Spraying high-adhesion rotational molding polyethylene material and preparation method thereof

By adding fillers and compatibilizers to polyethylene materials, controlling particle size distribution and processing temperature, the adhesion problem caused by low surface tension of polyethylene materials is solved, high adhesion and excellent mechanical properties are achieved, and the process is simplified. Reduced costs.

CN118978759APending Publication Date: 2024-11-19SHANGHAI LANGDOW NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411275341.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the prior art, the surface tension of the polyethylene material is low, resulting in poor adhesion of spraying or ink, and pretreatment methods such as flame treatment have insufficient stability and operability, making it difficult to achieve good adhesion gain.

Method used

Sprayed high adhesion rotomolded polyethylene materials, the formula includes polyethylene, fillers, compatibilizers and antioxidants. Through the combination of low-density polyethylene, talc, PE-G-MAH and other components, the particle size distribution is controlled and Processing temperature, improves the surface tension and adhesion of the material, and is formed using a twin-screw extruder and a rotomolding machine.

Benefits of technology

It significantly improves the adhesion of the material, enhances the mechanical properties, simplifies the process route, reduces the preparation cost, and achieves a stable adhesion gain effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978759A_ABST
    Figure CN118978759A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and discloses a spray-coating high-adhesion rotational molding polyethylene material which comprises the following components in percentage by mass: 60-90% of polyethylene, 10-20% of filler, 5-10% of compatilizer and 5-10% of antioxidant. 5-30% of a filler; 5-15% of a compatilizer; and 0.2-5% of an antioxidant. According to the invention, all the component materials are prepared according to the mass percent, and the polyethylene molded product is prepared by the corresponding preparation method, so that the surface tension of the polyethylene molded product can be obviously improved, the printing or spraying adhesive force of the polyethylene molded product is further improved, and meanwhile, the prepared compound also has excellent mechanical properties and is suitable for industrial production. The adhesive is high in tensile strength, bending strength and impact strength, simple in process manufacturing route, free of complex processing equipment, easy to realize product industrialization, low in preparation cost, stable in application method, simple to operate and good in adhesive force gain effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and specifically relates to a spray-coated high-adhesion roto-molded polyethylene material and a preparation method thereof. Background Art

[0002] Polyethylene is a thermoplastic resin obtained by polymerization of ethylene monomer. In industry, it also includes copolymers of ethylene and a small amount of α-olefins. Polyethylene is odorless, non-toxic, feels like wax, has excellent low-temperature resistance, and good chemical stability. Because the polymer molecules are connected by carbon-carbon single bonds, they can withstand the corrosion of most acids and alkalis, are insoluble in general solvents at room temperature, have low water absorption, and have excellent electrical insulation. It is mainly used to manufacture films, packaging materials, containers, pipes, monofilaments, wires and cables, daily necessities, etc., and can be used as high-frequency insulation materials for televisions, radars, etc.

[0003] Polyethylene is a non-polar material with small surface free energy and low surface wet tension, generally around 30 dynes / cm. Theoretically, if the surface tension of an object is lower than 33 dynes / cm, ordinary inks or adhesives will not adhere firmly. There are also some pretreatment methods in the prior art to improve spray adhesion, such as flame treatment, corona, plasma, etc., but they do not reach a good combination in terms of the stability of the effect and application method, the simplicity of operation, the adhesion gain effect, etc., so improvements are needed. Summary of the invention

[0004] The object of the present invention is to provide a spray-coated high-adhesion roto-molded polyethylene material and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0005] In order to achieve the above object, the present invention provides the following technical solution: a spray high adhesion roto-molded polyethylene material, comprising the following components: polyethylene, filler, compatibilizer and antioxidant, the raw material formula is calculated by mass percentage:

[0006] Polyethylene: 60-90%;

[0007] Filler: 5-30%;

[0008] Compatibilizer: 5-15%;

[0009] Antioxidant: 0.2-5%.

[0010] As a preferred technical solution of the present invention, the polyethylene is selected from low-density polyethylene of model LDPE-5202, and the density range of the polyethylene material when selected needs to be controlled within 0.910-0.965 g / cm 3 , at 190°C and 2.16Kg, the melt flow rate needs to be controlled at 1-20g / 10min.

[0011] As a preferred technical solution of the present invention, the polyethylene material can include any common additives, including flame retardants, light stabilizers, pigments or the like, which are 0.4% by mass.

[0012] As a preferred technical solution of the present invention, the filler is selected from one or more of carbon black, graphite, ferroferric oxide, carbon nanotubes, metal powder, calcium oxide, calcium carbonate, talc, aluminum hydroxide and aluminum oxide.

[0013] As a preferred technical solution of the present invention, the compatibilizer is PE-G-MAH, and the density of the compatibilizer needs to be selected in the range of 0.850-0.900 g / cm 3 , materials with a melt flow rate range of 0.5-20.0 g / 10 min under the conditions of 190°C and 2.16 kg.

[0014] As a preferred technical solution of the present invention, the antioxidants are antioxidant 1010 and antioxidant 168, and the mass percentages of the two antioxidants are 0.2% and 0.4%.

[0015] In order to achieve the above another object, the present invention provides the following technical solution: a method for preparing a spray-coated high-adhesion rotomolded polyethylene material, the specific steps are as follows:

[0016] Step 1:

[0017] Prepare 89% LDPE-5202, 5% talc, 5% PE-G-MAH, 0.2% antioxidant 1010, 0.4% antioxidant 168 and 0.4% light stabilizer in parts by mass;

[0018] Step 2:

[0019] The above components are put into a high-speed mixer for thorough mixing to obtain a preparation raw material, and then the mixed raw material is put into a twin-screw extruder, and the twin-screw extruder is used for melt blending, and the processing temperature is set within 180-200° C., so as to extrude and pelletize to obtain pellets;

[0020] Step 3:

[0021] The obtained pellets are put into a plastic grinding disc mill for grinding operation, and the temperature of the grinding disc is set to ≤65°C, the rotation speed of the grinding disc is within the range of 2500-3200rpm, and then a multi-layer sieve is used for particle size screening to screen out pellets of four different particle sizes, namely, below 20 mesh, 20-50 mesh, 50-100 mesh and above 100 mesh;

[0022] Step 4:

[0023] Selecting granules with particle sizes of 20-50 mesh, 50-100 mesh and above 100 mesh and fully mixing them in a ratio of 1:6:3 to obtain a polyethylene powder material with large and small particle sizes;

[0024] Step 5:

[0025] The polyethylene powder material is placed in a rotomolding machine for rotomolding, and the rotomolding temperature is set at 230° C. and the molding cycle is set at 45 minutes to obtain a rotomolded product, i.e., a polyethylene molded product;

[0026] Step 6:

[0027] The rotomolded products are tested for dyne value, and the tested dyne value is above 38. Then they are printed with ink and after sufficient curing, the coating adhesion is tested by the coating adhesion test - cross-cut method. The test result is level 1 or level 0, and it has long-term effectiveness.

[0028] As a preferred technical solution of the present invention, the screw diameter of the twin-screw extruder described in step 2 is 35 and the aspect ratio is 36:1.

[0029] As a preferred technical solution of the present invention, the coating adhesion described in step six is ​​tested according to the cross-cut test of paint and varnish films of GB / T9286-1998.

[0030] The beneficial effects of the present invention are as follows:

[0031] The present invention configures each component material according to mass percentage, and obtains a polyethylene molded product through a corresponding preparation method, thereby being able to significantly improve the surface tension of the product, thereby improving the adhesion of the product when printed or sprayed, and the prepared composite has excellent mechanical properties, and has high tensile strength, bending strength, and impact strength, and the process production route is simple, does not require complex processing equipment, is easy to realize product industrialization, has low preparation cost, is stable in application method, is simple in operation, and has good adhesion gain effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is the material formula table of the present invention. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The embodiment of the present invention provides a spray-coated high-adhesion rotomolded polyethylene material, comprising the following components: polyethylene, filler, compatibilizer and antioxidant, and the raw material formula is calculated by mass percentage as follows:

[0035] Polyethylene: 60-90%;

[0036] Filler: 5-30%;

[0037] Compatibilizer: 5-15%;

[0038] Antioxidant: 0.2-5%.

[0039] On the one hand, the present invention adopts raw materials with low crystallinity when selecting polyethylene materials, thereby effectively reducing the surface tension of the product; on the other hand, fillers and compatibilizers are added as polar components for blending to improve its wettability and adhesion; on the other hand, the polyethylene modified material is ground and the powder particle size distribution is controlled (large and small particle size compounding) to ensure the density of the molded product. The present invention improves the surface tension of the polyethylene molded product from these three aspects, thereby achieving a better surface spraying or printing adhesion effect.

[0040] Among them, polyethylene uses low-density polyethylene of model LDPE-5202, and the density range of polyethylene material needs to be controlled within 0.910-0.965g / cm 3 , at 190°C and 2.16Kg, the melt flow rate needs to be controlled at 1-20g / 10min.

[0041] Density: 0.910-0.965g / cm 3 , polyethylene materials with a melt flow rate (190°C, 2.16Kg) in the range of 1-20g / 10min can be used. In addition to LDPE-5202, LDPE-5203 and LDPE-0701 can also be used.

[0042] The polyethylene material can include any common additives, including flame retardants, light stabilizers, pigments or the like, which is 0.4% by mass.

[0043] By adding additives to polyethylene materials, the physical properties of polyethylene can be effectively improved, thereby further improving the performance of polyethylene molded products.

[0044] The filler is selected from one or more of carbon black, graphite, ferroferric oxide, carbon nanotubes, metal powder, calcium oxide, calcium carbonate, talcum powder, aluminum hydroxide and aluminum oxide.

[0045] The selection of fillers depends on the specific production conditions. A variety of fillers are available, which improves the flexibility and convenience of material matching.

[0046] Among them, the compatibilizer is PE-G-MAH. When selecting the compatibilizer, it is necessary to select a material with a density range of 0.850-0.900g / cm3 and a melt flow rate range of 0.5-20.0g / 10min under the conditions of 190°C and 2.16Kg.

[0047] The compatibilizer can be any brand and model commonly used in the market, and can be used directly after purchasing it from the manufacturer.

[0048] The antioxidants selected are antioxidant 1010 and antioxidant 168, and the mass percentages of the two antioxidants are 0.2% and 0.4%.

[0049] Antioxidant 1010 and Antioxidant 168 are both commercially available products and can be directly purchased on the market.

[0050] like Figure 1 As shown, the embodiment of the present invention provides a method for preparing a spray-coated high-adhesion rotomolded polyethylene material, and the specific steps are as follows:

[0051] Step 1:

[0052] Prepare 89% LDPE-5202, 5% talc, 5% PE-G-MAH, 0.2% antioxidant 1010, 0.4% antioxidant 168 and 0.4% light stabilizer in parts by mass;

[0053] Step 2:

[0054] The above components are put into a high-speed mixer for thorough mixing to obtain a preparation raw material, and then the mixed raw material is put into a twin-screw extruder, and the twin-screw extruder is used for melt blending, and the processing temperature is set within 180-200° C., so as to extrude and pelletize to obtain pellets;

[0055] Step 3:

[0056] The obtained pellets are put into a plastic grinding disc mill for grinding operation, and the temperature of the grinding disc is set to ≤65°C, the rotation speed of the grinding disc is within the range of 2500-3200rpm, and then a multi-layer sieve is used for particle size screening to screen out pellets of four different particle sizes, namely, below 20 mesh, 20-50 mesh, 50-100 mesh and above 100 mesh;

[0057] Step 4:

[0058] Selecting granules with particle sizes of 20-50 mesh, 50-100 mesh and above 100 mesh and fully mixing them in a ratio of 1:6:3 to obtain a polyethylene powder material with large and small particle sizes;

[0059] Step 5:

[0060] The polyethylene powder material is placed in a rotomolding machine for rotomolding, and the rotomolding temperature is set at 230° C. and the molding cycle is set at 45 minutes to obtain a rotomolded product, i.e., a polyethylene molded product;

[0061] Step 6:

[0062] The rotomolded products are tested for dyne value, and the tested dyne value is above 38. Then they are printed with ink and after sufficient curing, the coating adhesion is tested by the coating adhesion test - cross-cut method. The test result is level 1 or level 0, and it has long-term effectiveness.

[0063] The invention puts raw materials of various components into a high-speed mixer for mixing, melts and blends them through a twin-screw extruder, extrude pellets, grinds and sieves the pellets through a plastic grinder and a multi-layer sieve to obtain raw materials with different particle sizes, mixes the pellets with different particle sizes, and performs rotational molding by a rotational molding machine to obtain a rotational molded polyethylene molded product with high adhesion. The process route is relatively simple, no complex equipment is needed, industrialization is easy to realize, the preparation cost is low, the application method is stable, and the operation is simple.

[0064] Among them, the screw diameter of the twin-screw extruder in step 2 is 35, and the aspect ratio is 36:1.

[0065] Strictly adopting an extruder with a screw diameter of 35 and an aspect ratio of 36:1 can obtain the required particle size raw materials and improve the efficiency of obtaining particle size raw materials.

[0066] The coating adhesion in step six is ​​tested according to the cross-cut test of paint and varnish films in GB / T 9286-1998.

[0067] Through these two test methods, the adhesion of polyethylene moldings can be effectively tested, thereby improving the persuasiveness and reliability of the test results.

[0068] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0069] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A spray-coated high-adhesion rotomolded polyethylene material, characterized in that: The composition includes the following ingredients: polyethylene, filler, compatibilizer and antioxidant. The raw material formula is calculated by mass percentage as follows: Polyethylene: 60-90%; Filler: 5-30%; Compatibilizer: 5-15%; Antioxidant: 0.2-5%.

2. The high-adhesion sprayable rotomolded polyethylene material according to claim 1, characterized in that: The polyethylene is selected from low-density polyethylene of model LDPE-5202, and the density range of the polyethylene material when selected needs to be controlled within 0.910-0.965 g / cm 3 , at 190°C and 2.16Kg, the melt flow rate needs to be controlled at 1-20g / 10min.

3. The spray-coated high-adhesion rotomolded polyethylene material according to claim 1, characterized in that: The polyethylene material can include any common additives including flame retardants, light stabilizers, pigments or the like, which is 0.4% by mass.

4. The spray-coated high-adhesion rotomolded polyethylene material according to claim 1, characterized in that: The filler is selected from one or more of carbon black, graphite, ferroferric oxide, carbon nanotubes, metal powder, calcium oxide, calcium carbonate, talcum powder, aluminum hydroxide and aluminum oxide.

5. The spray-coated high-adhesion rotomolded polyethylene material according to claim 1, characterized in that: The compatibilizer is PE-G-MAH. The compatibilizer needs to be selected from materials with a density range of 0.850-0.900 g / cm 3 and a melt flow rate range of 0.5-20.0 g / 10 min under the conditions of 190° C. and 2.16 kg.

6. The high-adhesion sprayable rotomolded polyethylene material according to claim 1, characterized in that: The antioxidants selected are antioxidant 1010 and antioxidant 168, and the mass percentages of the two antioxidants are 0.2% and 0.4%.

7. A method for preparing a spray-coated high-adhesion rotomolded polyethylene material according to any one of claims 1 to 6, characterized in that: The specific steps are as follows: Step 1: Prepare 89% LDPE-5202, 5% talc, 5% PE-G-MAH, 0.2% antioxidant 1010, 0.4% antioxidant 168 and 0.4% light stabilizer in parts by mass; Step 2: The above components are put into a high-speed mixer for thorough mixing to obtain a preparation raw material, and then the mixed raw material is put into a twin-screw extruder, and the twin-screw extruder is used for melt blending, and the processing temperature is set within 180-200° C., so as to extrude and pelletize to obtain pellets; Step 3: The obtained pellets are put into a plastic grinding disc mill for grinding operation, and the temperature of the grinding disc is set to ≤65°C, the rotation speed of the grinding disc is within the range of 2500-3200rpm, and then a multi-layer sieve is used for particle size screening to screen out pellets of four different particle sizes, namely, below 20 mesh, 20-50 mesh, 50-100 mesh and above 100 mesh; Step 4: Selecting granules with particle sizes of 20-50 mesh, 50-100 mesh and above 100 mesh and fully mixing them in a ratio of 1:6:3 to obtain a polyethylene powder material with large and small particle sizes; Step 5: The polyethylene powder material is placed in a rotomolding machine for rotomolding, and the rotomolding temperature is set at 230° C. and the molding cycle is set at 45 minutes to obtain a rotomolded product, i.e., a polyethylene molded product; Step 6: The rotomolded products are tested for dyne value, and the tested dyne value is above 38. Then they are printed with ink and after sufficient curing, the coating adhesion is tested by the coating adhesion test - cross-cut method. The test result is level 1 or level 0, and it has long-term effectiveness.

8. The method for preparing a spray-coated high-adhesion rotomolded polyethylene material according to claim 7, characterized in that: The twin-screw extruder described in step 2 has a screw diameter of 35 and an aspect ratio of 36:

1.

9. The method for preparing a spray-coated high-adhesion rotomolded polyethylene material according to claim 7, characterized in that: The coating adhesion described in step 6 is tested according to the cross-cut test for paint and varnish films of GB / T 9286-1998.