By adding concave and convex rod soil to 30Cr2Ni4MoV steel and adopting a specific heat treatment process, the problem of large differences in grain size and internal and external grain size in the prior art is solved, and the performance and flaw detection sensitivity of the low-pressure rotor are improved.
Patent Information
- Application Number
- CN202410963950.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-19
AI Technical Summary
The existing 30Cr2Ni4MoV steel has larger grains during the preparation process, and the internal and external grain sizes vary greatly after forging, resulting in poor performance of low-voltage rotors.
By adding a small amount of concave and convex rod soil to the formula of 30Cr2Ni4MoV steel and using specific heat treatment processes, including superheat treatment, casting, postforging heat treatment, quenching and tempering, the total weight of carbon, chromium, nickel, molybdenum, and vanadium is controlled to concave and convex weight by using specific heat treatment processes, including superheat treatment, casting, postforging heat treatment, quenching and tempering. The weight of the rod soil is 46 times to 49 times to reduce the difference in grain size and internal and external grain size.
It effectively reduces the grain size of 30Cr2Ni4MoV steel, improves the grain size level, enhances the flaw detection sensitivity, reduces the difference in internal and external grain sizes, and improves performance.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of alloy steel, and in particular to a 30Cr2Ni4MoV steel, a preparation method and an application thereof. Background Art
[0002] Low-pressure rotors are generally used in aircraft engines and nuclear power units. In aircraft engines, low-pressure rotors usually refer to the combination of low-pressure compressors and low-pressure turbines, which together constitute one of the core components of the engine.
[0003] The low-pressure rotor is generally made of 30Cr2Ni4MoV steel, but the 30Cr2Ni4MoV steel prepared by the prior art has larger grains and a large difference in grain size inside and outside after forging, resulting in poor performance of the prepared low-pressure rotor. Summary of the invention
[0004] In order to solve at least one of the above technical problems, a 30Cr2Ni4MoV steel with smaller grains and smaller difference in internal and external grain sizes after forging is developed. The present application provides a 30Cr2Ni4MoV steel, a preparation method and an application.
[0005] On the one hand, the present application provides a 30Cr2Ni4MoV steel, which is prepared from the following components by weight percentage:
[0006] Carbon 0.28-0.35wt%;
[0007] Chromium 1.45-1.75wt%;
[0008] Nickel 1.4-1.8wt%;
[0009] Molybdenum 0.2-0.3wt%;
[0010] Vanadium 0.1-0.2wt%;
[0011] Attapulgite 0.05-0.1wt%;
[0012] Iron balance.
[0013] Preferably, the total weight of the carbon, chromium, nickel, molybdenum and vanadium is 46 to 49 times the weight of attapulgite.
[0014] Preferably, the particle size of the attapulgite is 0.2 to 1 μm.
[0015] In a second aspect, the present application provides a method for preparing the above-mentioned 30Cr2Ni4MoV steel, comprising the following steps:
[0016] S1. Take the formulated amounts of chromium, nickel, molybdenum, vanadium and iron respectively, heat them until they are melted, add carbon powder and attapulgite, and mix them evenly;
[0017] S2, heating to above 1500℃ for overheating treatment;
[0018] S3. Cool to 1500°C or below and cast to obtain 30Cr2Ni4MoV steel.
[0019] In a third aspect, the present application provides a post-forging heat treatment method for the above-mentioned 30Cr2Ni4MoV steel, comprising the following steps:
[0020] S1 one-step normalizing
[0021] Slowly increase the temperature to 850-900℃ at a temperature rise of 20-25℃ / h, then quickly increase the temperature to 950-1000℃ at a temperature rise of 45-50℃ / h, keep warm for 3-5h, slowly decrease the temperature to 850-900℃ at a temperature drop of 5-10℃, and air cool to 200-250℃ and keep warm for 3-5h;
[0022] S2 secondary normalizing
[0023] Slowly increase the temperature to 750-800℃ at a rate of 10-15℃ / h, keep it warm for 3-5h, slowly decrease the temperature to 650-700℃ at a rate of 5-10℃, and air cool to 150-200℃ and keep it warm for 2-3h;
[0024] S3 one-time tempering
[0025] Slowly increase the temperature to 550-600℃ at a rate of 20-25℃ / h, keep warm for 2-3h and air cool;
[0026] S4 Quenching
[0027] Heat to 820-850℃, immerse in water and cool quickly;
[0028] S5 secondary tempering
[0029] Heat to 600-620℃ and immerse in water to cool quickly.
[0030] In a fourth aspect, the present application provides application of the above-mentioned 30Cr2Ni4MoV steel in the field of low-pressure rotors.
[0031] In summary, after adding a small amount of attapulgite, the present invention can reduce the grain size of 30Cr2Ni4MoV steel, improve the grain size grade of 30Cr2Ni4MoV steel, and reduce the difference in grain size between the inside and outside of 30Cr2Ni4MoV steel; the flaw detection sensitivity is higher.
[0032] In the technical solution of the present invention, when the total weight of carbon, chromium, nickel, molybdenum and vanadium is in the range of 46 to 49 times the weight of attapulgite, the prepared 30Cr2Ni4MoV steel has smaller grains, smaller difference in grain size between the inside and the outside, and higher flaw detection sensitivity. DETAILED DESCRIPTION
[0033] The present application is further described in detail below with reference to the embodiments.
[0034] In the following examples of the present application, unless otherwise specified, the main components involved were purchased from commercially available products. Specific embodiments
[0036] Example 1
[0037] This embodiment is used to prepare a 30Cr2Ni4MoV steel, which is prepared from the following components in percentage by weight:
[0038] Carbon: 0.28wt%; Chromium: 1.45wt%; Nickel: 1.6wt%; Molybdenum: 0.2wt%; Vanadium: 0.2wt%; Attapulgite: 0.05wt%; Iron: the balance. The total weight of carbon, chromium, nickel, molybdenum and vanadium is 75 times the weight of the Attapulgite.
[0039] The preparation method of 30Cr2Ni4MoV steel in this embodiment is as follows:
[0040] Take the formulated amounts of chromium, nickel, molybdenum, vanadium and iron respectively, heat them until they are melted, add carbon powder and attapulgite, and mix them evenly; heat them to above 1500° C. for overheat treatment; cool them to 1500° C. or below for casting, and obtain 30Cr2Ni4MoV steel.
[0041] The post-forging heat treatment method of 30Cr2Ni4MoV steel in this embodiment is as follows:
[0042] Slowly increase the temperature to 850-900℃ at a temperature rise of 20-25℃ / h, then quickly increase the temperature to 950-1000℃ at a temperature rise of 45-50℃ / h, keep warm for 3-5h, slowly decrease the temperature to 850-900℃ at a temperature drop of 5-10℃, and air cool to 200-250℃ and keep warm for 3-5h;
[0043] Slowly increase the temperature to 750-800℃ at a rate of 10-15℃ / h, keep it warm for 3-5h, slowly decrease the temperature to 650-700℃ at a rate of 5-10℃, and air cool to 150-200℃ and keep it warm for 2-3h;
[0044] Slowly increase the temperature to 550-600℃ at a rate of 20-25℃ / h, keep warm for 2-3h and air cool;
[0045] Heat to 820-850℃, immerse in water and cool quickly;
[0046] Heat to 600-620℃ and immerse in water to cool quickly.
[0047] Example 2
[0048] This embodiment is used to prepare a 30Cr2Ni4MoV steel, which is prepared from the following components in percentage by weight:
[0049] Carbon: 0.3wt%; Chromium: 1.75wt%; Nickel: 1.5wt%; Molybdenum: 0.2wt%; Vanadium: 0.2wt%; Attapulgite: 0.08wt%; Iron: the balance. The total weight of carbon, chromium, nickel, molybdenum and vanadium is 49 times the weight of Attapulgite.
[0050] The preparation method of 30Cr2Ni4MoV steel in this embodiment is as follows:
[0051] Take the formulated amounts of chromium, nickel, molybdenum, vanadium and iron respectively, heat them until they are melted, add carbon powder and attapulgite, and mix them evenly; heat them to above 1500° C. for overheat treatment; cool them to 1500° C. or below for casting, and obtain 30Cr2Ni4MoV steel.
[0052] The post-forging heat treatment method of 30Cr2Ni4MoV steel in this embodiment is as follows:
[0053] Slowly increase the temperature to 850-900℃ at a temperature rise of 20-25℃ / h, then quickly increase the temperature to 950-1000℃ at a temperature rise of 45-50℃ / h, keep warm for 3-5h, slowly decrease the temperature to 850-900℃ at a temperature drop of 5-10℃, and air cool to 200-250℃ and keep warm for 3-5h;
[0054] Slowly increase the temperature to 750-800℃ at a rate of 10-15℃ / h, keep it warm for 3-5h, slowly decrease the temperature to 650-700℃ at a rate of 5-10℃, and air cool to 150-200℃ and keep it warm for 2-3h;
[0055] Slowly increase the temperature to 550-600℃ at a rate of 20-25℃ / h, keep warm for 2-3h and air cool;
[0056] Heat to 820-850℃, immerse in water and cool quickly;
[0057] Heat to 600-620℃ and immerse in water to cool quickly.
[0058] Example 3
[0059] This embodiment is used to prepare a 30Cr2Ni4MoV steel, which is prepared from the following components in percentage by weight:
[0060] Carbon: 0.32wt%; Chromium: 1.55wt%; Nickel: 1.4wt%; Molybdenum: 0.3wt%; Vanadium: 0.1wt%; Attapulgite: 0.08wt%; Iron: the balance. The total weight of carbon, chromium, nickel, molybdenum and vanadium is 46 times the weight of Attapulgite.
[0061] The preparation method of 30Cr2Ni4MoV steel in this embodiment is as follows:
[0062] Take the formulated amounts of chromium, nickel, molybdenum, vanadium and iron respectively, heat them until they are melted, add carbon powder and attapulgite, and mix them evenly; heat them to above 1500° C. for overheat treatment; cool them to 1500° C. or below for casting, and obtain 30Cr2Ni4MoV steel.
[0063] The post-forging heat treatment method of 30Cr2Ni4MoV steel in this embodiment is as follows:
[0064] Slowly increase the temperature to 850-900℃ at a temperature rise of 20-25℃ / h, then quickly increase the temperature to 950-1000℃ at a temperature rise of 45-50℃ / h, keep warm for 3-5h, slowly decrease the temperature to 850-900℃ at a temperature drop of 5-10℃, and air cool to 200-250℃ and keep warm for 3-5h;
[0065] Slowly increase the temperature to 750-800℃ at a rate of 10-15℃ / h, keep it warm for 3-5h, slowly decrease the temperature to 650-700℃ at a rate of 5-10℃, and air cool to 150-200℃ and keep it warm for 2-3h;
[0066] Slowly increase the temperature to 550-600℃ at a rate of 20-25℃ / h, keep warm for 2-3h and air cool;
[0067] Heat to 820-850℃, immerse in water and cool quickly;
[0068] Heat to 600-620℃ and immerse in water to cool quickly.
[0069] Example 4
[0070] This embodiment is used to prepare a 30Cr2Ni4MoV steel, which is prepared from the following components in percentage by weight:
[0071] Carbon: 0.35wt%; Chromium: 1.65wt%; Nickel: 1.8wt%; Molybdenum: 0.3wt%; Vanadium: 0.1wt%; Attapulgite: 0.1wt%; Iron: the balance. The total weight of carbon, chromium, nickel, molybdenum and vanadium is 42 times the weight of Attapulgite.
[0072] The preparation method of 30Cr2Ni4MoV steel in this embodiment is as follows:
[0073] Take the formulated amounts of chromium, nickel, molybdenum, vanadium and iron respectively, heat them until they are melted, add carbon powder and attapulgite, and mix them evenly; heat them to above 1500° C. for overheat treatment; cool them to 1500° C. or below for casting, and obtain 30Cr2Ni4MoV steel.
[0074] The post-forging heat treatment method of 30Cr2Ni4MoV steel in this embodiment is as follows:
[0075] Slowly increase the temperature to 850-900℃ at a temperature rise of 20-25℃ / h, then quickly increase the temperature to 950-1000℃ at a temperature rise of 45-50℃ / h, keep warm for 3-5h, slowly decrease the temperature to 850-900℃ at a temperature drop of 5-10℃, and air cool to 200-250℃ and keep warm for 3-5h;
[0076] Slowly increase the temperature to 750-800℃ at a rate of 10-15℃ / h, keep it warm for 3-5h, slowly decrease the temperature to 650-700℃ at a rate of 5-10℃, and air cool to 150-200℃ and keep it warm for 2-3h;
[0077] Slowly increase the temperature to 550-600℃ at a rate of 20-25℃ / h, keep warm for 2-3h and air cool;
[0078] Heat to 820-850℃, immerse in water and cool quickly;
[0079] Heat to 600-620℃ and immerse in water to cool quickly.
[0080] Comparative Example 1
[0081] This comparative example is used to prepare a 30Cr2Ni4MoV steel, which is prepared from the following components in percentage by weight:
[0082] Carbon: 0.28wt%; Chromium: 1.45wt%; Nickel: 1.6wt%; Molybdenum: 0.2wt%; Vanadium: 0.2wt%; Iron: balance.
[0083] The preparation method of the comparative example 30Cr2Ni4MoV steel is as follows:
[0084] Take formulated amounts of chromium, nickel, molybdenum, vanadium and iron respectively, heat them until they are melted, add carbon powder and mix them evenly; heat them to above 1500° C. for overheat treatment; cool them to 1500° C. or below for casting to obtain 30Cr2Ni4MoV steel.
[0085] The post-forging heat treatment method of the 30Cr2Ni4MoV steel in this comparative example is as follows:
[0086] Slowly increase the temperature to 850-900℃ at a temperature rise of 20-25℃ / h, then quickly increase the temperature to 950-1000℃ at a temperature rise of 45-50℃ / h, keep warm for 3-5h, slowly decrease the temperature to 850-900℃ at a temperature drop of 5-10℃, and air cool to 200-250℃ and keep warm for 3-5h;
[0087] Slowly increase the temperature to 750-800℃ at a rate of 10-15℃ / h, keep it warm for 3-5h, slowly decrease the temperature to 650-700℃ at a rate of 5-10℃, and air cool to 150-200℃ and keep it warm for 2-3h;
[0088] Slowly increase the temperature to 550-600℃ at a rate of 20-25℃ / h, keep warm for 2-3h and air cool;
[0089] Heat to 820-850℃, immerse in water and cool quickly;
[0090] Heat to 600-620℃ and immerse in water to cool quickly.
[0091] Comparative Example 2
[0092] This comparative example is used to prepare a 30Cr2Ni4MoV steel, which is prepared from the following components in percentage by weight:
[0093] Carbon: 0.3wt%; Chromium: 1.75wt%; Nickel: 1.5wt%; Molybdenum: 0.2wt%; Vanadium: 0.2wt%; Iron: balance.
[0094] The preparation method of the comparative example 30Cr2Ni4MoV steel is as follows:
[0095] Take formulated amounts of chromium, nickel, molybdenum, vanadium and iron respectively, heat them until they are melted, add carbon powder and mix them evenly; heat them to above 1500° C. for overheat treatment; cool them to 1500° C. or below for casting to obtain 30Cr2Ni4MoV steel.
[0096] The post-forging heat treatment method of the 30Cr2Ni4MoV steel in this comparative example is as follows:
[0097] Slowly increase the temperature to 850-900℃ at a temperature rise of 20-25℃ / h, then quickly increase the temperature to 950-1000℃ at a temperature rise of 45-50℃ / h, keep warm for 3-5h, slowly decrease the temperature to 850-900℃ at a temperature drop of 5-10℃, and air cool to 200-250℃ and keep warm for 3-5h;
[0098] Slowly increase the temperature to 750-800℃ at a rate of 10-15℃ / h, keep it warm for 3-5h, slowly decrease the temperature to 650-700℃ at a rate of 5-10℃, and air cool to 150-200℃ and keep it warm for 2-3h;
[0099] Slowly increase the temperature to 550-600℃ at a rate of 20-25℃ / h, keep warm for 2-3h and air cool;
[0100] Heat to 820-850℃, immerse in water and cool quickly;
[0101] Heat to 600-620℃ and immerse in water to cool quickly.
[0102] Comparative Example 3
[0103] This comparative example is used to prepare a 30Cr2Ni4MoV steel, which is prepared from the following components in percentage by weight:
[0104] Carbon: 0.32wt%; Chromium: 1.55wt%; Nickel: 1.4wt%; Molybdenum: 0.3wt%; Vanadium: 0.1wt%; Iron: balance.
[0105] The preparation method of the comparative example 30Cr2Ni4MoV steel is as follows:
[0106] Take formulated amounts of chromium, nickel, molybdenum, vanadium and iron respectively, heat them until they are melted, add carbon powder and mix them evenly; heat them to above 1500° C. for overheat treatment; cool them to 1500° C. or below for casting to obtain 30Cr2Ni4MoV steel.
[0107] The post-forging heat treatment method of the 30Cr2Ni4MoV steel in this comparative example is as follows:
[0108] Slowly increase the temperature to 850-900℃ at a temperature rise of 20-25℃ / h, then quickly increase the temperature to 950-1000℃ at a temperature rise of 45-50℃ / h, keep warm for 3-5h, slowly decrease the temperature to 850-900℃ at a temperature drop of 5-10℃, and air cool to 200-250℃ and keep warm for 3-5h;
[0109] Slowly increase the temperature to 750-800℃ at a rate of 10-15℃ / h, keep it warm for 3-5h, slowly decrease the temperature to 650-700℃ at a rate of 5-10℃, and air cool to 150-200℃ and keep it warm for 2-3h;
[0110] Slowly increase the temperature to 550-600℃ at a rate of 20-25℃ / h, keep warm for 2-3h and air cool;
[0111] Heat to 820-850℃, immerse in water and cool quickly;
[0112] Heat to 600-620℃ and immerse in water to cool quickly.
[0113] Comparative Example 4
[0114] This comparative example is used to prepare a 30Cr2Ni4MoV steel, which is prepared from the following components in percentage by weight:
[0115] Carbon: 0.35wt%; Chromium: 1.65wt%; Nickel: 1.8wt%; Molybdenum: 0.3wt%; Vanadium: 0.1wt%; Iron: balance.
[0116] The preparation method of the comparative example 30Cr2Ni4MoV steel is as follows:
[0117] Take formulated amounts of chromium, nickel, molybdenum, vanadium and iron respectively, heat them until they are melted, add carbon powder and mix them evenly; heat them to above 1500° C. for overheat treatment; cool them to 1500° C. or below for casting to obtain 30Cr2Ni4MoV steel.
[0118] The post-forging heat treatment method of the 30Cr2Ni4MoV steel in this comparative example is as follows:
[0119] Slowly increase the temperature to 850-900℃ at a temperature rise of 20-25℃ / h, then quickly increase the temperature to 950-1000℃ at a temperature rise of 45-50℃ / h, keep warm for 3-5h, slowly decrease the temperature to 850-900℃ at a temperature drop of 5-10℃, and air cool to 200-250℃ and keep warm for 3-5h;
[0120] Slowly increase the temperature to 750-800℃ at a rate of 10-15℃ / h, keep it warm for 3-5h, slowly decrease the temperature to 650-700℃ at a rate of 5-10℃, and air cool to 150-200℃ and keep it warm for 2-3h;
[0121] Slowly increase the temperature to 550-600℃ at a rate of 20-25℃ / h, keep warm for 2-3h and air cool;
[0122] Heat to 820-850℃, immerse in water and cool quickly;
[0123] Heat to 600-620℃ and immerse in water to cool quickly.
[0124] The performance of the 30Cr2Ni4MoV steel prepared in the above Examples 1 to 4 and Comparative Examples 1 to 4 was tested, and the results are shown in Table 1.
[0125] Table 1
[0126] Material Internal grain size External grain size Flaw detection sensitivity / mm Example 1 9 9 0.53 Example 2 10 10 0.35 Example 3 10 10 0.29 Example 4 9 10 0.58 Comparative Example 1 7 5 1.1 Comparative Example 2 7 5 1.3 Comparative Example 3 7 5 1.4 Comparative Example 4 7 5 1.2
[0127] It can be seen from Examples 1 to 4, Comparative Examples 1 to 4 and Table 1 that the technical solution of the present application can reduce the grain size of 30Cr2Ni4MoV steel, improve the grain size grade of 30Cr2Ni4MoV steel, and reduce the difference in grain size between the inside and outside of 30Cr2Ni4MoV steel after adding a small amount of attapulgite; the flaw detection sensitivity is higher.
[0128] It can be seen from Examples 1 to 4 and Table 1 that when the total weight of carbon, chromium, nickel, molybdenum and vanadium in the technical scheme of the present application is in the range of 46 to 49 times the weight of attapulgite, the prepared 30Cr2Ni4MoV steel has smaller grains, a smaller difference in grain size between the inside and the outside, and a higher sensitivity in flaw detection.
[0129] To verify this conclusion, the applicant made the following Examples 5 to 10
[0130] Example 5
[0131] In this embodiment, based on the first embodiment, the addition amount of attapulgite is increased to 0.08wt%, and the total weight of carbon, chromium, nickel, molybdenum and vanadium is 47 times the weight of attapulgite; other formulas and processes are the same as those in the first embodiment.
[0132] Example 6
[0133] In this embodiment, based on the first embodiment, the addition amount of attapulgite is increased to 0.1wt%, and the total weight of carbon, chromium, nickel, molybdenum and vanadium is 37 times the weight of attapulgite; other formulas and processes are the same as those in the first embodiment.
[0134] In this embodiment, based on the embodiment 2, the addition amount of attapulgite is increased to 0.08wt%, and the total weight of carbon, chromium, nickel, molybdenum and vanadium is 79 times the weight of attapulgite; the other formulas and processes are the same as those in the embodiment 2.
[0135] Example 8
[0136] In this embodiment, based on the embodiment 2, the addition amount of attapulgite is increased to 0.1wt%, and the total weight of carbon, chromium, nickel, molybdenum and vanadium is 40 times the weight of attapulgite; the other formulas and processes are the same as those in the embodiment 2.
[0137] Example 9
[0138] In this embodiment, based on the third embodiment, the addition amount of attapulgite is increased to 0.08wt%, and the total weight of carbon, chromium, nickel, molybdenum and vanadium is 73 times the weight of attapulgite; the other formulas and processes are the same as those in the third embodiment.
[0139] Example 10
[0140] In this embodiment, based on the third embodiment, the addition amount of attapulgite is increased to 0.1wt%, and the total weight of carbon, chromium, nickel, molybdenum and vanadium is 37 times the weight of attapulgite; the other formulas and processes are the same as those in the third embodiment.
[0141] The performance of the 30Cr2Ni4MoV steel prepared in Examples 5 to 10 was tested, and the results are shown in Table 2.
[0142] Table 2
[0143] Material Internal grain size External grain size Flaw detection sensitivity / mm Example 1 9 9 0.53 Example 5 10 10 0.46 Example 6 9 10 0.55 Example 7 9 9 0.59 Example 2 10 10 0.35 Example 8 9 10 0.56 Example 9 9 10 0.51 Example 3 10 10 0.29 Example 10 9 9 0.57
[0144] By comparing Example 1 with Examples 5-6; Example 2 with Examples 7-8; Example 3 with Examples 9-10, it can be seen that when the total weight of carbon, chromium, nickel, molybdenum and vanadium in the technical scheme of the present application is in the range of 46 to 49 times the weight of attapulgite, the prepared 30Cr2Ni4MoV steel has smaller grains, a smaller difference in grain size between the inside and the outside, and a higher sensitivity in flaw detection.
[0145] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A 30Cr2Ni4MoV steel, characterized in that: Prepared from the following components by weight percentage: Carbon 0.28-0.35wt%; Chromium 1.45-1.75wt%; Nickel 1.4-1.8wt%; Molybdenum 0.2-0.3wt%; Vanadium 0.1-0.2wt%; Attapulgite 0.05-0.1wt%; Iron balance.
2. The 30Cr2Ni4MoV steel according to claim 1, characterized in that The total weight of the carbon, chromium, nickel, molybdenum and vanadium is 46 to 49 times the weight of attapulgite.
3. The 30Cr2Ni4MoV steel according to claim 1, characterized in that The particle size of the attapulgite is 0.2 to 1 μm.
4. A method for preparing the 30Cr2Ni4MoV steel according to claim 1, characterized in that: The following steps are involved: S1. Take the formulated amounts of chromium, nickel, molybdenum, vanadium and iron respectively, heat them until they are melted, add carbon powder and attapulgite, and mix them evenly; S2, heating to above 1500℃ for overheating treatment; S3. Cool to 1500°C or below and cast to obtain 30Cr2Ni4MoV steel.
5. A post-forging heat treatment method for 30Cr2Ni4MoV steel according to claim 1, characterized in that: The following steps are involved: S1 one-step normalizing Slowly increase the temperature to 850-900℃ at a temperature rise of 20-25℃ / h, then quickly increase the temperature to 950-1000℃ at a temperature rise of 45-50℃ / h, keep warm for 3-5h, slowly decrease the temperature to 850-900℃ at a temperature drop of 5-10℃, and air cool to 200-250℃ and keep warm for 3-5h; S2 secondary normalizing Slowly increase the temperature to 750-800℃ at a rate of 10-15℃ / h, keep it warm for 3-5h, slowly decrease the temperature to 650-700℃ at a rate of 5-10℃, and air cool to 150-200℃ and keep it warm for 2-3h; S3 one-time tempering Slowly increase the temperature to 550-600℃ at a rate of 20-25℃ / h, keep warm for 2-3h and air cool; S4 Quenching Heat to 820-850℃, immerse in water and cool quickly; S5 secondary tempering Heat to 600-620℃ and immerse in water to cool quickly.
6. Application of the 30Cr2Ni4MoV steel according to claim 1 in the field of low-pressure rotors.