treatment using the methods described herein. In certain embodiments, the entire surface of the positive electrode material has a rod-like morphology, or at least 0.01% of the surface area coverage has a rod-like morphology, or at least 0.1% of the surface area has a rod-like morphology, or at least 5% of the surface area has a rod-like morphology, or at least 9.8% of the surface area has a rod-like morphology, or at least 15.3% of the surface area has a rod-like morphology, or at least 21.5% of the surface area has a rod-like morphology, or at least 35.4% of the surface area has a rod-like morphology, or at least 41.2% of the surface area has a rod-like morphology, or at least 49.8% of the surface area has a rod-like morphology, or at least 55.1% of the surface area has a rod-like morphology, or at least 61.5% of the surface area has a rod-like morphology, or at least 73.5% of the surface area has a rod-like morphology, or at least 84.5% of the surface area has a rod-like morphology. By having a rod-like morphology on the surface of the positive electrode material, the stability of the interface contact between the positive electrode material and the current collector can be improved, thereby increasing the rate of sodium ion transmission and electronic conductivity. However, it should be understood that the rod-shaped described herein refers to a slender form or a slender structure, and can also be described as a columnar shape, etc.
[0058] In some embodiments, the rod-like morphology may have a specific length, i.e., the average length of the rod-like morphology may be no less than 1.6 μm, no less than 2.1 μm, no less than 2.4 μm, no less than 2.6 μm, no less than 2.8 μm, or no less than 2.9 μm. In certain embodiments, the rod-like morphology may have a specific diameter (i.e., the radial diameter of the rod), i.e., the average diameter of the rod-like morphology may be no less than 154 nm, no less than 167 nm, no less than 179 nm, no less than 189 nm, no less than 208 nm, no less than 238 nm, no less than 268 nm, no less than 294 nm, or no less than 283 nm.
[0059] In some embodiments, the mass ratio of the rod-shaped material to the mass ratio of the positive electrode material can be specific. For example, the mass ratio of the rod-shaped material to the mass ratio of the positive electrode material can be 2% to 10%. In some embodiments, the mass ratio of the rod-shaped material to the mass ratio of the positive electrode material can be no less than 0.5%, or no less than 0.8%, or no less than 1.5%, or no less than 2.7%, or no less than 3.4%, or no less than 4.7%, or no less than 5.9%, or no less than 6.7%, or no less than 9.4%. In some specific embodiments, the mass ratio is no less than 15.8%, or no less than 20.1%, or no less than 30.5%, or no less than 36.8%.
[0060] In some embodiments, the positive electrode material of the battery can be a polyanionic compound, a layered oxide, a spinel compound, Prussian blue or a ternary lithium battery positive electrode material. The polyanionic compound can include sodium vanadium phosphate, lithium iron phosphate, sodium titanium phosphate and sodium fluoride phosphate. The layered oxide can include LiMO2 and NaMO2, wherein M can be Co, Ni, Mn, V or Fe. The spinel compound can include LiN2O4, wherein N can be Co, Nix, Mn or V. The positive electrode material of the ternary lithium battery can be lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide. It should be understood that the treatment method described herein can also treat some other positive electrode materials.
[0061] In some embodiments, it should be understood that other substances that can enhance the electrochemical performance of the cathode materials described herein may also be introduced.
[0062] Another aspect of the present invention provides a positive electrode material. In an exemplary embodiment of the positive electrode material of the present invention, the positive electrode material can be obtained by treating the method for treating a battery positive electrode material described herein. In some embodiments, at least a portion of the surface of the positive electrode material comprises a carbon layer, and at least a portion of the surface has a rod-like morphology, wherein the carbon layer is a carbon layer doped with active particles after cold plasma treatment.
[0063] In some embodiments, as described herein, the doping amount may be no less than 50 ppm.
[0064] In some embodiments, as described herein, the active species is one of oxygen, nitrogen, or a combination thereof.
[0065] In some embodiments, as described herein, the rod-like morphology may have an average length of 1.5 μm to 3 μm and an average diameter of 150 nm to 300 nm.
[0066] In some embodiments, as described herein, the mass ratio of the rod-shaped material can be specific. For example, the mass ratio of the rod-shaped material to the positive electrode material can be 2% to 10%.
[0067] Another aspect of the present invention provides a positive electrode sheet comprising a current collector and a positive electrode material layer disposed on the current collector, wherein the positive electrode material comprises a positive electrode material treated by the method for treating a battery positive electrode material as described above, or comprises the positive electrode material as described above. In addition to the positive electrode material described above, the positive electrode material layer may further comprise a conductive agent and a binder. The positive electrode material layer may be incorporated into the positive electrode sheet using methods known in the art.
[0068] Another aspect of the present invention provides a battery, in particular a sodium ion battery, comprising the positive electrode sheet as described above. It should be understood that the battery also comprises other essential components that constitute the battery, and the assembly method of the battery is known in the art.
[0069] In some embodiments, the battery can be a button cell. Assembly of a button cell can be known in the art. For example, the positive electrode sheet can be placed in a glove box to assemble the button cell.
[0070] In order to better understand the above exemplary embodiments of the present invention, they are further described below with reference to specific examples.
[0071] Example 1
[0072] A method for processing a positive electrode material of a battery comprises the following steps:
[0073] Step 1, preparation of sodium vanadium phosphate positive electrode material: using a conventional coating process, aluminum foil is used to coat the cut piece to obtain a sodium vanadium phosphate positive electrode material with a thickness of 80 μm.
[0074] Step 2, nitrogen DBD cold plasma activation treatment: first, the sodium vanadium phosphate positive electrode material in step (1) is coated with the active material on one side, and nitrogen DBD cold plasma activation treatment is performed for 1 minute under nitrogen DBD cold plasma with a gas flow rate of 10 ml / s, an operating current of 1 A, and a voltage of 150 V. The activated sodium vanadium phosphate positive electrode material is obtained after cooling to room temperature.
[0075] Step 3, assembly of button cells: Place the sodium vanadium phosphate positive electrode material after activation treatment in step (2) into the glove box, assemble the button cells, and perform battery testing after standing for 12 hours.
[0076] The sodium vanadium phosphate cathode material obtained after nitrogen DBD cold plasma activation treatment was physically characterized. It can be seen from the XRD pattern of the sodium vanadium phosphate cathode material in Figure 1 that the physical properties of the sodium vanadium phosphate cathode material after nitrogen DBD cold plasma activation treatment (DBD-1min in the figure) are not changed compared with those without treatment (DBD-0min in the figure), indicating that nitrogen DBD cold plasma treatment will not destroy the crystal structure of sodium vanadium phosphate. It can be seen from the XPS pattern of the sodium vanadium phosphate cathode material in Figure 2 that, compared with the electrode sheet that has not undergone nitrogen DBD-0min, a NaF layer is produced after nitrogen DBD-1min treatment.
[0077] Example 2
[0078] A method for processing a positive electrode material of a battery comprises the following steps:
[0079] Step 1, preparation of sodium vanadium phosphate positive electrode material: using a conventional coating process, aluminum foil is used to coat the cut piece to obtain a sodium vanadium phosphate positive electrode material with a thickness of 80 μm.
[0080] Step 2, nitrogen DBD cold plasma activation treatment: first, the sodium vanadium phosphate positive electrode material in step (1) is coated with the active material on one side, and nitrogen DBD cold plasma activation treatment is performed for 2 minutes at a gas flow rate of 10 ml / s, an operating current of 1 A, and a voltage of 150 V under nitrogen DBD cold plasma, and then cooled to room temperature to obtain the activated sodium vanadium phosphate positive electrode material.
[0081] Step 3, assembly of button cells: Place the sodium vanadium phosphate positive electrode material after the activation treatment described in step (2) into a glove box, assemble the button cells, and perform battery testing after standing for 12 hours.
[0082] The morphological characterization and physical and electrochemical tests of the sodium vanadium phosphate cathode material obtained by nitrogen DBD cold plasma activation treatment were carried out. The nitrogen doping content in the carbon layer was 159ppm. The SEM images in Figures 3 and 4 show that compared with the sodium vanadium phosphate cathode material that has not been treated with nitrogen DBD cold plasma (as shown in Figure 2), the surface of the treated sodium vanadium phosphate cathode material (as shown in Figure 3) produces a rod-like morphology (rod-like structure, slender structure), which can improve the interfacial contact between the sodium vanadium phosphate cathode material and the electrolyte. As shown in the voltage-capacity diagram in Figure 5, the polarization of the battery dropped from 0.04V to within 0.03V, and the charge and discharge platform was more stable and had a higher specific capacity.
[0083] Example 3
[0084] A method for processing a positive electrode material of a battery comprises the following steps:
[0085] Step 1, preparation of sodium vanadium phosphate positive electrode material: using a conventional coating process, aluminum foil is used to coat the cut piece to obtain a sodium vanadium phosphate positive electrode material with a thickness of 80 μm.
[0086] Step 2, nitrogen DBD cold plasma activation treatment: first, the sodium vanadium phosphate positive electrode material in step (1) is coated with the active material on one side, and nitrogen DBD cold plasma activation treatment is performed for 4 minutes at a gas flow rate of 10 ml / s, an operating current of 1 A, and a voltage of 150 V under nitrogen DBD cold plasma, and then cooled to room temperature to obtain the activated sodium vanadium phosphate positive electrode material.
[0087] Step 3, assembly of button cells: placing the activated sodium vanadium phosphate cathode material into a glove box, assembling button cells, and performing battery testing after standing for 12 hours.
[0088] Physical and electrochemical tests were conducted on the sodium vanadium phosphate cathode material obtained after nitrogen DBD cold plasma activation treatment. The nitrogen doping content in the carbon layer was 87ppm. The contact angle of the untreated sodium vanadium phosphate cathode material to the electrolyte is shown in Figure 6. The contact angle of the treated sodium vanadium phosphate cathode material to the electrolyte is shown in Figure 7. Its contact angle to the electrolyte decreased from 14.15° to 12.4°, proving that the sodium vanadium phosphate cathode material has improved wettability to the electrolyte after treatment. At the same time, as shown in the EIS (electrochemical impedance spectroscopy) in Figure 8, the interfacial impedance is reduced from 3200Ω to 2500Ω compared to the untreated material.
[0089] Example 4
[0090] A method for processing a positive electrode material of a battery comprises the following steps:
[0091] Step 1, preparation of sodium vanadium phosphate positive electrode material: using a conventional coating process, aluminum foil is used to coat the cut piece to obtain a sodium vanadium phosphate positive electrode material with a thickness of 80 μm.
[0092] Step 2, nitrogen DBD cold plasma activation treatment: first, the sodium vanadium phosphate positive electrode material in step (1) is coated with the active material on one side, and nitrogen DBD cold plasma activation treatment is performed for 6 minutes at a gas flow rate of 10 ml / s, an operating current of 1 A, and a voltage of 150 V under nitrogen DBD cold plasma, and then cooled to room temperature to obtain the activated sodium vanadium phosphate positive electrode material.
[0093] Step 3, assembly of button cells: Place the sodium vanadium phosphate positive electrode material after the activation treatment described in step (2) into a glove box, assemble the button cells, and perform battery testing after standing for 12 hours.
[0094] Physical and electrochemical tests were performed on the sodium vanadium phosphate cathode material obtained by nitrogen DBD cold plasma activation treatment. The content of nitrogen doping in the carbon layer was 308 ppm. The XPS of the untreated sodium vanadium phosphate cathode material is shown in Figure 9, and the XPS of the treated sodium vanadium phosphate cathode material is shown in Figure 10. The contents of pyridinic nitrogen, pyrrolic nitrogen, and graphitized nitrogen are increased (pyridinic nitrogen, pyrrolic nitrogen, and graphitized nitrogen are three different forms of nitrogen particles doped into the carbon layer), thereby increasing the defects of the carbon layer, which helps to improve the electronic conductivity and ionic conductivity of sodium vanadium phosphate.
[0095] Example 5
[0096] A method for processing a positive electrode material of a battery comprises the following steps:
[0097] Step 1, preparation of sodium vanadium phosphate positive electrode material: using a conventional coating process, aluminum foil is used to coat the cut piece to obtain a sodium vanadium phosphate positive electrode material with a thickness of 80 μm.
[0098] Step 2, oxygen RF cold plasma activation treatment: first, the sodium vanadium phosphate positive electrode material in step (1) is coated with the active material on one side, and oxygen RF cold plasma activation treatment is performed for 6 minutes at a gas flow rate of 10 ml / s, an operating current of 1 A, and a voltage of 100 V under oxygen RF cold plasma, and then cooled to room temperature to obtain the activated sodium vanadium phosphate positive electrode material.
[0099] Step 3, assembly of button cells: Place the activated sodium vanadium phosphate positive electrode material described in step (2) into a glove box, assemble button cells, and perform battery testing after standing for 12 hours.
[0100] Physical and electrochemical testing of the sodium vanadium phosphate cathode material, obtained by oxygen RF cold plasma activation, revealed an argon-doped carbon layer at 287 ppm. Compared to untreated cathodes, the material exhibited lower polarization and impedance, with polarization reduced by 43% and impedance by 18%.
[0101] Example 6
[0102] A method for processing a positive electrode material of a battery comprises the following steps:
[0103] Step 1, preparation of sodium vanadium phosphate positive electrode material: using a conventional coating process, aluminum foil is used to coat the cut piece to obtain a sodium vanadium phosphate positive electrode material with a thickness of 80 μm.
[0104] Step 2, nitrogen-oxygen mixture CD cold plasma activation treatment: first, the sodium vanadium phosphate positive electrode material in step (1) is coated with the active material on one side, and nitrogen-oxygen mixture CD cold plasma activation treatment is performed for 4 minutes at a gas flow rate of 10 ml / s, a working current of 2 A, and a voltage of 100 V under nitrogen-oxygen mixture CD cold plasma, and then cooled to room temperature to obtain an activated sodium vanadium phosphate positive electrode material.
[0105] Step 3, assembly of button cells: Place the activated sodium vanadium phosphate cathode material described in step (2) into a glove box and assemble button cells. All batteries must be left to stand for 12 hours before testing.
[0106] Physical and electrochemical testing of the sodium vanadium phosphate cathode material, obtained by cold plasma activation with a nitrogen-oxygen mixture (CD) plasma, revealed a nitrogen-oxygen doping concentration of 378 ppm in the carbon layer, resulting in lower polarization and impedance compared to untreated electrodes. The voltage-capacity of the sodium vanadium phosphate at 5C is shown in Figure 11. The treated battery increased its capacity by 13.6% and reduced its polarization by approximately 45%. The long-term cycling profile of the sodium vanadium phosphate at 5C is shown in Figure 12. The treated battery's capacity retention improved by 14%.
[0107] Example 7
[0108] A method for processing a positive electrode material of a battery comprises the following steps:
[0109] Step 1, preparation of sodium vanadium phosphate positive electrode material: using a conventional coating process, aluminum foil is used to coat the cut piece to obtain a sodium vanadium phosphate positive electrode material with a thickness of 80 μm.
[0110] Step 2, oxygen CD cold plasma activation treatment: first, the sodium vanadium phosphate positive electrode material in step (1) is coated with the active material on one side, and oxygen CD cold plasma activation treatment is performed for 4 minutes at a gas flow rate of 10 ml / s, a working current of 2 A, and a voltage of 100 V under oxygen CD cold plasma, and then cooled to room temperature to obtain an activated sodium vanadium phosphate positive electrode material.
[0111] Step 3, assembly of button cells: Place the activated sodium vanadium phosphate cathode material described in step (2) into a glove box and assemble button cells. All batteries must be left to stand for 12 hours before testing.
[0112] Physical and electrochemical tests were conducted on the positive electrode material of sodium vanadium phosphate obtained by oxygen CD cold plasma activation treatment. The oxygen doping content in the carbon layer was 587ppm. Compared with the untreated electrode, it had lower polarization and impedance, with polarization reduced by 45% and impedance reduced by 20%.
[0113] Example 8
[0114] A method for processing a positive electrode material comprises the following steps:
[0115] Step 1, preparation of lithium iron phosphate positive electrode material: using a conventional coating process, aluminum foil is used to coat the cut piece to obtain a lithium iron phosphate positive electrode material with a thickness of 80 μm.
[0116] Step 2, nitrogen DBD cold plasma activation treatment: first, the lithium iron phosphate positive electrode material in step (1) is coated with the active material on one side, and nitrogen DBD cold plasma activation treatment is performed for 4 minutes at a gas flow rate of 10 ml / s, an operating current of 4 A, and a voltage of 100 V under nitrogen DBD cold plasma, and then cooled to room temperature to obtain an activated lithium iron phosphate positive electrode material.
[0117] Step 3, assembly of button cells: Place the activated lithium iron phosphate cathode material described in step (2) into a glove box and assemble button cells. All batteries must be left to stand for 12 hours before testing.
[0118] Physical and electrochemical testing of the lithium iron phosphate cathode material obtained by nitrogen DBD cold plasma activation revealed a nitrogen doping concentration of 600 ppm in the carbon layer. Compared to untreated electrodes, the cathode exhibited lower polarization, higher capacity, and higher capacity retention. The voltage and capacity of the lithium iron phosphate treated at 5C are shown in Figure 13. The polarization of the treated battery was reduced by approximately 86%, while the capacity increased by 42.7%. The long-term cycling profile of the lithium iron phosphate treated at 5C is shown in Figure 14, showing a 69.7% improvement in capacity retention.
[0119] Example 9
[0120] A method for processing lithium iron phosphate positive electrode material comprises the following steps:
[0121] Step 1, preparation of lithium iron phosphate positive electrode material: using a conventional coating process, aluminum foil is used to coat the cut piece to obtain a lithium iron phosphate positive electrode material with a thickness of 80 μm.
[0122] Step 2, nitrogen DBD cold plasma activation treatment: first, the lithium iron phosphate positive electrode material in step (1) is coated with the active material on one side, and nitrogen DBD cold plasma activation treatment is performed for 10 minutes under nitrogen DBD cold plasma with a gas flow rate of 10 ml / s, an operating current of 4 A, and a voltage of 100 V. The activated lithium iron phosphate positive electrode material is obtained by cooling to room temperature.
[0123] Step 3, assembly of button cells: Place the activated lithium iron phosphate cathode material described in step (2) into a glove box and assemble button cells. All batteries must be left to stand for 12 hours before testing.
[0124] Physical and electrochemical testing of the lithium iron phosphate cathode material obtained by nitrogen DBD cold plasma activation revealed a nitrogen doping content of 700 ppm in the carbon layer, resulting in lower impedance compared to untreated electrodes. EIS traces of the lithium iron phosphate before and after treatment are shown in Figure 15. After treatment, the battery impedance decreased from 126.3Ω to 27.2Ω.
[0125] Although the present invention has been described above with reference to the exemplary embodiments, it will be apparent to those skilled in the art that various modifications and variations may be made to the exemplary embodiments of the present invention without departing from the spirit and scope defined in the claims.
Claims
1. A method for processing anode materials of a battery, It is characterized in that The following steps are involved: A battery positive electrode material having a carbon layer on at least a portion of its surface to be treated is subjected to cold plasma treatment to dope the carbon layer with active particles, wherein the active particle doping amount is not less than 50 ppm.
2. The method for processing a positive electrode material of a battery according to claim 1, It is characterized in that The power of cold plasma treatment is 100W to 500W.
3. The method for processing a positive electrode material of a battery according to claim 1 or 2, It is characterized in that The voltage of cold plasma treatment is 50V~150V, and the treatment current is 0.4A~2A.
4. The method for processing a positive electrode material of a battery according to claim 1 or 2, It is characterized in that The cold plasma treatment time is 1 min to 60 min.
5. The method for processing anode material of a battery according to claim 1 or 2, It is characterized in that The discharge for generating the cold plasma is selected from one or a combination of radio frequency plasma discharge, corona discharge, dielectric barrier discharge and sliding arc discharge.
6. The method for processing anode material of a battery according to claim 1 or 2, It is characterized in that The active particle doping is oxygen doping, nitrogen doping or a combination thereof.
7. The method for processing a positive electrode material of a battery according to claim 1 or 2, It is characterized in that The cold plasma treatment includes inputting one or a combination of precursor gases of oxygen and nitrogen into a cold plasma generator to generate active particles to dope the carbon layer, wherein the flow rate of the precursor gas is 1 ml / s to 15 ml / s.
8. The method for processing anode material of a battery according to claim 1 or 2, It is characterized in that The positive electrode material of the battery is a polyanion compound, a layered oxide, a spinel compound, Prussian blue or a ternary lithium battery positive electrode material.
9. The method for processing a positive electrode material of a battery according to claim 8, It is characterized in that The positive electrode materials of the battery are sodium vanadium phosphate, lithium iron phosphate, sodium titanium phosphate, sodium fluoride phosphate, LiMO 2 、NaMO 2 、LiN 2 O 4 , lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide, wherein M is Co, Ni, Mn, V or Fe, and N is Co, Nix, Mn or V.
10. The method for processing a positive electrode material of a battery according to claim 1, 2 or 8, It is characterized in that At least a portion of the surface of the doped battery positive electrode material has a rod-like shape.
11. The method for processing a positive electrode material of a battery according to claim 10, It is characterized in that The average length of the rod-like morphology is 1.5 μm to 3 μm, and the average diameter is 150 nm to 300 nm.
12. A battery positive electrode material, It is characterized in that At least a portion of its surface contains a carbon layer and at least a portion of the surface has a rod-like shape and forms a NaF layer, wherein the carbon layer is a carbon layer doped with active particles after cold plasma treatment, and the doping amount is not less than 50ppm.
13. The battery positive electrode material according to claim 12, It is characterized in that The active particles are oxygen, nitrogen or a combination thereof.
14. The battery positive electrode material according to claim 12 or 13, It is characterized in that The average length of the rod-like morphology is 1.5 μm to 3 μm, and the average diameter is 150 nm to 300 nm.
15. The battery positive electrode material according to claim 12 or 13, It is characterized in that The average thickness of the NaF layer is 6 nm to 10 nm, and the content of NaF is not less than 500 ppm.
16. A positive electrode sheet, It is characterized in that The invention comprises a current collector and a positive electrode material layer arranged on the current collector, wherein the positive electrode material layer comprises a battery positive electrode material processed by the method for processing a battery positive electrode material according to any one of claims 1 to 11 or comprises a battery positive electrode material according to any one of claims 12 to 14.
17. A battery, It is characterized in that Contains the positive electrode sheet as claimed in claim 16.