Preparation method of DLP photocuring 3D printing high-entropy fluorite oxide ceramic
Through DLP photocuring 3D printing technology, the problem of difficulty in preparing complex structures of high-entropy ceramics is solved in traditional methods, and the rapid and high-precision preparation of high-entropy fluorite oxide ceramics is achieved, and its application in multiple fields has been expanded.
Patent Information
- Application Number
- CN202411049056.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional ceramic preparation methods are difficult to make complex structures and personalized high-entropy ceramic materials, limiting their application in multiple key areas.
High entropy fluorite oxide ceramics were prepared by ball milling and drying oxide powder, mixing photosensitive resin and photoinitiator, 3D printing was performed and sintered in a muffle furnace.
It has achieved rapid and high-precision preparation of complex structures of high-entropy fluorite oxide ceramics, which broadened its application prospects in aerospace, thermoelectric materials and other fields.
Smart Images

Figure CN118978406A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing. Background Art
[0002] With the continuous progress of industry, advanced ceramic materials have been widely used in many key fields, such as petrochemical, steel metallurgy, mechanical electronics, aerospace, etc. The demand for ceramic materials in these fields is increasing, and this growing demand has put forward higher standards for the preparation speed, dimensional accuracy and complexity of performance structure of ceramic materials. Although the preparation and application of ceramic materials have a long history, traditional ceramic preparation methods, such as slurry sintering and machining cutting, have limitations in some aspects, especially in the manufacture of ceramics with complex structures and personalized needs. The emergence of 3D printing technology provides a new solution to this challenge. In recent years, the rapid development of 3D printing technology has made it possible to prepare ceramics with complex structures and personalized customization. This technology not only makes up for the shortcomings of traditional processing methods, but also brings new opportunities and possibilities to the field of ceramic manufacturing.
[0003] In recent years, the novel material design concept of "high entropy" has gradually emerged, and its origin can be traced back to the research and development of high entropy alloys. By carefully adjusting the ratio of different alloy elements and dissolving them together to form a unique single-phase solid solution, this concept has led to a new trend in materials science research. In addition, the concept of high entropy has been further extended to many fields such as high entropy ceramics, high entropy polymers and high entropy composite materials. The reason why high entropy materials have attracted much attention is due to their four core effects: high entropy effect in thermodynamics, lattice distortion effect in structure, hysteresis effect in dynamics and "cocktail" effect in performance. These effects together give high entropy materials excellent performance, making them have great potential and application value in the field of materials science. High entropy ceramics, also known as high entropy compounds, are a class of solid solutions of inorganic compounds. High-entropy ceramics with fluorite structures have excellent thermal properties, corrosion resistance, and mechanical properties. They have broad application prospects, including high-temperature protection and insulation in aerospace, thermoelectric materials, catalysts, etc. They are currently mainly prepared by solid-phase reaction, coprecipitation, sol-gel, and plasma sintering. However, due to the limitations of these molding methods, it is difficult to prepare special-shaped devices with complex structures. In response to the above problems, the present invention proposes a method for preparing DLP photocuring 3D printed high-entropy fluorite oxide ceramics. Applying 3D printing technology to high-entropy ceramics can produce devices with complex structures, achieve high-precision customized preparation, and further broaden the application prospects of high-entropy ceramics. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing, and to prepare high-entropy fluorite oxide ceramics with complex shapes by 3D printing, with fast printing speed, high precision and simple process.
[0005] To achieve the above object, the present invention provides a method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing, which specifically comprises the following steps:
[0006] S1, weighing various oxide powders and placing them in a ball mill, adding a dispersant, and after the ball milling, placing the slurry in a drying oven for drying;
[0007] S2, putting the dried oxide powder, photosensitive resin, photoinitiator and dispersant into a ball mill, and ball milling to obtain a uniformly mixed ceramic slurry;
[0008] S3, placing the ceramic slurry in a silo of a 3D printer, importing a 3D model for printing, and obtaining a high-entropy ceramic green body;
[0009] S4. Place the printed green body into a muffle furnace for degreasing and sintering to obtain high entropy fluorite oxide ceramics.
[0010] Preferably, in S1, the oxide powder includes zirconium oxide, yttrium oxide, hafnium oxide, cerium oxide, ytterbium oxide, erbium oxide, lanthanum oxide, and praseodymium oxide, and the particle size of the oxide powder is less than 10 μm, and the purity is ≥99.9%.
[0011] Preferably, in S1, the dispersant is anhydrous ethanol, the drying temperature is 60-70° C., and the drying time is 6-10 hours.
[0012] Preferably, in S1 and S2, the ball mill uses zirconium oxide balls as grinding media, the material-ball ratio in the ball mill is 1:2, the ball mill speed is 300 rad / min, and the ball milling time is 10 to 12 hours.
[0013] Preferably, in S2, the photosensitive resin is one or more of 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, and polyamino acrylate;
[0014] The photoinitiator is one or more of (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, camphorquinone, and 2-isopropylthioxanthone;
[0015] The dispersant is one or more of DISPERBYK-111, oleic acid, and ammonium citrate.
[0016] Preferably, in S2, the amount of dispersant added is 2 to 4 wt % of the oxide powder mass.
[0017] Preferably, in S2, the amount of photoinitiator added is 2-4 wt % of the mass of the photosensitive resin.
[0018] Preferably, in S3, the 3D printing process uses ultraviolet light with a wavelength of 385 nm, the printing layer thickness is 30 to 100 μm, and the printing speed is >100 layers / h.
[0019] Preferably, in S4, the degreasing temperature is 400-600° C., and the heating rate is 0.5-1° C. / min.
[0020] Preferably, in S4, the sintering temperature is 1500-1600° C., and the sintering time is 3-5 hours.
[0021] Therefore, the present invention provides a method for preparing high-entropy fluorite oxide ceramics by DLP photocuring 3D printing, by preparing a ceramic slurry with a high solid content, and then using DLP photocuring 3D printing technology to prepare a single-phase high-entropy fluorite oxide ceramic with a complex shape.
[0022] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is an X-ray diffraction pattern of a DLP light-cured 3D printed high-entropy fluorite oxide ceramic obtained in Example 1 of the present invention;
[0024] Figure 2 is an X-ray diffraction pattern of a DLP light-cured 3D printed high-entropy fluorite oxide ceramic obtained in Example 2 of the present invention;
[0025] Figure 3 This is a macroscopic optical picture of the porous high-entropy ceramic plate with a complex structure of the TPMS in Example 2 of the present invention. DETAILED DESCRIPTION
[0026] The present invention provides a preparation method of DLP light-curing 3D printing high-entropy fluorite oxide ceramics, comprising the following steps:
[0027] S1. Weigh the oxide powder and place it in a ball mill. The ball mill uses zirconium oxide balls as grinding media and anhydrous ethanol as a dispersant for ball milling. The material-ball ratio in the ball mill is 1:2, the ball mill speed is 300 rad / min, and the effective ball milling time is 10-12 hours. The ball milling mixes the raw materials evenly. After the ball milling is completed, the slurry is placed in a drying oven at 60-80°C and dried for 6-10 hours to obtain a powder with uniform composition.
[0028] The oxide powder includes zirconium oxide, yttrium oxide, hafnium oxide, cerium oxide, ytterbium oxide, erbium oxide, lanthanum oxide, and praseodymium oxide, with a particle size of less than 10 μm and a purity of ≥99.9%.
[0029] S2. Put the dried oxide powder together with the photosensitive resin, photoinitiator and dispersant into a ball mill, use zirconium oxide balls as the ball milling medium, the material-ball ratio in the ball mill is 1:2, the ball mill speed is 300rad / min, the effective ball milling time is 10 to 12h, and the ball milling obtains a uniformly mixed ceramic slurry.
[0030] The amount of dispersant added is 2-4wt% of the mass of the oxide powder, and the amount of photoinitiator added is 2-4wt% of the photosensitive resin; the photosensitive resin is one or more of 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, and polyamino acrylate; the photoinitiator is one or more of (2,4,6-trimethylbenzoyl) diphenyl phosphine oxide, camphorquinone, and 2-isopropylthioxanthone; the dispersant is one or more of DISPERBYK-111, oleic acid, and ammonium citrate.
[0031] S3. The ceramic slurry is placed in the hopper of the 3D printer, and the 3D model is imported for printing to obtain a high-entropy ceramic green body. During the 3D printing process, ultraviolet light with a wavelength of 385 nm is used, the printing layer thickness is 30 to 100 μm, and the printing speed is >100 layers / h.
[0032] S4. Place the printed green body into a muffle furnace for debinding at a temperature range of 400-600°C with a heating rate of 0.5-1°C / min, and then sinter at 1500-1600°C for 3-5h to obtain high entropy ceramics.
[0033] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Any other changes, modifications, substitutions, combinations, and simplifications made without violating the spirit and principle of the present invention should all be equivalent replacement methods and are included in the protection scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application, and all belong to the scope of protection of the present invention.
[0034] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.
[0035] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.
[0036] Unless otherwise specified in the present invention, the reagents, instruments, and equipment used are those commonly used by technicians in this field.
[0037] Example 1
[0038] This embodiment provides a method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing, which specifically includes the following steps:
[0039] S1, according to the chemical formula (La 0.2 G 0.2 Sm 0.2 Pr 0.2 Y 0.2 )2Zr2O7 weigh Y2O3, Gd2O3, Sm2O3, Pr6O 11 La2O3 and ZrO2 powders were placed in a ball mill and milled with zirconium oxide balls as grinding media and anhydrous ethanol as dispersant. The material-ball ratio in the ball mill was 1:2, the ball milling speed was 300 rad / min, and the ball milling time was 10 h. The milled slurry was dried at a drying oven temperature of 60 °C for 8 h.
[0040] S2. 1,6-hexanediol diacrylate and trimethylolpropane triacrylate are mixed in a volume ratio of 4:1 to prepare a photosensitive resin. Subsequently, the dried oxide powder and the prepared photosensitive resin are added into a ball mill in a volume ratio of 2:3. Then, 3% of the mass of the photosensitive resin as photoinitiator (2,4,6-trimethylbenzoyl) diphenylphosphine oxide and 3% of the mass of the oxide powder as dispersant DISPERBYK-111 are added. Zirconium oxide is used as the ball milling medium, the material-to-ball ratio is 1:2, and the ball milling is performed at 300 rad / min for 12 hours to obtain a uniform ceramic slurry with a solid content of 40 vol%.
[0041] S3. The ceramic slurry is loaded into the hopper of the 3D printer, and then the printing model is imported into the 3D printer, and the ceramic green body is printed with a layer thickness of 30 μm and an ultraviolet light with a wavelength of 385 nm for 20 seconds.
[0042] S4. Place the printed green body into a muffle furnace and heat it from room temperature to 400°C at a rate of 5°C / min, then debinder it at a rate of 1°C / min and heat it to 600°C, then heat it to 1600°C at a rate of 3°C / min for sintering. The sintering time is 4h, and finally cool it to 600°C at a rate of 3°C / min and cool it with the furnace.
[0043] Figure 1 The X-ray diffraction pattern shows that a high-entropy oxide ceramic with a single-phase fluorite structure is prepared in this embodiment.
[0044] Example 2
[0045] This embodiment provides a method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing, which specifically includes the following steps:
[0046] S1, according to the chemical formula (La 0.2 G 0.2 Er 0.2 Yb 0.2 Y 0.2 )2Zr2O7: Y2O3, Gd2O3, Er2O3, Yb2O3, La2O3 and ZrO2 powders are weighed in proportion and placed in a ball mill. Zirconia balls are used as grinding media and anhydrous ethanol is used as dispersant for ball milling. The material-ball ratio in the ball mill is 1:2, the ball milling speed is 300 rad / min, and the ball milling time is 10 h. The milled slurry is dried in the drying oven at 60°C for 8 h.
[0047] S2. Prepare a photosensitive resin with 1,6-hexanediol diacrylate, trimethylolpropane triacrylate and polyamino acrylate in a volume ratio of 7:2:1, then add the dried oxide powder and the prepared photosensitive resin into a ball mill in a volume ratio of 4:6, then add 2% of the total mass of photoinitiator (2,4,6-trimethylbenzoyl) diphenylphosphine oxide and 2% of the mass of the oxide powder dispersant DISPERBYK-111, use zirconium oxide as the ball milling medium, with a material-to-ball ratio of 1:2, and ball mill at 300 rad / min for 12 hours to obtain a uniform ceramic slurry with a solid content of 40 vol%.
[0048] S3. Load the ceramic slurry into the hopper of the 3D printer, then import the TPMS structure 3D model into the 3D printer, and print it with a layer thickness of 50 μm and a UV light of 385 nm wavelength for 10 s to obtain a ceramic green body.
[0049] S4. Place the printed green body into a muffle furnace and heat it from room temperature to 300°C at a rate of 5°C / min, then debind and heat it to 600°C at a rate of 0.5°C / min, then heat it to 1550°C at a rate of 3°C / min for sintering. The sintering time is 6h, and finally cool it to 600°C at a rate of 3°C / min and then cool it in the furnace.
[0050] Figure 2 The X-ray diffraction pattern shows that a high-entropy oxide ceramic with a single-phase fluorite structure is prepared in this embodiment.
[0051] Figure 3This is a macroscopic optical picture of the porous high-entropy ceramic plate with a complex structure of the TPMS of this embodiment.
[0052] In summary, the present invention adopts the above-mentioned DLP light-curing 3D printing method for preparing high-entropy fluorite oxide ceramics, and can use 3D printing to prepare high-entropy oxide ceramics with a single-phase fluorite structure, with fast printing speed, high precision and simple process.
[0053] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing high-entropy fluorite oxide ceramics by DLP photocuring 3D printing, characterized in that: The specific steps include: S1, weighing various oxide powders and placing them in a ball mill, adding a dispersant, and after the ball milling, placing the slurry in a drying oven for drying; S2, putting the dried oxide powder, photosensitive resin, photoinitiator and dispersant into a ball mill, and ball milling to obtain a uniformly mixed ceramic slurry; S3, placing the ceramic slurry in a silo of a 3D printer, importing a 3D model for printing, and obtaining a high-entropy ceramic green body; S4. Place the printed green body into a muffle furnace for degreasing and sintering to obtain high entropy fluorite oxide ceramics.
2. The method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing according to claim 1, characterized in that: In S1, the oxide powder includes zirconium oxide, yttrium oxide, hafnium oxide, cerium oxide, ytterbium oxide, erbium oxide, lanthanum oxide, and praseodymium oxide. The particle size of the oxide powder is less than 10 μm, and the purity is ≥99.9%.
3. The method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing according to claim 1, characterized in that: In the above S1, the dispersant is anhydrous ethanol, the drying temperature is 60-70° C., and the drying time is 6-10 hours.
4. The method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing according to claim 1, characterized in that: In S1 and S2, the ball mill uses zirconium oxide balls as grinding media, the material-ball ratio in the ball mill is 1:2, the ball mill speed is 300 rad / min, and the ball milling time is 10 to 12 hours.
5. The method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing according to claim 1, characterized in that: In S2, the photosensitive resin is one or more of 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, and polyamino acrylate; The photoinitiator is one or more of (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, camphorquinone, and 2-isopropylthioxanthone; The dispersant is one or more of DISPERBYK-111, oleic acid, and ammonium citrate.
6. The method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing according to claim 1, characterized in that: In the S2, the amount of dispersant added is 2-4 wt% of the oxide powder mass.
7. The method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing according to claim 1, characterized in that: In S2, the amount of photoinitiator added is 2-4 wt% of the mass of the photosensitive resin.
8. The method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing according to claim 1, characterized in that: In S3, the 3D printing process uses ultraviolet light with a wavelength of 385 nm, the printing layer thickness is 30 to 100 μm, and the printing speed is greater than 100 layers / h.
9. The method for preparing high-entropy fluorite oxide ceramics by DLP light-curing 3D printing according to claim 1, characterized in that: In the above S4, the degreasing temperature is 400-600°C, and the heating rate is 0.5-1°C / min.
10. The method for preparing high-entropy fluorite oxide ceramics by DLP photocuring 3D printing according to claim 1, characterized in that: In the step S4, the sintering temperature is 1500-1600° C. and the sintering time is 3-5 hours.
Citation Information
Patent Citations
Cordierite precursor photocuring paste and preparation method of porous cordierite ceramic with complex structure
CN114835511A
High-entropy ferrite porous ceramic with surface modified with metal clusters as well as preparation method and application of high-entropy ferrite porous ceramic
CN115433019A
Low-thermal-conductivity CMAS-corrosion-resistant high-entropy zirconate ceramic material as well as preparation method and application thereof
CN115925417A
3D printing high-entropy oxide ceramic and preparation method thereof
CN117326850A
High temperature sintering systems and methods
US20220219986A1
Cited By
High-entropy ceramic material as well as preparation method and application thereof
CN119350026A