Alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin as well as preparation method and application thereof
By developing alkali-soluble light/thermal double curing aliphatic polyester acrylate resin without aromatic structure, the problem of yellowing of existing alkali development soldering inks in white soldering inks is solved, and the problem of yellowing in soldering inks is realized. Excellent light/thermal curing performance and alkali corrosion development enhance its application prospects.
Patent Information
- Application Number
- CN202411278745.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The resins in existing alkaline development solder resist inks have poor yellowing resistance in white solder resist ink applications, making it difficult to meet industrial needs.
Develop an alkali-soluble light/thermal double curing aliphatic polyester acrylate resin to prepare polyester with acrylate groups at the end by reaction of aliphatic biepoxy compounds, aliphatic dibasic acids and unsaturated carboxylic acids. The intermediate product is reacted with aliphatic cyclic dianhydride to form a resin without aromatic structure, and has excellent light/thermal curing properties and alkaline corrosion development.
This resin overcomes the yellowing problem in solder resist inks, has good light/thermal curing properties and alkaline corrosion development. It is suitable for the field of low yellow change solder resist inks, improving application prospects.
Smart Images

Figure CN118978676A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solder resist ink resins, and in particular relates to an alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin and a preparation method and application thereof. Background Art
[0002] UV curing technology is a curing technology that uses ultraviolet light to decompose photoinitiators to produce free radicals, which in turn initiates the polymerization of double bonds in prepolymers to form a cross-linked structure. Compared with traditional thermal curing, UV curing does not require heating, and cross-linking and curing can be completed within a few seconds to tens of seconds at room temperature, which can greatly shorten production time and reduce energy consumption. In addition, the system does not contain organic solvents, making it more convenient and environmentally friendly. Among them, epoxy acrylate is the most widely used and largest-volume photocurable oligomer, with the characteristics of fast curing speed and low cost. The cured film made from it has the advantages of high rigidity, high hardness, high gloss, and excellent chemical resistance. However, due to the interaction between molecules, epoxy acrylate resins have high viscosity and brittleness, which limits their application in electronics, aerospace and other fields.
[0003] Solder resist ink is one of the key materials for making printed circuit boards (PCBs). It is applied to the etched circuit board and cured to form a protective film with excellent insulation, heat resistance, adhesion, etc., which can prevent the circuit from disconnecting. In the tinning process, solder resist ink can also control the tinning area to prevent short circuits caused by dense solder joints, but the traditional screen printing solder resist ink has poor positioning accuracy and resolution, and the dry film type solder resist ink has poor adhesion to the circuit board. Since the concept of alkali-developable photosensitive solder resist ink was proposed in the late 1980s, some foreign institutions have conducted many related development and research. The solder resist ink mainly contains carboxylated epoxy acrylate resin and B component epoxy resin. After being fully printed on the etched circuit board through the screen, the solvent is pre-baked to remove the solvent, and the photocured latent image is obtained by mask exposure. After being developed with a dilute alkali aqueous solution, it is further cured by heating at medium temperature to form a high-performance solder resist layer. The photo-imaging type solder resist ink has excellent positioning accuracy and adhesion.
[0004] At present, most of the light / heat dual-curing resins used in alkali-developable solder resist inks contain aromatic ring structures, such as the o-cresol epoxy acrylate resin, which is widely used in the field of solder resist inks. However, the aromatic structure contained in it has poor yellowing resistance, which limits its application in white solder resist inks. At the same time, although the yellowing can be alleviated to a certain extent by adding antioxidants to the resin, it cannot fundamentally solve the problem of resin yellowing. Therefore, the development of alkali-developable solder resist ink resins with good yellowing resistance is one of the problems that need to be solved in the industry. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the present invention proposes an alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin, which has excellent light / heat curing performance and alkaline etching developability, and has good application prospects in the field of solder resist inks, especially low yellowing solder resist inks.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] The first aspect of the present invention provides an alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin, the molecular structure of the polyester acrylate resin is shown in formula (I):
[0008]
[0009] In formula (I), R1 is derived from the corresponding aliphatic diepoxy compound, including (a) and mixtures thereof; R2 is derived from the corresponding aliphatic dibasic acid, including and mixtures thereof, wherein n=8-25; R3 is derived from the corresponding aliphatic cyclodianhydride, including and mixtures thereof; R4 is derived from the corresponding unsaturated carboxylic acid, including H, CH3 and mixtures thereof; m is determined by the number average molecular weight of the resin, the number average molecular weight of the resin is Mn=5000-10000, and the acid value is 60-80 mgKOH / g.
[0010] Preferably, in the polyester acrylate resin represented by formula (I), R1 is selected from (a) + (e) or (d) + (e), more preferably (a) + (e), and the mass ratio of (a): (e) is preferably 9:1 to 8:2; R2 is selected from R3 is selected from R4 is selected from H.
[0011] More preferably, the polyester acrylate resin has the following structural formula:
[0012]
[0013] R1 is R`1 is Its molecular weight Mn = 400 ~ 1000; R2 is selected from R3 is x1 and x2 are determined by the number average molecular weight of the resin, x1:x2=10:1~4:1, and the number average molecular weight of the resin is 5500~9100.
[0014] The second aspect of the present invention provides a method for preparing the alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin according to the first aspect, comprising the following steps:
[0015] S1. As shown in the following reaction formula, an aliphatic diepoxy compound, an aliphatic dibasic acid and a ring-opening reaction catalyst are dissolved in a solvent under an inert atmosphere, and heated to react until the acid value = 0 to obtain a polyester intermediate product with an epoxy group at the end;
[0016] This step of reaction is that the diepoxy compound and the dibasic acid undergo a ring-opening addition reaction between the epoxy group and the carboxyl group to generate a polyester intermediate product with an epoxy group at the end;
[0017]
[0018] In the reaction formula, the values of R1 and R2 are the same as those in Example 1 or 2; the molar ratio of y to x is 0.8:1 to 0.9:1; m is determined by the number average molecular weight of the product, which is M n =4500~8500;
[0019] S2. As shown in the following reaction formula, a polymerization inhibitor and an unsaturated carboxylic acid are added to the intermediate product of S1, and a ring-opening reaction catalyst and a solvent are added, and the reaction is continued by heating until the epoxy value = 0, so as to obtain a polyester intermediate product with an acrylate / methacrylate group at the end;
[0020] This step of reaction is the ring-opening addition of the terminal epoxy group of the intermediate product obtained in S1 with the carboxyl group of the unsaturated carboxylic acid to generate a polyester intermediate product with an acrylate / methacrylate group at the end;
[0021]
[0022] In the reaction formula, the values of R1, R2, and R4 are the same as those in Example 1 or 2; m is determined by the number average molecular weight of the product, which is M n =4500~8500;
[0023] S3, adding aliphatic cyclodianhydride and solvent to the intermediate product of S2, heating and reacting until the acid value is 60-80, to obtain the target product;
[0024] This step is to react the hydroxyl side group of the intermediate product obtained in S2 with the cyclic dianhydride to convert the hydroxyl side group into a carboxyl side group;
[0025]
[0026] In the reaction formula, the values of R1, R2, R3, R4 and m are the same as those in Example 1 or 2.
[0027] Preferably, in S1, the aliphatic diepoxy compound is selected from hydrogenated bisphenol A diglycidyl ether, polyethylene glycol diglycidyl ether, 1,4-butanediol glycidyl ether, neopentyl glycol diglycidyl ether, 1,2-cyclohexanediol diglycidyl ether and mixtures thereof.
[0028] More preferably, the aliphatic diepoxy compound is selected from hydrogenated bisphenol A diglycidyl ether, polyethylene glycol glycidyl ether, 1,2-cyclohexanediol diglycidyl ether and mixtures thereof.
[0029] More preferably, the aliphatic diepoxy compound is selected from a mixture of polyethylene glycol glycidyl ether and hydrogenated bisphenol A epoxy resin, and the mass ratio of polyethylene glycol glycidyl ether (such as polyethylene glycol 400 diglycidyl ether) to hydrogenated bisphenol A epoxy resin (such as epoxy resin 1510) is 1:9 to 2:8.
[0030] Preferably, in S1, the aliphatic dibasic acid is selected from 1,4-cyclohexyldicarboxylic acid, C4-C10 aliphatic dibasic acid and mixtures thereof.
[0031] More preferably, the aliphatic dibasic acid is selected from 1,4-cyclohexyldicarboxylic acid.
[0032] Preferably, the ring-opening reaction catalyst in S1 is selected from tertiary amines, trialkylphosphines and mixtures thereof, and the added amount thereof is 0.2% to 1% of the total mass of the reactants.
[0033] More preferably, the ring-opening reaction catalyst is selected from triethylamine, triphenylphosphine and mixtures thereof, more preferably triphenylphosphine.
[0034] Preferably, the solvent in S1 is selected from at least one of ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, dipropylene glycol methyl ether, propylene glycol methyl ether, trimethylbenzene and tetramethylbenzene.
[0035] More preferably, the solvent is selected from diethylene glycol ethyl ether acetate.
[0036] Preferably, in S2, the unsaturated carboxylic acid is selected from acrylic acid, methacrylic acid and a mixture thereof, and the molar number of the unsaturated carboxylic acid added is 1.1 times the theoretically remaining molar number of epoxy groups in the system after the reaction of S1 is completed. The theoretically remaining molar number of epoxy groups in the system is calculated by subtracting the molar number of carboxyl groups contained in the dicarboxylic acid from the molar number of epoxy groups contained in the diepoxy compound.
[0037] More preferably, the unsaturated carboxylic acid is selected from acrylic acid.
[0038] Preferably, in S2, the polymerization inhibitor is selected from 2,6-di-tert-butyl-p-cresol (BHT) and 4-methoxyphenol, and the added amount of each polymerization inhibitor is 0.2% to 0.4% of the mass of the unsaturated carboxylic acid added in S2.
[0039] Preferably, the aliphatic cyclodianhydride in S3 is selected from hexahydrophthalic anhydride, succinic anhydride and a mixture thereof, and the amount thereof added is such that the acid value of the final product system is 60 to 80 mgKOH / g, and the specific calculation formula is:
[0040]
[0041] More preferably, the aliphatic cyclodianhydride is selected from hexahydrophthalic anhydride.
[0042] The third aspect of the present invention provides the use of the alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin described in the first aspect in the preparation of solder resist ink.
[0043] The terminal acrylate groups in the polyester acrylate resin molecules of the present invention give the polymer light-curing properties, and the carboxyl side groups give the polymer alkali solubility and thermosetting properties (forming a thermosetting system with an added polyepoxy compound), and the structure does not contain an aromatic structure. It is used in the preparation of solder mask inks to solve the problem of yellowing.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] The present invention discloses an aliphatic polyester acrylate resin, wherein the terminal acrylate group contained in the polyester acrylate resin gives the resin photocuring properties, and the carboxyl side group contained in the polyester acrylate resin gives the resin alkali solubility and heat curing properties, so the polyester acrylate resin belongs to an alkali-soluble light / heat dual-curing resin. The present invention also discloses a preparation method of the aliphatic polyester acrylate resin, namely, firstly, an intermediate product with an epoxy group at the end is obtained by reacting an aliphatic diepoxy compound and an aliphatic dibasic acid, then the intermediate product is reacted with acrylic acid to obtain an intermediate product with an acrylate group at the end, and finally the intermediate product is reacted with an aliphatic cyclodianhydride to obtain a target product. The aliphatic polyester acrylate resin prepared by the method of the present invention has excellent light / heat curing properties and alkaline etching developability, and because the resin does not contain an aromatic structure, it can be used to prepare solder resist ink to overcome its defect of not being resistant to yellowing, so it has good application prospects in the field of low yellowing solder resist ink. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is the GPC graph of the polyester intermediate with epoxy groups at the end;
[0047] Figure 2 It is the GPC chart of polyester acrylate resin;
[0048] Figure 3 This is a comparison chart of polyester acrylate resin before and after the development test. DETAILED DESCRIPTION
[0049] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0050] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0051] The molecular weight of the product was determined by GPC. The GPC test conditions were as follows: an Agilent Technologies PL-GPC 50 gel permeation chromatograph was used for the determination. The GPC columns were one Agilent PL 10 μm MIXED-B gel column and two Agilent PL 5 μm MIXED-D gel columns connected in series. Polystyrene (PS) was used as the standard sample. The test temperature of the refractive index detector was 40 °C. THF was used as the mobile phase at a flow rate of 1.0 mL min -1 .
[0052] Example 1: Synthesis of polyester acrylate resin
[0053] S1. First, under a nitrogen atmosphere, 13.5 g of epoxy resin 1510, 1.5 g of polyethylene glycol 400 diglycidyl ether (PEG400DG), 10.45 g of diethylene glycol ethyl ether acetate (DGMEA) and 5.9 g of 1,4-cyclohexanedicarboxylic acid (CHDA) were added to the reactor, heated to 120° C. and stirred for 10 minutes, and then 0.052 g of triphenylphosphine (PPh3, 0.25 wt%) as a ring-opening reaction catalyst was added, and the reaction was continued at 120° C. for 6 hours until the acid value = 0, to obtain a polyester intermediate product with an epoxy group at the end. The number average molecular weight of the product measured by GPC was about 7500 ( Figure 1 ), the reaction formula is as follows:
[0054]
[0055] Where: R1 is R`1 is Its molecular weight Mn = 400; R2 is selected from (x1+x2):y (molar ratio) = 1:0.9; x1:x2 = 10:1.
[0056] S2. Add 0.622 g of acrylic acid (AA) to the intermediate product of S1 under a nitrogen atmosphere, and add a portion of triphenylphosphine catalyst (0.052 g), 0.0012 g of 2,6-di-tert-butyl-p-cresol (BHT), 0.0012 g of 4-methoxyphenol (MEHQ) and 4 g of diethylene glycol ethyl ether acetate. After mixing, continue to stir and react at 120° C. for 8 hours until the epoxy value = 0, to obtain a polyester intermediate product with an acrylate / methacrylate group at the end, and the reaction formula is as follows:
[0057]
[0058] Where: R1 is R`1 is Its molecular weight Mn = 400; R2 is selected from (x1+x2):y (molar ratio) = 1:0.9; x1:x2 = 10:1.
[0059] S3, under nitrogen protection, the intermediate product of S2 was cooled to 100°C, and then 6.06g of hexahydrophthalic anhydride (HHPA) and 2g of diethylene glycol ethyl ether acetate were added, and the mixture was stirred and reacted at this temperature for 3 hours until the acid value was 80mg KOH / g. After stopping the reaction, a polyester acrylate resin was obtained, and its number average molecular weight was about 9100 ( Figure 2 ), the reaction formula is as follows:
[0060]
[0061] Where: R1 is R`1 is Its molecular weight Mn = 400; R2 is selected from R3 is (x1+x2):y (molar ratio) = 1:0.9; x1:x2 = 10:1.
[0062] Examples 2-7 and Comparative Example 1: Synthesis of Polyester Acrylate Resin
[0063] The raw materials and reaction methods used in Examples 2 to 7 and Comparative Example 1 are the same as those in Example 1, except that the proportions of the reactants are different. The amounts of the reactants and the reaction results in Examples 1 to 7 and Comparative Example 1 are shown in Table 1.
[0064] Table 1 Synthesis of polyester acrylate resins of Examples 1-7 and Comparative Example 1
[0065]
[0066]
[0067] Experimental example: Alkali solubility and light / heat curing test of polyester acrylate resin
[0068] First, the polyester acrylate resins obtained in Examples 1 to 7 and Comparative Example 1 were respectively coated on a glass slide using a 15 μm coating rod, and after drying at 70° C., they were placed in a 1% Na2CO3 solution at a temperature of 60° C. for an alkali solubility test. During the test, magnetic stirring was performed at 600 rpm. The test results are shown in Table 2.
[0069] As can be seen from Table 2, the polyester acrylate resins of Examples 1 to 7 have good alkali solubility, while Comparative Example 1, in the case of a resin molecular weight close to that of other examples, has poor solubility in a sodium bicarbonate aqueous solution due to the absence of PEG400DG, and still does not dissolve after immersion for 20 minutes. It can be seen that in order to obtain good alkali solubility, it is necessary to add an appropriate amount of PEG400DG. At the same time, from the comparison of Examples 1, 4, and 7, it can be seen that with the increase of the PEG400DG content in the resin, the alkali dissolution time of the resin is shortened due to the good water solubility of PEG; and from the comparison of Examples 4, 5, and 6, it can be seen that the greater the acid value of the resin, the more carboxyl groups are introduced, and the better the alkali solubility.
[0070] Table 2 Test results of resin alkali solubility of Examples 1 to 7 and Comparative Example 1
[0071]
[0072] Note: * means no dissolution within 20 min.
[0073] At the same time, the polyester acrylate resins of Examples 1 to 7 were used to prepare white light / heat curing resins, and their light curing properties were further compared and studied, as follows:
[0074] (1) The polyester acrylate resins obtained in Examples 1 to 7 were respectively mixed with a reactive diluent (trimethylolpropane triacrylate, TMPTA), a curing agent (hydrogenated bisphenol A epoxy resin 1510), a photoinitiator (TPO, (2,4,6-trimethylbenzoyl)phenylphosphine oxide) and a solvent (diethylene glycol monoethyl ether acetate, DGMEA) to prepare a light / heat curing composite resin. The proportions of each component are shown in Table 3.
[0075] Table 3 Formulas of light / heat curing composite resins prepared from polyester acrylate resins obtained in different embodiments
[0076]
[0077] (2) The prepared composite resin is evenly coated on a glass slide, dried at 70°C for 30 minutes, and then exposed to ultraviolet light for 10 seconds under a 395nm, 300W ultraviolet lamp to obtain a photocured film. Then, heat treatment is performed at 120°C and 150°C for 2 hours and 1.5 hours respectively to further heat cure the photocured coating film, and the coating film sample is obtained after cooling to room temperature.
[0078] (3) The hardness of the coating samples after light curing and heat curing was measured according to the coating pencil hardness method of GB / T 6739-1996, and the degree of curing was measured by the gel content determination method. The test results are shown in Table 4.
[0079] From the results in Table 4, it can be seen that the degree of photocuring is related to the double bond content in the polyester acrylate resin. After the resin with a high double bond content is photocured, the degree of photocuring is significantly improved. After photocuring, the degree of curing is significantly improved by heat curing at 150°C for 1.5 hours compared with heat curing at 120°C for 2 hours, and the pencil hardness is also improved. The above results show that the polyester acrylate resins of the present invention have good light / heat dual curing properties.
[0080] Table 4 Light / heat curing performance test of polyester acrylate resin of Examples 1-7*
[0081]
[0082] *Hardness 1: Hardness after light curing; G1: Gel content after light curing; Hardness 2: Hardness after heat curing at 120℃ for 2h after light curing; G2: Gel content after heat curing at 120℃ for 2h after light curing; Hardness 3: Hardness after heat curing at 150℃ for 1.5h after light curing; G3: Gel content after heat curing at 150℃ for 1.5h after light curing.
[0083] Finally, the polyester acrylate resins obtained in Examples 1 to 7 and Comparative Example 1 were prepared into light / heat curing resin white pastes, and the developability test was carried out as follows:
[0084] (1) Preparation of white color paste: Prepare a composite resin according to the formula in Table 3, and then add titanium dioxide to prepare a white color paste, where the amount of titanium dioxide added is 35wt% of the composite resin. The specific preparation method is: add the composite resin, titanium dioxide and zirconium beads (2mm, the amount added is equal to the mass of the resin) into a grinding pot, grind for 1 hour, and filter with a 400-mesh screen to obtain a white light / heat curing resin color paste (Examples 1-7).
[0085] (2) White resin photocuring: The obtained white resin color paste was evenly coated on a glass slide, dried at 70°C for 30 min, and a portion of the coating was covered with a round cover as a mask. The coating was then exposed to ultraviolet light at 395 nm and 300 W for 10 s to obtain a cured coating.
[0086] (3) Development test: The thickness of the light-cured coating film was measured with a paint film thickness meter, and then the coating film was placed in a 1% Na2CO3 solution at a temperature of 60°C for an alkali solubility test. During the test, magnetic stirring was performed at 600 rpm. The test results are shown in Table 5 ( Figure 3 (a comparison chart before and after alkali dissolution).
[0087] As can be seen from Table 5, the alkali dissolution time is related to factors such as resin molecular weight, hydrophilic group content, acid value, and film thickness. It can be seen from Examples 3, 7, and Comparative Example 1 that when the film thickness of Example 3 is smaller than that of Example 7, the alkali dissolution time is extended, indicating that as the PEG content in the resin increases, the alkali solubility also increases; among Examples 4, 5, and 6, the dissolution of Example 6 is not good, and it can be seen that as the acid value of the system decreases, the alkali solubility of the ink after photocuring also decreases; it can be seen from Examples 2 and 3 that the alkali washing time of the photosensitive resin with a high molecular weight after photocuring will be longer.
[0088] Table 5 Development test results of white resin color paste prepared in different embodiments after photocuring
[0089]
[0090] *Partially dissolved.
[0091] In summary, the alkali-soluble light / heat dual-curing polyester acrylate resin prepared by the method of the present invention has excellent light / heat curing performance and alkali etching developability. Since it does not contain an aromatic structure that is prone to yellowing, it has good application prospects in the field of solder resist inks, especially low-yellowing solder resist inks.
[0092] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. An alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin, characterized in that: The molecular structure of the polyester acrylate resin is shown in formula (I): In formula (I), R1 is derived from the corresponding aliphatic diepoxy compound, including and mixtures thereof, wherein n=8-25; R2 is derived from the corresponding aliphatic dibasic acid, including and mixtures thereof; R3 is derived from the corresponding aliphatic cyclic dianhydride, including and mixtures thereof; R4 is derived from the corresponding unsaturated carboxylic acid, including H, CH3 and mixtures thereof; m is determined by the number average molecular weight of the resin, the number average molecular weight of the resin is Mn=5000-10000, and the acid value is 60-80 mgKOH / g.
2. The alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin according to claim 1, characterized in that: In the polyester acrylate resin represented by formula (I), R1 is selected from (a) + (e) or (d) + (e); R2 is selected from R3 is selected from R4 is selected from H.
3. The alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin according to claim 2, characterized in that: The polyester acrylate resin has the following structural formula: R1 is R`1 is Its molecular weight Mn = 400 ~ 1000; R2 is selected from R3 is x1 and x2 are determined by the number average molecular weight of the resin, x1:x2=10:1~4:1, and the number average molecular weight of the resin is 5500~9100.
4. The method for preparing the alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin according to claim 1 or 2, characterized in that: The following steps are involved: S1. As shown in the following reaction formula, an aliphatic diepoxy compound, an aliphatic dibasic acid and a ring-opening reaction catalyst are dissolved in a solvent under an inert atmosphere, and heated to react until the acid value = 0 to obtain a polyester intermediate product with an epoxy group at the end; In the reaction formula, the values of R1 and R2 are the same as those in Example 1 or 2; the molar ratio of y to x is 0.8:1 to 0.9:1; m is determined by the number average molecular weight of the product, which is M n =4500~8500; S2. As shown in the following reaction formula, a polymerization inhibitor and an unsaturated carboxylic acid are added to the intermediate product of S1, and a ring-opening reaction catalyst and a solvent are added, and the reaction is continued by heating until the epoxy value = 0, so as to obtain a polyester intermediate product with an acrylate / methacrylate group at the end; In the reaction formula, the values of R1, R2, and R4 are the same as those in Example 1 or 2; m is determined by the number average molecular weight of the product, which is M n =4500~8500; S3, adding aliphatic cyclodianhydride and solvent to the intermediate product of S2, heating and reacting until the acid value is 60-80, to obtain the target product; In the reaction formula, the values of R1, R2, R3, R4 and m are the same as those in Example 1 or 2.
5. The method for preparing the alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin according to claim 4, characterized in that: In S1, the aliphatic diepoxy compound is selected from hydrogenated bisphenol A diglycidyl ether, polyethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,2-cyclohexanediol diglycidyl ether and mixtures thereof; the aliphatic dibasic acid is selected from 1,4-cyclohexyl dicarboxylic acid, C4-C10 aliphatic dibasic acid and mixtures thereof.
6. The method for preparing the alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin according to claim 4, characterized in that: S1 The ring-opening reaction catalyst is selected from tertiary amines, trialkylphosphines and mixtures thereof, and the added amount thereof is 0.2% to 1% of the total mass of the reactants.
7. The method for preparing the alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin according to claim 4, characterized in that: S1 The solvent is selected from at least one of ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol diethyl ether acetate, diethylene glycol butyl ether acetate, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, dipropylene glycol methyl ether, propylene glycol methyl ether, trimethylbenzene and tetramethylbenzene.
8. The method for preparing the alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin according to claim 4, characterized in that: In S2, the unsaturated carboxylic acid is selected from acrylic acid, methacrylic acid and a mixture thereof, and the molar number of the unsaturated carboxylic acid added is 1.1 times the theoretical molar number of epoxy groups remaining in the system after the reaction of S1 is completed, and the theoretical molar number of epoxy groups remaining in the system is calculated by subtracting the molar number of carboxyl groups contained in the dicarboxylic acid from the molar number of epoxy groups contained in the diepoxy compound; the inhibitor is selected from 2,6-di-tert-butyl-p-cresol (BHT) and 4-methoxyphenol, and the added amount of each inhibitor is 0.2% to 0.4% of the mass of the unsaturated carboxylic acid added in S2.
9. The method for preparing the alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin according to claim 4, characterized in that: S3 The aliphatic cyclodianhydride is selected from hexahydrophthalic anhydride, succinic anhydride and a mixture thereof, and the amount thereof added is such that the acid value of the final product system is 60-80 mgKOH / g. The specific calculation formula is:
10. Use of the alkali-soluble light / heat dual-curing aliphatic polyester acrylate resin according to any one of claims 1 to 3 in the preparation of solder resist ink.
Citation Information
Patent Citations
Epoxy acrylic resin, and preparation method and applications thereof
CN109988283A
Modified polyester acrylate resin and preparation method thereof
CN114805767A
Thermosetting hydrophobic polyester resin as well as preparation method and application thereof
CN115926131A
Photocurable composition, cured product of same, and coated article
WO2024024370A1