Preparation method of halogen-free flame-retardant nylon composite material
By modifying 2-carboxyethylphenylphosphoric acid and combining copper salt antioxidants and maleic anhydride grafts, the problems of its molecular weight reduction and poor mechanical properties in nylon composite materials are solved, achieving high efficiency The flame retardant and stability are improved, reaching the V0 level flame retardant performance.
Patent Information
- Application Number
- CN202411265740.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When added to the polyamide, 2-carboxyethylphenylphosphoric acid leads to problems such as the polymer's molecular weight and poor mechanical properties, and the acidity of its aqueous solution makes the polymerization reaction unstable, affecting the flame retardant performance.
By modifying decyldiamine with 2-carboxyethylphenylphosphoric acid, amide bonds and phosphonates are formed to form modified halogen-free flame retardants, and when preparing nylon composites, the modified flame retardants are used to prepare the nylon composite materials. , copper salt antioxidants and maleic anhydride graft compatible agents to improve the flame retardancy and stability of the material.
It effectively improves the flame retardancy and stability of composite materials, improves tensile strength, bending strength and anti-aging properties, so that the material reaches the V0 level flame retardant standard.
Smart Images

Figure CN118978692A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of long carbon chain nylon materials, in particular to a method for preparing a halogen-free flame-retardant nylon composite material. Background Art
[0002] Nylon 1012 is a product of the polymerization of two monomers, decanediamine and dodecanedioic acid, referred to as PA1012 in English. It is a new type of nylon developed by Evonik Industries of Germany in the 1980s and 1990s. The monomer decanediamine of PA1012 comes from biomass materials, which belongs to some bio-sourced nylon plastic varieties. It is also the latest long carbon chain nylon developed after PA1010, PA11 and PA12.
[0003] 2-Carboxyethylphenylphosphonic acid has the advantages of simple synthesis process and low production cost. As a halogen-free and efficient reactive organic flame retardant, it has the advantages of being halogen-free and non-toxic. When used as a reactive flame retardant for polymer matrix flame retardancy, it also has the advantages of good flame retardant stability and no migration and precipitation over time. 2-Carboxyethylphenylphosphonic acid has now been widely used in the flame retardant modification of various polymer materials such as polyester and epoxy resin. The initial decomposition temperature of 2-carboxyethylphenylphosphonic acid is low. Once it exceeds its own decomposition temperature, it will decompose rapidly and has poor thermal stability. It cannot be used for flame retardancy of polymer materials with high processing or polymerization temperatures. And because it contains phosphoric acid and carboxylic acid groups in its structure, the aqueous solution of 2-carboxyethylphenylphosphorous acid is acidic. If it is directly added to the condensation polymerization reaction system of polyamide, on the one hand, it will destroy the molar ratio of the two condensation groups in the reaction system, end-cap the polymer, reduce the molecular weight of the polymer, and act as an inhibitor; on the other hand, because the aqueous solution is acidic, it will accelerate the reverse reaction of the condensation polymerization process, promote the hydrolysis of the polymer, and shift the reaction equilibrium to the left, which is not conducive to the reaction, resulting in low molecular weight and poor mechanical properties of the polymer material. If 2-carboxyethylphenylphosphorous acid is used for flame retardant modification of long carbon chain polyamide PA1012, 2-carboxyethylphenylphosphorous acid needs to be modified to meet the polymerization conditions of PA1012. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a halogen-free flame-retardant nylon composite material. Decanediamine, one of the monomers for synthesizing PA1012, is used to modify 2-carboxyethylphenyl hypophosphorous acid. The amino group (-NH2) of decanediamine reacts with the carboxylic acid group (-COOH) of 2-carboxyethylphenyl hypophosphorous acid to generate an amide bond (-CONH-), and can also react with the hypophosphorous acid group (-PO(OH)H) of 2-carboxyethylphenyl hypophosphorous acid to form a phosphonate. The problem of molecular weight reduction and poor mechanical properties caused by adding 2-carboxyethylphenyl hypophosphorous acid into PA1012 is solved, and the flame retardancy and stability of the composite material are effectively improved.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention provides a halogen-free flame-retardant nylon composite material, which comprises the following components by mass percentage:
[0007] Modified halogen-free flame retardant 10-20%, decanediamine 35-55%, dodecanedioic acid 25-45%, compatibilizer 0.1-2%, antioxidant 0.2-0.6%, lubricant 0.2-0.4% and nucleating agent 0.3-0.5%.
[0008] Further, based on the above technical solution of the present invention, the preparation method of the modified halogen-free flame retardant comprises the following steps:
[0009] Decanediamine is placed in a solvent, and the mixture is stirred while cooling to obtain a mixed solution; 2-carboxyethylphenylphosphorous acid is added to the mixed solution, and the mixture is heated and stirred, and after cooling, the mixture is filtered, and the obtained filter cake is washed to obtain a modified halogen-free flame retardant.
[0010] Further, based on the above technical solution of the present invention, the solvent is a polar solvent;
[0011] Preferably, the polar solvent includes one or more of water, ethanol, methanol, dimethyl sulfoxide or acetonitrile. Further, based on the above technical solution of the present invention, the cooling and stirring conditions include:
[0012] The temperature is 0-5°C, the stirring rate is 130-180r / min, and the stirring time is 30-60min;
[0013] And / or, the conditions of heating and stirring include:
[0014] The temperature is 60-90°C, the stirring rate is 130-180r / min, and the stirring time is 6-8h;
[0015] And / or, the washing comprises:
[0016] The detergent is a polar solvent;
[0017] Preferably, the polar solvent includes one or more of water, ethanol, methanol, dimethyl sulfoxide or acetonitrile;
[0018] And / or, the detergent is the same as the solvent.
[0019] Further, based on the above technical solution of the present invention, the mass ratio of the decanediamine to the solvent is 1:2-3;
[0020] The mass ratio of the decanediamine to the 2-carboxyethylphenylphosphorous acid is 2-3:1.
[0021] Further, on the basis of the above technical solution of the present invention, the compatibilizer is a polymer containing maleic anhydride grafts;
[0022] Preferably, the polymer containing maleic anhydride grafts includes one or more of maleic anhydride grafted polyolefins, maleic anhydride grafted polyesters, maleic anhydride grafted polyethers, and maleic anhydride grafted polyamides;
[0023] And / or, the antioxidant is a copper salt antioxidant;
[0024] Preferably, the copper salt antioxidant includes one or more of styrene copper maleate, copper naphthenate, triphenylphosphine copper, copper linoleate, and copper stearate;
[0025] And / or, the lubricant is one or more of paraffin wax, polyethylene wax, polypropylene wax, polysiloxane, and silicone powder;
[0026] And / or, the nucleating agent is a sodium salt of a long carbon chain linear saturated carboxylic acid or a calcium salt of a long carbon chain linear saturated carboxylic acid;
[0027] Preferably, the long carbon chain linear saturated carboxylic acid sodium salt includes one or more of sodium laurate, sodium stearate, sodium oleate, and sodium myristic acid;
[0028] Preferably, the long carbon chain linear saturated carboxylic acid calcium salt includes one or more of TMN-102, calcium stearate, and calcium montanate.
[0029] The present invention also provides a method for preparing the halogen-free flame-retardant nylon composite material as described above, comprising the following steps:
[0030] S1: placing the modified halogen-free flame retardant, decanediamine and dodecanedioic acid in water, adjusting the pH value, and then transferring to a reactor for heating reaction to obtain PA1012;
[0031] S2: Dry PA1012, compatibilizer, antioxidant, lubricant and nucleating agent, and mix them evenly in a stirrer;
[0032] S3: The uniformly mixed materials are melt-blended in a twin-screw extruder and extruded into granules.
[0033] Further, based on the above technical solution of the present invention, step S1 specifically includes the following steps:
[0034] S11: placing the modified halogen-free flame retardant, decanediamine and dodecanedioic acid in water, adjusting the pH value to 7.3-7.5, transferring to a reactor, and heating the reactor for 2-3 hours at a reactor temperature of 210-250° C., a stirring rate of 100-120 r / min, and a reactor pressure of 2.4-2.6 MPa;
[0035] S12: After the heating reaction is completed, the temperature is raised to 260-270°C, and exhaust and pressure reduction are started;
[0036] Preferably, the pressure reduction rate is 0.001-0.015 MPa / s, and the pressure reduction time is 40-50 min;
[0037] S13: After the pressure reduction is completed, the vacuum pump is further started to maintain the negative pressure in the reactor at 0.98-0.95 MPa for 1-2 hours; finally, nitrogen is filled in to break the vacuum, and the reactor is cooled and crushed to obtain PA1012.
[0038] Further, on the basis of the above technical solution of the present invention, in step S1, the mass ratio of the modified halogen-free flame retardant to water is 1:4-6;
[0039] And / or, the drying condition in step S2 is drying at 100-120° C. for 4-6 hours;
[0040] And / or, in step S2, the stirring time is 10-20 min, and the stirring rate is 100-120 r / min.
[0041] Furthermore, on the basis of the above technical solution of the present invention, the setting conditions of the twin-screw extruder are: the temperature of zone 1 is 250-270°C, the temperature of zone 2 is 260-280°C, the temperature of zone 3 is 270-290°C, the temperature of zone 4 is 280-300°C, the temperature of zone 5 is 290-310°C, and the head temperature is 300-320°C; the screw speed is controlled at 220-350r / min, the conveying time of the mixture in the screw is 3-5min, and the pressure is 12-20Pa.
[0042] The present invention provides a halogen-free flame-retardant nylon composite material and a preparation method thereof, and the beneficial effects are as follows:
[0043] 1. The present invention utilizes decanediamine, one of the monomers for synthesizing PA1012, to modify 2-carboxyethylphenyl hypophosphorous acid. The amino group (-NH2) of decanediamine reacts with the carboxylic acid group (-COOH) of 2-carboxyethylphenyl hypophosphorous acid to generate an amide bond (-CONH-), and can also react with the hypophosphorous acid group (-PO(OH)H) of 2-carboxyethylphenyl hypophosphorous acid to form a phosphonate, thereby solving the problems of molecular weight reduction and poor mechanical properties caused by adding 2-carboxyethylphenyl hypophosphorous acid into PA1012, and effectively improving the flame retardancy and stability of the composite material.
[0044] 2. The reason why the present invention selects copper salt antioxidants is that when copper salt antioxidants are oxidized, the copper ions produced as a transition metal have good coordination ability and can react with polyamide molecules to form complexes, which can decompose the hydroperoxides produced by the oxidation of PA1012 into inactive substances. The hydrogen atoms in the methylene groups adjacent to nitrogen on the PA1012 molecular chain are affected by the intramolecular conjugation effect, which reduces the reaction activity and helps to slow down the free radical chain reaction, improve the thermal stability and anti-aging performance of the material, and keep the PA1012 molecular chain intact for a long time. 1+ , Cu 2+ It can continue to regenerate through redox reactions and free radical capture reactions, and always maintain high antioxidant activity during the reaction process.
[0045] 3. The present invention uses a polymer containing maleic anhydride grafts as a compatibilizer, which can effectively improve the adhesion and compatibility of the material and has good bonding with polar polymers (such as nylon, polyester, epoxy resin, etc.).
[0046] 4. The halogen-free flame-retardant nylon composite material provided by the present invention has a tensile strength of 145-170 MPa, a flexural strength of 240-280 MPa, an elongation at break of 01-0.14%, and a flame retardant grade of V0. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0048] Figure 1 The infrared spectra of 2-carboxyethylphenyl hypophosphorous acid and the modified halogen-free flame retardant provided by the present invention are shown. DETAILED DESCRIPTION
[0049] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.
[0050] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0051] According to a first aspect of the present invention, there is provided a halogen-free flame-retardant nylon composite material, comprising the following components by mass percentage:
[0052] Modified halogen-free flame retardant 10-20%, decanediamine 35-55%, dodecanedioic acid 25-45%, compatibilizer 0.1-2%, antioxidant 0.2-0.6%, lubricant 0.2-0.4% and nucleating agent 0.3-0.5%.
[0053] Specifically, the modified halogen-free flame retardant is 2-carboxyethylphenylphosphinate modified by decanediamine.
[0054] As an optional embodiment of the present invention, the preparation method of the modified halogen-free flame retardant comprises the following steps:
[0055] Decanediamine is placed in a solvent, and the mixture is stirred while cooling to obtain a mixed solution; 2-carboxyethylphenylphosphorous acid is added to the mixed solution, and the mixture is heated and stirred, and after cooling, the mixture is filtered, and the obtained filter cake is washed to obtain a modified halogen-free flame retardant.
[0056] Specifically, the present invention utilizes decanediamine, one of the monomers for synthesizing PA1012, to modify 2-carboxyethylphenyl hypophosphorous acid. The amino group (-NH2) of decanediamine reacts with the carboxylic acid group (-COOH) of 2-carboxyethylphenyl hypophosphorous acid to generate an amide bond (-CONH-), and can also react with the hypophosphorous acid group (-PO(OH)H) of 2-carboxyethylphenyl hypophosphorous acid to form a phosphonate, thereby solving the problems of reduced molecular weight and poor mechanical properties caused by adding 2-carboxyethylphenyl hypophosphorous acid into PA1012, and effectively improving the flame retardancy and stability of the composite material.
[0057] like Figure 1 As shown in the figure, it is the infrared spectra of 2-carboxyethylphenylphosphite (CEPPA) and modified halogen-free flame retardant. From the curve of 2-carboxyethylphenylphosphite, we can see that 3042cm -1 It is the stretching vibration peak of -OH in the carboxyl group (-COOH). The characteristic peak of C=O in -COOH appears at 1733cm -1 , 1150cm -1 and 805cm -1 The characteristic absorption peak at is caused by P=O.
[0058] V in -NH2 in the modified halogen-free flame retardant curve N-H The characteristic absorption peak caused by -1 and 1680cm -1 The characteristic peak caused by P=O in phosphonate appears at 1235cm -1 The above figure shows that the hypophosphorous acid group of 2-carboxyethylphenyl hypophosphorous acid reacts with the amino group of decanediamine to form a phosphonate.
[0059] Among them, 1543cm -1 The characteristic peak of the NH bond in decanediamine appears at , indicating that the modified halogen-free flame retardant is a mixture of modified 2-carboxyethylphenylphosphorous acid and decanediamine.
[0060] As an optional embodiment of the present invention, the solvent is a polar solvent;
[0061] Preferably, the polar solvent includes one or more of water, ethanol, methanol, dimethyl sulfoxide or acetonitrile.
[0062] Specifically, the reason why the present invention selects a polar solvent as the solvent is that both decanediamine and 2-carboxyethylphenylphosphorous acid have good solubility in polar solvents. Further, after decanediamine and 2-carboxyethylphenylphosphorous acid react, the generated amide bonds and phosphonates are also in polar solvents. Therefore, the modified halogen-free flame retardant obtained in step S2 of the present invention is a mixture of modified 2-carboxyethylphenylphosphorous acid and decanediamine. However, since decanediamine is one of the monomers for synthesizing PA1012, the mixture of modified 2-carboxyethylphenylphosphorous acid and decanediamine can be directly used to prepare a halogen-free flame retardant nylon composite material without introducing other impurities.
[0063] More preferably, water is selected as the solvent in the present invention.
[0064] Wherein, ethanol is an ethanol solution with a concentration of 70%, and methanol is a methanol solution with a concentration of 70%.
[0065] As an optional embodiment of the present invention, the conditions for cooling and stirring include:
[0066] The temperature is 0-5°C (such as 1°C, 2°C, 3°C, 4°C, etc.), the stirring rate is 130-180r / min (such as 140r / min, 150r / min, 160r / min, 170r / min, etc.), and the stirring time is 30-60min (such as 40min, 50min, etc.).
[0067] As an optional embodiment of the present invention, the conditions for heating and stirring include:
[0068] The temperature is 60-90°C (such as 65°C, 70°C, 75°C, 80°C, etc.), the stirring rate is 130-180r / min (such as 140r / min, 150r / min, 160r / min, 170r / min, etc.), and the stirring time is 6-8h (such as 6.5h, 7h, 7.5h, etc.;
[0069] And / or, the washing comprises:
[0070] The detergent is a polar solvent;
[0071] Preferably, the polar solvent includes one or more of water, ethanol, methanol, dimethyl sulfoxide or acetonitrile;
[0072] And / or, the detergent is the same as the solvent.
[0073] Specifically, the reason for selecting the detergent and solvent to be the same is to prevent the introduction of other impurities.
[0074] As an optional embodiment of the present invention, the mass ratio of the decanediamine to the solvent is 1:2-3 (such as 1:2, 1:2.5, 1:2.8, etc.);
[0075] The mass ratio of the decanediamine to the 2-carboxyethylphenylphosphorous acid is 2-3:1 (such as 2.2:1, 2.5:1, 2.8:1, etc.).
[0076] As an optional embodiment of the present invention, the compatibilizer is a polymer containing maleic anhydride grafts;
[0077] Preferably, the polymer containing maleic anhydride grafts includes one or more of maleic anhydride grafted polyolefins, maleic anhydride grafted polyesters, maleic anhydride grafted polyethers, and maleic anhydride grafted polyamides;
[0078] Specifically, the present invention adopts a polymer containing maleic anhydride grafts as a compatibilizer. The polymer containing maleic anhydride grafts is usually composed of a main chain and multiple side chains. This structure enables the grafted polymer to act as a bridge between different polymers, improve the interfacial compatibility between two or more polymers, and reduce phase separation at the interface; and the polymer containing maleic anhydride grafts contains polar carboxyl (-COOH) functional groups, which enables it to form hydrogen bonds or other interactions with polar polymers (such as nylon, polyester, epoxy resin, etc.), thereby improving the adhesion and compatibility of the material.
[0079] And / or, the antioxidant is a copper salt antioxidant;
[0080] Preferably, the copper salt antioxidant includes one or more of styrene copper maleate, copper naphthenate, triphenylphosphine copper, copper linoleate, and copper stearate;
[0081] Specifically, the reason why the present invention selects copper salt antioxidants is that when copper salt antioxidants are oxidized, the copper ions produced as a transition metal have good coordination ability and can react with PA1012 molecules to form complexes, which can decompose the hydroperoxides produced by the oxidation of PA1012 into inactive substances. The hydrogen atoms in the methylene groups adjacent to nitrogen on the PA1012 molecular chain are affected by the intramolecular conjugation effect, which reduces the reaction activity and helps to slow down the free radical chain reaction, improve the thermal stability and anti-aging performance of the material, and keep the PA1012 molecular chain intact for a long time. 1+ , Cu 2+ It can continue to regenerate through redox reactions and free radical capture reactions, and always maintain high antioxidant activity during the reaction process.
[0082] And / or, the lubricant is one or more of paraffin wax, polyethylene wax, polypropylene wax, polysiloxane, and silicone powder;
[0083] And / or, the nucleating agent is a sodium salt of a long carbon chain linear saturated carboxylic acid or a calcium salt of a long carbon chain linear saturated carboxylic acid;
[0084] Preferably, the long carbon chain linear saturated carboxylic acid sodium salt includes one or more of sodium laurate, sodium stearate, sodium oleate, and sodium myristic acid;
[0085] Preferably, the long carbon chain linear saturated carboxylic acid calcium salt includes one or more of TMN-102, calcium stearate, and calcium montanate.
[0086] According to a second aspect of the present invention, there is provided a method for preparing the halogen-free flame-retardant nylon composite material as described above, comprising the following steps:
[0087] S1: placing the modified halogen-free flame retardant, decanediamine and dodecanedioic acid in water, adjusting the pH value, and then transferring to a reactor for heating reaction to obtain PA1012;
[0088] S2: Dry PA1012, compatibilizer, antioxidant, lubricant and nucleating agent, and mix them evenly in a stirrer;
[0089] S3: The uniformly mixed materials are melt-blended in a twin-screw extruder and extruded into granules.
[0090] As an optional implementation of the present invention, step S1 specifically includes the following steps:
[0091] S11: placing the modified halogen-free flame retardant, decanediamine and dodecanedioic acid in water, adjusting the pH value to 7.3-7.5, transferring to a reactor, and heating the reactor for 2-3 hours at a reactor temperature of 210-250°C (such as 220°C, 230°C, 240°C, etc.), a stirring rate of 100-120r / min (such as 105r / min, 110r / min, 115r / min, etc.), and a pressure in the reactor of 2.4-2.6MPa;
[0092] S12: After the heating reaction is completed, the temperature is raised to 260-270°C (such as 262°C, 265°C, 268°C, etc.), and exhaust and pressure reduction are started;
[0093] Preferably, the depressurization rate is 0.001-0.015 MPa / s (such as 0.005 MPa / s, 0.008 MPa / s, 0.012 MPa / s, etc.), and the depressurization time is 40-50 min;
[0094] S13: After the pressure reduction is completed, the vacuum pump is further started to maintain the negative pressure in the reactor at 0.98-0.95 MPa for 1-2 hours; finally, nitrogen is filled in to break the vacuum, and the reactor is cooled and crushed to obtain PA1012.
[0095] As an optional embodiment of the present invention, in step S1, the mass ratio of the modified halogen-free flame retardant to water is 1:4-6 (such as 1:4, 1:5, 1:6, etc.);
[0096] And / or, in step S2, the drying condition is drying at 100-120° C. (such as 105° C., 110° C., 115° C., etc.) for 4-6 h (such as 4.5 h, 5 h, 5.5 h, etc.);
[0097] And / or, in step S2, the stirring time is 10-20 min (such as 12 min, 14 min, 16 min, 18 min, etc.), and the stirring rate is 100-120 r / min (such as 105 r / min, 110 r / min, 115 r / min, etc.).
[0098] As an optional embodiment of the present invention, the setting conditions of the twin-screw extruder are: the temperature of zone 1 is 250-270°C (for example, 255°C, 260°C, 265°C, etc.), the temperature of zone 2 is 260-280°C (for example, 265°C, 270°C, 275°C, etc.), the temperature of zone 3 is 270-290°C (for example, 275°C, 280°C, 285°C, etc.), the temperature of zone 4 is 280-300°C (for example, 285°C, 290°C, 295°C, etc.), the temperature of zone 5 is 290-310°C (for example, 295°C, 300°C, 305°C, etc.) etc.), the head temperature is 300-320℃ (such as 305℃, 310℃, 315℃, etc.); the screw speed is controlled at 220-350r / min (such as 240r / min, 260r / min, 280r / min, 300r / min, 320r / min, 340r / min, etc.), the mixture conveying time in the screw is 3-5min (such as 3.5min, 4min, 4.5min, etc.), and the pressure is 12-20Pa (such as 14Pa, 16Pa, 18Pa, etc.).
[0099] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.
[0100] The raw materials used in the present invention are all commercially available materials.
[0101] Example 1
[0102] Preparation of modified halogen-free flame retardant:
[0103] 40 kg of decanediamine was placed in 80 kg of water, and the mixture was stirred while cooling at a temperature of 0° C., a stirring rate of 130 r / min, and a stirring time of 60 min to obtain a mixed solution; 20 kg of 2-carboxyethylphenylphosphorous acid was added to the mixed solution, and the mixture was heated and stirred at a temperature of 90° C., a stirring rate of 130 r / min, and a stirring time of 8 h. After cooling, the mixture was filtered, and the obtained filter cake was washed with water to obtain a modified halogen-free flame retardant.
[0104] Preparation of halogen-free flame-retardant nylon composite materials:
[0105] S1: 10 kg of modified halogen-free flame retardant, 40 kg of decanediamine and 30 kg of dodecanedioic acid were placed in 50 kg of water, the pH value was adjusted to 7.3, and the mixture was transferred to a reactor. The reaction was heated for 3 hours at a reactor temperature of 210 ° C, a stirring rate of 100 r / min, and a pressure of 2.4 MPa.
[0106] After the heating reaction is completed, the temperature is raised to 260°C and the exhaust and pressure reduction are started;
[0107] Preferably, the pressure reduction rate is 0.001 MPa / s and the pressure reduction time is 50 min;
[0108] After the pressure reduction was completed, the vacuum pump was further started to maintain the negative pressure in the reactor at 0.98 MPa for 2 h; finally, nitrogen was filled in to break the vacuum, and the reactor was cooled and crushed to obtain PA1012.
[0109] S2: The obtained PA1012, 1 kg of maleic anhydride grafted polyolefin, 0.5 kg of styrene copper maleate, 0.3 kg of paraffin wax and 0.4 kg of sodium laurate were dried at 100°C for 4 h, and mixed evenly in a stirrer for 20 min at a stirring rate of 120 r / min;
[0110] S3: The uniformly mixed materials are melt-blended in a twin-screw extruder, and the setting conditions of the twin-screw extruder are: zone 1 temperature 250°C, zone 2 temperature 260°C, zone 3 temperature 270°C, zone 4 temperature 280°C, zone 5 temperature 290°C, and head temperature 300°C; the screw speed is controlled at 220r / min, the mixed material is conveyed in the screw for 5min, and the pressure is 12Pa; after melt-blending extrusion, water cooling, air drying, pelletizing, and drying, a halogen-free flame-retardant nylon composite material is obtained.
[0111] The performance data of the halogen-free flame-retardant nylon composite material prepared in this example are shown in Table 1.
[0112] Example 2
[0113] Preparation of modified halogen-free flame retardant:
[0114] 40 kg of decanediamine was placed in 80 kg of ethanol, and the mixture was stirred while cooling at 2° C., at a stirring rate of 150 r / min, and for 40 min to obtain a mixed solution; 20 kg of 2-carboxyethylphenylphosphorous acid was added to the mixed solution, and the mixture was heated and stirred at 70° C., at a stirring rate of 150 r / min, and for 7 h. After cooling, the mixture was filtered, and the filter cake was washed with ethanol to obtain a modified halogen-free flame retardant.
[0115] Preparation of halogen-free flame-retardant nylon composite materials:
[0116] S1: 15 kg of modified halogen-free flame retardant, 35 kg of decanediamine and 35 kg of dodecanedioic acid were placed in 60 kg of water, the pH value was adjusted to 7.5, and the mixture was transferred to a reactor. The reaction was heated for 2.5 h at a temperature of 220 ° C, a stirring rate of 110 r / min, and a pressure of 2.5 MPa in the reactor.
[0117] After the heating reaction is completed, the temperature is raised to 265°C and the exhaust and pressure reduction are started;
[0118] Preferably, the pressure reduction rate is 0.012 MPa / s and the pressure reduction time is 40 min;
[0119] After the pressure reduction was completed, the vacuum pump was further started to maintain the negative pressure in the reactor at 0.95 MPa for 1 hour; finally, nitrogen was filled in to break the vacuum, and the reactor was cooled and crushed to obtain PA1012.
[0120] S2: The obtained PA1012, 0.5 kg of maleic anhydride grafted polyester, 0.6 kg of copper cyclohexaneate, 0.4 kg of polyethylene wax and 0.5 kg of sodium stearate were dried at 120°C for 6 h, and mixed evenly in a stirrer for 20 min at a stirring rate of 120 r / min;
[0121] S3: The uniformly mixed materials are melt-blended in a twin-screw extruder, and the setting conditions of the twin-screw extruder are: zone 1 temperature 270°C, zone 2 temperature 280°C, zone 3 temperature 290°C, zone 4 temperature 300°C, zone 5 temperature 310°C, and die head temperature 320°C; the screw speed is controlled at 350r / min, the mixed material is conveyed in the screw for 3min, and the pressure is 20Pa; after melt-blending extrusion, water cooling, air drying, pelletizing, and drying, a halogen-free flame-retardant nylon composite material is obtained.
[0122] The performance data of the halogen-free flame-retardant nylon composite material prepared in this example are shown in Table 1.
[0123] Example 3
[0124] Preparation of modified halogen-free flame retardant:
[0125] 40 kg of decanediamine was placed in 80 kg of methanol, and the mixture was stirred while cooling at a temperature of 5° C., a stirring rate of 130 r / min, and a stirring time of 60 min to obtain a mixed solution; 20 kg of 2-carboxyethylphenylphosphorous acid was added to the mixed solution, and the mixture was heated and stirred at a temperature of 90° C., a stirring rate of 130 r / min, and a stirring time of 8 h. After cooling, the mixture was filtered, and the obtained filter cake was washed with methanol to obtain a modified halogen-free flame retardant.
[0126] Preparation of halogen-free flame-retardant nylon composite materials:
[0127] S1: 20 kg of modified halogen-free flame retardant, 55 kg of decanediamine and 45 kg of dodecanedioic acid were placed in 80 kg of water, the pH value was adjusted to 7.5, and the mixture was transferred to a reactor. The reaction was carried out under the conditions of a reactor temperature of 250 ° C, a stirring rate of 120 r / min, and a pressure in the reactor of 2.6 MPa for 3 hours;
[0128] After the heating reaction is completed, the temperature is raised to 270°C and the exhaust and pressure reduction are started;
[0129] Preferably, the pressure reduction rate is 0.015 MPa / s and the pressure reduction time is 50 min;
[0130] After the pressure reduction was completed, the vacuum pump was further started to maintain the negative pressure in the reactor at 0.95 MPa for 2 h; finally, nitrogen was filled in to break the vacuum, and the reactor was cooled and crushed to obtain PA1012.
[0131] S2: The obtained PA1012, 0.5 kg of maleic anhydride grafted polyether, 0.2 kg of triphenylphosphine copper, 0.2 kg of polypropylene wax and 0.5 kg of calcium stearate were dried at 120°C for 5 h, and mixed evenly in a stirrer for 15 min at a stirring rate of 100 r / min;
[0132] S3: The uniformly mixed materials are melt-blended in a twin-screw extruder, and the setting conditions of the twin-screw extruder are: zone 1 temperature 260°C, zone 2 temperature 270°C, zone 3 temperature 280°C, zone 4 temperature 290°C, zone 5 temperature 300°C, and die head temperature 310°C; the screw speed is controlled at 300r / min, the mixed material is conveyed in the screw for 4min, and the pressure is 15Pa; after melt-blending extrusion, water cooling, air drying, pelletizing, and drying, a halogen-free flame-retardant nylon composite material is obtained.
[0133] The performance data of the halogen-free flame-retardant nylon composite material prepared in this example are shown in Table 1.
[0134] Example 4
[0135] Preparation of modified halogen-free flame retardant:
[0136] 40 kg of decanediamine was placed in 80 kg of dimethyl sulfoxide, and the mixture was stirred while cooling at a temperature of 0° C., a stirring rate of 130 r / min, and a stirring time of 60 min to obtain a mixed solution; 20 kg of 2-carboxyethylphenylphosphorous acid was added to the mixed solution, and the mixture was heated and stirred at a temperature of 90° C., a stirring rate of 130 r / min, and a stirring time of 8 h. After cooling, the mixture was filtered, and the obtained filter cake was washed with dimethyl sulfoxide to obtain a modified halogen-free flame retardant.
[0137] Preparation of halogen-free flame-retardant nylon composite materials:
[0138] S1: 17 kg of modified halogen-free flame retardant, 45 kg of decanediamine and 40 kg of dodecanedioic acid were placed in 70 kg of water, the pH value was adjusted to 7.3, and the mixture was transferred to a reactor. The reaction was heated for 2 h at a temperature of 250 ° C, a stirring rate of 100 r / min, and a pressure of 2.4 MPa in the reactor.
[0139] After the heating reaction is completed, the temperature is raised to 270°C and the exhaust and pressure reduction are started;
[0140] Preferably, the pressure reduction rate is 0.001 MPa / s and the pressure reduction time is 50 min;
[0141] After the pressure reduction was completed, the vacuum pump was further started to maintain the negative pressure in the reactor at 0.98 MPa for 1.5 h; finally, nitrogen was filled in to break the vacuum, and the reactor was cooled and crushed to obtain PA1012.
[0142] S2: The obtained PA1012, 0.1 kg of maleic anhydride grafted polyamide, 0.6 kg of copper linoleate, 0.2 kg of silicone powder and 0.3 kg of calcium montanate were dried at 100°C for 5 h, and mixed in a stirrer for 20 min at a stirring rate of 120 r / min.
[0143] S3: The uniformly mixed materials are melt-blended in a twin-screw extruder, and the setting conditions of the twin-screw extruder are: zone 1 temperature 250°C, zone 2 temperature 260°C, zone 3 temperature 270°C, zone 4 temperature 280°C, zone 5 temperature 290°C, and head temperature 300°C; the screw speed is controlled at 220r / min, the mixed material is conveyed in the screw for 5min, and the pressure is 12Pa; after melt-blending extrusion, water cooling, air drying, pelletizing, and drying, a halogen-free flame-retardant nylon composite material is obtained.
[0144] The performance data of the halogen-free flame-retardant nylon composite material prepared in this example are shown in Table 1.
[0145] Example 5
[0146] Preparation of modified halogen-free flame retardant:
[0147] 40 kg of decanediamine was placed in 80 kg of acetonitrile, and the mixture was stirred while cooling at a temperature of 0° C., a stirring rate of 130 r / min, and a stirring time of 60 min to obtain a mixed solution; 20 kg of 2-carboxyethylphenylphosphorous acid was added to the mixed solution, and the mixture was heated and stirred at a temperature of 90° C., a stirring rate of 130 r / min, and a stirring time of 8 h. After cooling, the mixture was filtered, and the obtained filter cake was washed with 22 of acetonitrile to obtain a modified halogen-free flame retardant.
[0148] Preparation of halogen-free flame-retardant nylon composite materials:
[0149] S1: 10 kg of modified halogen-free flame retardant, 35 kg of decanediamine and 35 kg of dodecanedioic acid were placed in 60 kg of water, the pH value was adjusted to 7.5, and the mixture was transferred to a reactor. The reaction was heated for 3 hours at a temperature of 230 ° C, a stirring rate of 110 r / min, and a pressure of 2.4 MPa in the reactor.
[0150] After the heating reaction is completed, the temperature is raised to 270°C and the exhaust and pressure reduction are started;
[0151] Preferably, the pressure reduction rate is 0.015 MPa / s and the pressure reduction time is 50 min;
[0152] After the pressure reduction was completed, the vacuum pump was further started to maintain the negative pressure in the reactor at 0.985 MPa for 1 hour; finally, nitrogen was filled in to break the vacuum, and the reactor was cooled and crushed to obtain PA1012.
[0153] S2: The obtained PA1012, 1.5 kg of maleic anhydride grafted polyether, 0.6 kg of copper stearate, 0.4 kg of polysiloxane and 0.5 kg of sodium myristate were dried at 120°C for 6 h, and mixed evenly in a stirrer for 20 min at a stirring rate of 120 r / min;
[0154] S3: The uniformly mixed materials are melt-blended in a twin-screw extruder, and the setting conditions of the twin-screw extruder are: zone 1 temperature 250°C, zone 2 temperature 260°C, zone 3 temperature 270°C, zone 4 temperature 280°C, zone 5 temperature 290°C, and head temperature 300°C; the screw speed is controlled at 220r / min, the mixed material is conveyed in the screw for 5min, and the pressure is 20Pa; after melt-blending extrusion, water cooling, air drying, pelletizing, and drying, a halogen-free flame-retardant nylon composite material is obtained.
[0155] The performance data of the halogen-free flame-retardant nylon composite material prepared in this example are shown in Table 1.
[0156] Comparative Example 1
[0157] In this comparative example, the halogen-free flame retardant 2-carboxyethylphenyl hypophosphorous acid is directly used to prepare the halogen-free flame retardant nylon composite material, and the remaining steps and technical parameters are the same as those in Example 1.
[0158] The performance data of the halogen-free flame-retardant nylon composite material prepared in this comparative example are shown in Table 1.
[0159] Comparative Example 2
[0160] Compared with Example 1, the antioxidant used in this comparative example is a di-p-aniline type antioxidant, which is an antioxidant that does not contain copper ions. The remaining steps and operations are the same as those in Example 1.
[0161] The performance data of the halogen-free flame-retardant nylon composite material prepared in this comparative example are shown in Table 1.
[0162] Performance Comparison
[0163] The performance testing method adopted by the present invention is as follows:
[0164] Tensile strength and elongation at break: tested according to GB / T1040 standard; specimen type is type I, specimen size (mm): 170 (length) × (20 ± 0.2) (end width) × (4 ± 0.2) (thickness), tensile speed is 50 mm / min;
[0165] Bending strength: Tested according to GB / T9341 standard; sample type: sample size (mm): (80±2)×(10±0.2)×(4±0.2), bending speed: 20mm / min;
[0166] Flame retardant performance: tested according to UL-94 standard, the sample thickness is about 1.5 mm; flame retardant level: V0>V1>V2.
[0167] The halogen-free flame-retardant nylon composite materials prepared in Examples 1-5 and Comparative Examples 1-2 were injection molded on an injection molding machine to prepare samples, and performance tests were performed, as shown in Table 1:
[0168] Table 1
[0169]
[0170] As shown in Table 1, compared with Example 1 of the present invention, since the halogen-free flame retardant 2-carboxyethylphenylphosphite is not modified in Comparative Example 1, the composite material prepared in Comparative Example 1 can continue to burn for up to 5 seconds after ignition, so it reaches V2 level in the vertical burning test, showing poor flame retardancy and causing the mechanical properties of the composite material to be reduced.
[0171] As shown in Table 1, compared with Example 1 of the present invention, since the antioxidant used in Comparative Example 2 is a di-p-aniline type antioxidant, which is an antioxidant without copper ions, the elongation at break is relatively higher than that in Example 1, indicating that the composite material prepared in Comparative Example 2 is relatively brittle, resulting in reduced tensile strength and flexural strength.
[0172] In summary, the present invention utilizes decanediamine, one of the monomers for synthesizing PA1012, to modify 2-carboxyethylphenyl hypophosphorous acid. The amino group (-NH2) of decanediamine reacts with the carboxylic acid group (-COOH) of 2-carboxyethylphenyl hypophosphorous acid to generate an amide bond (-CONH-), and can also react with the hypophosphorous acid group (-PO(OH)H) of 2-carboxyethylphenyl hypophosphorous acid to form a phosphonate, thereby solving the problems of reduced molecular weight and poor mechanical properties caused by adding 2-carboxyethylphenyl hypophosphorous acid into PA1012, and effectively improving the flame retardancy and stability of the composite material.
[0173] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A halogen-free flame-retardant nylon composite material, characterized in that: In terms of mass percentage, it includes the following components: Modified halogen-free flame retardant 10-20%, decanediamine 35-55%, dodecanedioic acid 25-45%, compatibilizer 0.1-2%, antioxidant 0.2-0.6%, lubricant 0.2-0.4% and nucleating agent 0.3-0.5%.
2. The halogen-free flame-retardant nylon composite material according to claim 1, characterized in that: The preparation method of the modified halogen-free flame retardant comprises the following steps: Decanediamine is placed in a solvent, and the mixture is stirred while cooling to obtain a mixed solution; 2-carboxyethylphenylphosphorous acid is added to the mixed solution, and the mixture is heated and stirred, and after cooling, the mixture is filtered, and the obtained filter cake is washed to obtain a modified halogen-free flame retardant.
3. The halogen-free flame-retardant nylon composite material according to claim 2, characterized in that: The solvent is a polar solvent; Preferably, the polar solvent includes one or more of water, ethanol, methanol, dimethyl sulfoxide or acetonitrile.
4. The halogen-free flame-retardant nylon composite material according to claim 2, characterized in that: The conditions for the cooling and stirring include: The temperature is 0-5°C, the stirring rate is 130-180r / min, and the stirring time is 30-60min; And / or, the conditions of heating and stirring include: The temperature is 60-90°C, the stirring rate is 130-180r / min, and the stirring time is 6-8h; And / or, the washing comprises: The detergent is a polar solvent; Preferably, the polar solvent includes one or more of water, ethanol, methanol, dimethyl sulfoxide or acetonitrile; And / or, the detergent is the same as the solvent.
5. The halogen-free flame-retardant nylon composite material according to claim 2, characterized in that: The mass ratio of the decanediamine to the solvent is 1:2-3; The mass ratio of the decanediamine to the 2-carboxyethylphenylphosphorous acid is 2-3:
1.
6. The halogen-free flame-retardant nylon composite material according to claim 1, characterized in that: The compatibilizer is a polymer containing maleic anhydride grafts; Preferably, the polymer containing maleic anhydride grafts includes one or more of maleic anhydride grafted polyolefins, maleic anhydride grafted polyesters, maleic anhydride grafted polyethers, and maleic anhydride grafted polyamides; And / or, the antioxidant is a copper salt antioxidant; Preferably, the copper salt antioxidant includes one or more of styrene copper maleate, copper naphthenate, triphenylphosphine copper, copper linoleate, and copper stearate; And / or, the lubricant is one or more of paraffin wax, polyethylene wax, polypropylene wax, polysiloxane, and silicone powder; And / or, the nucleating agent is a sodium salt of a long carbon chain linear saturated carboxylic acid or a calcium salt of a long carbon chain linear saturated carboxylic acid; Preferably, the long carbon chain linear saturated carboxylic acid sodium salt includes one or more of sodium laurate, sodium stearate, sodium oleate, and sodium myristic acid; Preferably, the long carbon chain linear saturated carboxylic acid calcium salt includes one or more of TMN-102, calcium stearate, and calcium montanate.
7. A method for preparing the halogen-free flame-retardant nylon composite material according to any one of claims 1 to 6, characterized in that: The steps include: S1: placing the modified halogen-free flame retardant, decanediamine and dodecanedioic acid in water, adjusting the pH value, and then transferring to a reactor for heating reaction to obtain PA1012; S2: Dry PA1012, compatibilizer, antioxidant, lubricant and nucleating agent, and mix them evenly in a stirrer; S3: The uniformly mixed materials are melt-blended in a twin-screw extruder and extruded into granules.
8. The method for preparing the halogen-free flame-retardant nylon composite material according to claim 7, characterized in that: Step S1 specifically includes the following steps: S11: placing the modified halogen-free flame retardant, decanediamine and dodecanedioic acid in water, adjusting the pH value to 7.3-7.5, transferring to a reactor, and heating the reactor for 2-3 hours at a reactor temperature of 210-250° C., a stirring rate of 100-120 r / min, and a reactor pressure of 2.4-2.6 MPa; S12: After the heating reaction is completed, the temperature is raised to 260-270°C, and exhaust and pressure reduction are started; Preferably, the pressure reduction rate is 0.001-0.015 MPa / s, and the pressure reduction time is 40-50 min; S13: After the pressure reduction is completed, the vacuum pump is further started to maintain the negative pressure in the reactor at 0.98-0.95 MPa for 1-2 hours; finally, nitrogen is filled in to break the vacuum, and the reactor is cooled and crushed to obtain PA1012.
9. The method for preparing the halogen-free flame-retardant nylon composite material according to claim 7, characterized in that: In step S1, the mass ratio of the modified halogen-free flame retardant to water is 1:4-6; And / or, the drying condition in step S2 is drying at 100-120° C. for 4-6 hours; And / or, in step S2, the stirring time is 10-20 min, and the stirring rate is 100-120 r / min.
10. The method for preparing the halogen-free flame-retardant nylon composite material according to claim 7, characterized in that: In step S3, the setting conditions of the twin-screw extruder are: zone 1 temperature 250-270°C, zone 2 temperature 260-280°C, zone 3 temperature 270-290°C, zone 4 temperature 280-300°C, zone 5 temperature 290-310°C, and head temperature 300-320°C; the screw speed is controlled at 220-350r / min, the mixed material is conveyed in the screw for 3-5min, and the pressure is 12-20Pa.
Citation Information
Patent Citations
Halogen-free flame-retardation nylon 6 montmorillonite nanocomposite and preparation method thereof
CN104211955A
In-situ-polymerized halogen-free flame-retardant nylon 6 / attapulgite nano composite material and preparation method thereof
CN104448299A
Permanent-flame-retardant nylon 6 material and preparation method therefor
CN105153414A
Flame-retardant nylon 66 copolymer material and preparation method therefor
CN105153415A
Halogen-free flame-retardant nylon composite material as well as preparation method and application thereof
CN110684344A
Cited By
Nano film-coated flame-retardant nylon filament and preparation method thereof
CN120273054A