Ultrathin transparent electromagnetic shielding film and preparation method and device thereof

By co-evaporating silver and aluminum materials in a vacuum coating machine and controlling their rate and content, an ultra-thin transparent electromagnetic shielding film was prepared. This solved the problem that transparent electromagnetic shielding materials could not simultaneously achieve high transmittance and strong shielding effect, thus achieving a balance between high transmittance and strong electromagnetic shielding.

CN118979224AActive Publication Date: 2024-11-19ZHONGSHAN INST OF CHANGCHUN UNIV OF SCI & TECH +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411090162.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Existing transparent electromagnetic shielding materials cannot simultaneously achieve both high transmittance and strong shielding effect.

Method used

An ultrathin transparent electromagnetic shielding film is prepared by co-evaporating and depositing silver and aluminum materials in a vacuum coating machine. By controlling the rate and content ratio of silver and aluminum materials, a small amount of aluminum is doped into the silver film to form an electromagnetic shielding film of silver particles and aluminum particles.

Benefits of technology

It achieves a balance between high transmittance and strong electromagnetic shielding effect, with a transmittance of over 88% and an electromagnetic shielding effect of 27dB in the 20MHz to 5GHz frequency band, meeting the requirements of high transparency and good electromagnetic shielding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979224A_ABST
    Figure CN118979224A_ABST
Patent Text Reader

Abstract

The invention provides an ultrathin transparent electromagnetic shielding film and a preparation method and device thereof, and is applied to the technical field of optical coating materials, electromagnetic shielding films and vacuum coating. A silver material and an aluminum material are used as raw materials and are co-evaporated and deposited to a shielding film base material in a vacuum coating machine; the electromagnetic shielding film comprises silver particles and aluminum particles; the silver material and the aluminum material are separated by a partition plate and are subjected to co-evaporation deposition on the shielding film base material respectively, and the first rate of the silver material in co-evaporation deposition and the second rate of the aluminum material in co-evaporation deposition are controlled respectively; the content ratio of the silver particles and the content ratio of the aluminum particles in the electromagnetic shielding film meet the electromagnetic shielding requirement and the light transmittance requirement, so that the electromagnetic shielding film has high transmittance and a strong shielding effect at the same time according to requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical fields of optical coating materials, electromagnetic shielding films and vacuum coating, and in particular to an ultra-thin transparent electromagnetic shielding film and a preparation method and device. Background Art

[0002] Transparent electromagnetic shielding films have great application demand in many fields such as communication equipment, medical equipment, instrumentation, aerospace, weapons and equipment, such as photoelectric guided missiles, laser guided missiles and fighter cockpits, and have attracted widespread attention. However, in current transparent shielding materials, it is difficult to have both high transmittance and strong shielding effect at the same time.

[0003] Based on this, a new technical solution is needed for an electromagnetic shielding film that has both high transmittance and strong shielding effect. Summary of the invention

[0004] In view of this, the embodiments of this specification provide an ultra-thin transparent electromagnetic shielding film and a preparation method and device.

[0005] The embodiments of this specification provide the following technical solutions:

[0006] The embodiment of the present specification provides a method for preparing an ultra-thin transparent electromagnetic shielding film, comprising: using a silver material and an aluminum material as raw materials, and co-evaporating and depositing the silver material and the aluminum material on a shielding film substrate in a vacuum coating machine to obtain an electromagnetic shielding film containing silver particles and aluminum particles; wherein the silver material and the aluminum material are separated by a partition and placed inside the vacuum coating machine, so that the silver material and the aluminum material are co-evaporated and deposited on the shielding film substrate respectively under the separation of the partition;

[0007] In the co-evaporation deposition process, according to the electromagnetic shielding requirements and transmittance requirements of the electromagnetic shielding film, the first rate of the silver material in the co-evaporation deposition is controlled, and the second rate of the aluminum material in the co-evaporation deposition is controlled, so that the proportion of silver particles and the proportion of aluminum particles in the electromagnetic shielding film meet the electromagnetic shielding requirements and transmittance requirements.

[0008] The embodiments of the present specification also provide an ultra-thin transparent electromagnetic shielding film, which is an electromagnetic shielding film prepared by the above-mentioned ultra-thin transparent electromagnetic shielding film preparation method.

[0009] The embodiment of this specification also provides a device for preparing an ultra-thin transparent electromagnetic shielding film, comprising:

[0010] A partition is erected at the bottom of the vacuum coating machine;

[0011] Dual electron guns are respectively located on both sides of the partition, each electron gun correspondingly serving as an evaporation source for evaporating silver material or an evaporation source for evaporating aluminum material;

[0012] A controller is connected to the electron gun and is used to control a first rate of the silver material in the co-evaporation deposition and a second rate of the aluminum material in the co-evaporation deposition according to the electromagnetic shielding requirements and the transmittance requirements of the electromagnetic shielding film, so that the proportion of the silver particles and the proportion of the aluminum particles in the electromagnetic shielding film meet the electromagnetic shielding requirements and the transmittance requirements.

[0013] Compared with the prior art, the at least one technical solution adopted in the embodiments of this specification can achieve the following beneficial effects:

[0014] In the present application, the silver material and the aluminum material are separated by a partition and co-evaporated and deposited onto the shielding film substrate respectively, and the first rate of the silver material in the co-evaporation deposition and the second rate of the aluminum material in the co-evaporation deposition are controlled respectively, so that the proportion of the silver particles in the electromagnetic shielding film meets the electromagnetic shielding requirements, and the proportion of the aluminum particles meets the transmittance requirements, so that both high transmittance and strong shielding effect can be achieved as needed. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 It is a schematic diagram of the structure of the ultra-thin transparent electromagnetic shielding film of the present application;

[0017] Figure 2 It is a schematic diagram of the co-evaporation structure of this application;

[0018] Figure 3 This is a spectrum transmittance diagram of the ultra-thin Ag-Al film obtained in the embodiment of the present application;

[0019] Figure 4 This is a SEM image of the ultra-thin Ag-Al film obtained in the embodiment of the present application;

[0020] Figure 5 This is the EDS image of the ultra-thin Ag-Al film obtained in the embodiment of the present application.

[0021] Figure numerals: 1. first monitoring probe; 2. second monitoring probe; 3. third monitoring probe; 4. evaporation source of silver material; 5. evaporation source of aluminum material; 6. partition; 7. correction baffle; 8. shielding film substrate; 9. connecting layer; 10. Ag-Al film. DETAILED DESCRIPTION

[0022] The embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0023] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.

[0024] It should be noted that various aspects of the embodiments within the scope of the appended claims are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0025] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show components related to the present application rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0026] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the examples can be practiced without these specific details.

[0027] The applicant has conducted in-depth research and improvement on coating materials and electromagnetic shielding films and found that ultra-thin metal films have excellent optoelectronic properties and stability, and have the potential to become transparent electromagnetic shielding. Among them, ultra-thin silver film (Ag) has become the most representative material for transparent electromagnetic shielding due to its excellent transparency and good conductivity. However, according to the island generation mode (Volmer-Weber) film growth mechanism, Ag with a thickness of less than 20nm is difficult to form a uniform and continuous Ag film, which leads to poor electromagnetic shielding effect of the film layer; as the thickness of the Ag film increases, the Ag particles thicken, and the separated silver particles condense, diffuse, and connect to form a continuous and uniform silver film. At this time, the electromagnetic shielding effect is good, but the visible transmittance is reduced.

[0028] Based on this, the technical solutions provided by the embodiments of the present application are described below in conjunction with the accompanying drawings.

[0029] The present invention provides a method for preparing an ultra-thin transparent electromagnetic shielding film. Figure 1 and Figure 2 As shown, it includes: using silver material and aluminum material as raw materials, respectively co-evaporating and depositing the silver material and the aluminum material onto a shielding film substrate 8 in a vacuum coating machine to obtain an electromagnetic shielding film containing silver particles and aluminum particles; the silver material and the aluminum material are separated by a partition 6 and placed inside the vacuum coating machine, so that under the separation of the partition 6, the silver material and the aluminum material are respectively co-evaporated and deposited onto the shielding film substrate 8.

[0030] In the co-evaporation deposition process, according to the electromagnetic shielding requirements and transmittance requirements of the electromagnetic shielding film, the first rate of the silver material in the co-evaporation deposition is controlled, and the second rate of the aluminum material in the co-evaporation deposition is controlled, so that the proportion of silver particles and the proportion of aluminum particles in the electromagnetic shielding film meet the electromagnetic shielding requirements and transmittance requirements. The silver Ag film is doped with a small amount of aluminum Al by the doping technology, which is conducive to the silver Ag film to achieve a continuous and uniform film layer in the ultra-thin case, while taking into account high transmittance and good electromagnetic shielding effect.

[0031] In one embodiment, a first monitoring probe 1 is used to monitor a first rate of the silver material in co-evaporation deposition, and a second monitoring probe 2 is used to monitor a second rate of the aluminum material in co-evaporation deposition; wherein the first monitoring probe 1 and the silver material are arranged on one side of the partition 6, and the second monitoring probe 2 and the aluminum material are arranged on the other side of the partition 6, and the connection line between the first monitoring probe 1 and the evaporation source 5 of the aluminum material passes through the partition 6, and similarly, the connection line between the second monitoring probe 2 and the evaporation source 4 of the silver material passes through the partition 6, so that during the co-evaporation deposition, the first monitoring probe 1 does not collect the deposition parameters corresponding to the aluminum material, and the second monitoring probe 2 does not collect the deposition parameters corresponding to the silver material.

[0032] In one embodiment, the first rate monitored by the first monitoring probe 1 is 0.4 nm / s to 0.6 nm / s, and / or the second rate monitored by the second monitoring probe 2 is 0.02 nm / s to 0.05 nm / s. The first monitoring probe 1 and the second monitoring probe 2 can be in the same plane, the evaporation source 4 of the silver material and the evaporation source 5 of the aluminum material can also be in the same plane, and the distance between the first monitoring probe 1 and the plane where the evaporation source 4 of the silver material is located can be 60 to 90 cm.

[0033] In one embodiment, the method for preparing the electromagnetic shielding film further comprises: monitoring the deposition rate and / or deposition thickness of the electromagnetic shielding film by means of a third monitoring probe 3 .

[0034] In one embodiment, the deposition rate monitored by the third monitoring probe 3 is 0.42nm / s to 0.44nm / s, and can be preferably 0.43nm / s; and / or, the deposition thickness monitored by the third monitoring probe 3 is 7nm to 10nm, wherein when the monitored deposition thickness exceeds 10nm, the co-evaporation process is stopped. The third monitoring probe 3 and the shielding film substrate 8 can be in the same plane, the evaporation source 4 of the silver material and the evaporation source 5 of the aluminum material can be in the same plane, and the distance between the third monitoring probe 3 and the plane where the evaporation source 4 of the silver material is located can be 100cm to 130cm.

[0035] In one embodiment, the silver material evaporates to form silver particles during co-evaporation deposition, and the aluminum material evaporates to form aluminum particles during co-evaporation deposition; a small portion of the silver particles and a small portion of the aluminum particles are deposited toward the shielding layer substrate by blocking most of the silver particles and most of the aluminum particles through the correction baffle 7, so that the first rate is lower than the evaporation rate at the evaporation source 4 of the silver material, and the second rate is lower than the evaporation rate at the evaporation source 5 of the aluminum material.

[0036] In one embodiment, the correction baffle 7 is divided into guide plates located on both sides of the plate surface where the partition 6 is located. The guide plates on both sides can be distributed obliquely upward in the direction of the plate surface where the partition 6 is located, and a gap is formed between the guide plates on both sides. The formed gap is located above the partition 6, so that the silver particles and aluminum particles contacting the guide plates can flow into the formed gap.

[0037] The guide plate on one side is located on the side where the silver material is located, and the guide plate on the other side is located on the side where the aluminum material is located; the guide plates on both sides have a closed state and an open state; when the guide plates on both sides are in the open state, they are distributed obliquely upward in the direction of the board surface where the partition 6 is located; when the guide plates on both sides are in the closed state, they can be horizontally distributed in the direction of the board surface where the partition 6 is located; when the guide plate on one side is in the closed state, it can be located 40cm to 60cm directly above the evaporation source 4 of the silver material, and the width can be 10 to 20cm; when the guide plate on the other side is in the closed state, it can be located 40cm to 60cm directly above the evaporation source 5 of the aluminum material, and the width can be 10 to 20cm.

[0038] Using precise monitoring technology, silver Ag film and aluminum Al film are prepared by electron beam evaporation. The deposition rate is very fast (usually >1.5nm / s), and the total thickness of the ultra-thin film is only a few nanometers (usually less than 10nm), so it is difficult to stably control the thickness of the film layer. The conventional correction baffle 7 is to improve the uniformity of the film layer, while the method based on the design of the ultra-wide correction baffle 7 in this application not only improves the uniformity of the film layer, but also blocks most of the film material particles and reduces the deposition rate on the sample surface, achieving the effect of high evaporation rate at the evaporation source position, but low deposition rate on the actual sample surface, and achieving the purpose of effectively and stably controlling the thickness of the ultra-thin Ag-Al film 10. The ultra-wide correction baffle 7 is located 40cm to 60cm above the evaporation source corresponding to the Al and Ag materials, with a width of 10 to 20cm. The first monitoring probe 1 and the second monitoring probe 2 are located 20cm-30cm above the correction baffle 7. The third monitoring probe 3 is basically in the same plane as the sample, 100cm to 130cm away from the evaporation source plane, and the specific size is modified and optimized according to the actual process.

[0039] In one embodiment, the electromagnetic shielding film preparation method further includes: after the co-evaporation deposition, the electromagnetic shielding film is subjected to a vacuum annealing process. A vacuum annealing technology is used. A reasonable vacuum annealing process is conducive to making the surface of the Ag-Al film 10 more uniform, reducing the roughness (RMS), and reducing defects in the coating process, such as incomplete crystallization, internal stress accumulation, and lattice defects.

[0040] In one embodiment, it is verified by experiments that the vacuum annealing process is: the vacuum degree is 2.0×10 -4 Pa, the heating rate is controlled within 20℃ / min, the highest temperature is 180℃-220℃, the holding time is 3-8min, and then it is cooled naturally to room temperature. -4 When the vacuum chamber is 3000MW, there is a lot of residual gas in the vacuum chamber. During high-temperature annealing, the metal film will react with the residual gas to generate compounds, which will reduce the electromagnetic shielding effect.

[0041] In one embodiment, the shielding film substrate 8 is any one of the following: K9, JGS1, JGS2, JGS3 and sapphire and other base materials. Silver Ag and aluminum Al are used as two metal materials, and the purity of the two materials must be above 99.99%.

[0042] And / or, the co-evaporation deposition process adopts electron beam co-evaporation, that is, the preparation method is vacuum electron beam co-evaporation evaporation technology.

[0043] And / or, before the co-evaporation process, the electron guns corresponding to the silver material and the aluminum material are fully pre-melted, and the deposition process is started when the error between the power of the electron gun and the power during deposition falls within a preset range.

[0044] And / or, before the co-evaporation treatment, the shielding film substrate 8 is cleaned and wiped with an alcohol-ether mixture.

[0045] And / or, before co-evaporation treatment, the vacuum chamber is evacuated, and when the vacuum degree reaches a first vacuum degree, the shielding film substrate 8 is pre-treated by ion cleaning, and the ion source parameters used for ion cleaning are voltage of 1200V, current of 950mA, and cleaning for 5-10 minutes.

[0046] In one embodiment, the method for preparing the electromagnetic shielding film further comprises: before the co-evaporation deposition, depositing a connection layer 9 on the shielding film substrate 8 to serve as a connection between the shielding film substrate 8 and the electromagnetic shielding film.

[0047] In one embodiment, when the vacuum degree is the second vacuum degree, a connection layer 9 of 10 nm to 15 nm is deposited on the shielding film substrate 8 at a preset rate, and / or the connection layer 9 is made of SiO2 or Al2O3. The connection layer 9 technology uses SiO2 or Al2O3 as the material of the connection layer 9, which can effectively improve the adhesion between the metal film and the substrate and improve the mechanical firmness of the film layer.

[0048] This application obtains an ultra-thin Ag-Al transparent electromagnetic shielding film by depositing two materials, silver Ag and aluminum Al, by co-evaporation and direct vacuum annealing after coating. The vacuum electron beam co-evaporation technology is used to evaporate Ag and Al at the same time, and the evaporation rate is used to control the proportion of the two materials in the Ag-Al film. Through process optimization and direct vacuum annealing, an ultra-thin, uniform and continuous Ag-Al transparent electromagnetic shielding metal film is obtained.

[0049] The present application can solve the current problem of high transmittance in the visible light range but poor electromagnetic shielding effect in the range of 20MHz to 5GHz, or good electromagnetic shielding effect in the range of 20MHz to 5GHz but low transmittance in the visible light range, and the inability to simultaneously take into account high visible transmittance and good electromagnetic shielding effect. The present application deposits two materials, Ag and Al, by co-evaporation and directly performs a vacuum annealing process after the coating is completed, to prepare an ultra-thin Ag-Al transparent electromagnetic shielding film with a transmittance of more than 88% at a wavelength of 550nm and an average electromagnetic shielding of 27dB in the frequency band of 20MHz to 5GHz.

[0050] The present specification also discloses an ultra-thin transparent electromagnetic shielding film, such as Figure 1 and Figure 2 As shown, an electromagnetic shielding film is prepared by using the method for preparing an ultra-thin transparent electromagnetic shielding film according to any of the above embodiments.

[0051] In one embodiment, the transmittance of the electromagnetic shielding film at a wavelength of 550 nm is above 85%; and / or the average electromagnetic shielding in the frequency band of 20 MHz to 5 GHz is 26 dB to 35 dB.

[0052] In one embodiment, the electromagnetic shielding film is a film in which aluminum particles are doped in silver particles, that is, an Ag-Al film 10. The film composition is: the content of silver particles in the electromagnetic shielding film accounts for 96Atomic% to 92Atomic%, and / or the content of aluminum particles accounts for 4Atomic% to 8Atomic%. Atomic% means atomic percentage. Experimental verification shows that the doping ratio should be maintained at 96Atomic% to 92Atomic% for Ag and 4Atomic% to 8Atomic% for Al.

[0053] In one embodiment, the electromagnetic shielding film is connected to the shielding film substrate 8 via a connecting layer 9. Figure 1 As shown, it is composed of a substrate, a connecting layer 9 and an Ag-Al film 10. The substrate can be an electromagnetic film substrate.

[0054] The present specification also provides a device for preparing an ultra-thin transparent electromagnetic shielding film, such as Figure 1 and Figure 2 As shown, including:

[0055] The partition 6 is erected at the bottom of the vacuum coating machine.

[0056] The dual electron guns are respectively located on both sides of the partition 6, and each electron gun corresponds to an evaporation source 4 for evaporating silver material or an evaporation source 5 for evaporating aluminum material.

[0057] The controller is connected to the electron gun and is used to control a first rate of the silver material in the co-evaporation deposition and a second rate of the aluminum material in the co-evaporation deposition according to the electromagnetic shielding requirements and the transmittance requirements of the electromagnetic shielding film, so that the proportion of the silver particles and the proportion of the aluminum particles in the electromagnetic shielding film meet the electromagnetic shielding requirements and the transmittance requirements.

[0058] In one embodiment, the electromagnetic shielding film preparation device also includes: a first monitoring probe 1 and a second monitoring probe 2 connected to the controller; the first monitoring probe 1 monitors the first rate of the silver material in the co-evaporation deposition, and the second monitoring probe 2 monitors the second rate of the aluminum material in the co-evaporation deposition; wherein the first monitoring probe 1 and the silver material are arranged on one side of the partition 6, and the second monitoring probe 2 and the aluminum material are arranged on the other side of the partition 6, and the connection line between the first monitoring probe 1 and the evaporation source 5 of the aluminum material passes through the partition 6, and similarly, the connection line between the second monitoring probe 2 and the evaporation source 4 of the silver material passes through the partition 6, so that during the co-evaporation deposition, the first monitoring probe 1 does not collect the deposition parameters corresponding to the aluminum material, and the second monitoring probe 2 does not collect the deposition parameters corresponding to the silver material.

[0059] In one embodiment, the first rate monitored by the first monitoring probe 1 is 0.4 nm / s to 0.6 nm / s, and / or the second rate monitored by the second monitoring probe 2 is 0.02 nm / s to 0.05 nm / s.

[0060] In one embodiment, the electromagnetic shielding film preparation device further includes: a third monitoring probe 3 connected to the controller, and the third monitoring probe 3 monitors the deposition rate and / or deposition thickness of the electromagnetic shielding film.

[0061] In one embodiment, the deposition rate monitored by the third monitoring probe 3 is 0.42nm / s to 0.44nm / s; and / or the deposition thickness monitored by the third monitoring probe 3 is 7nm to 10nm, wherein when the monitored deposition thickness exceeds 10nm, the co-evaporation process is stopped.

[0062] In one embodiment, the electromagnetic shielding film preparation device also includes: a corrected baffle 7; the silver material evaporates to form silver particles during co-evaporation deposition, and the aluminum material evaporates to form aluminum particles during co-evaporation deposition; the corrected baffle 7 blocks most of the silver particles and most of the aluminum particles, and allows a small portion of the silver particles and a small portion of the aluminum particles to be deposited onto the shielding layer substrate, so that the first rate is lower than the evaporation rate at the evaporation source 4 of the silver material, and the second rate is lower than the evaporation rate at the evaporation source 5 of the aluminum material.

[0063] In one embodiment, the correction baffle 7 is divided into guide plates located on both sides of the plate surface where the partition 6 is located, and the guide plates on both sides can be distributed obliquely upward in the direction of the plate surface where the partition 6 is located, and a gap is formed between the guide plates on both sides, and the formed gap is located above the partition 6, so that the silver particles and aluminum particles contacting the guide plates flow into the formed gap. The controller can be connected to the correction baffle to control the opening and closing of the correction baffle and the opening angle of the guide plate.

[0064] In one embodiment, the vacuum coating machine includes a 1300 type vacuum coating machine.

[0065] The present specification also provides a method for manufacturing an ultra-thin transparent electromagnetic shielding film. Figure 1 and Figure 2 As shown, a 1300 type vacuum coating machine is used, which is equipped with dual electron guns, RF17cm radio frequency ion source, three sets of multi-probe quartz crystal monitoring systems and a cryogenic pump + dry pump oil-free exhaust system.

[0066] The double electron gun co-evaporation technology was used to prepare the Ag-Al transparent electromagnetic shielding film on the K9 substrate with a diameter of 30 mm and a thickness of 2 mm. The co-evaporation diagram is shown in the figure below. Figure 2 shown.

[0067] Co-evaporation scheme allocation: two groups of electron gun evaporation sources evaporate Ag and Al respectively, the third monitoring probe 3 monitors the deposition rate and thickness of Ag-Al, the first monitoring probe 1 monitors the deposition rate and thickness of Ag, the second monitoring probe 2 monitors the deposition rate and thickness of Al, and the function of the isolation baffle is to prevent the Ag deposition rate from affecting the second monitoring probe 2 and the Al deposition rate from affecting the second monitoring probe 2.

[0068] The deposition rate is controlled by adjusting the electron gun power to ensure that the deposition rate is 0.4nm / s to 0.6nm / s for Ag and 0.02nm / s to 0.05nm / s for Al. The thickness of the Ag-Al film 10 is 7nm to 10nm, and the average transmittance at 550nm is 85% to 91%; the electromagnetic shielding in the 20MHz to 5GHz frequency band is 26dB to 35dB on average.

[0069] The specific preparation process is as follows:

[0070] 1. Clean and wipe the K9 substrate with an alcohol-ether mixture, the K9 substrate can be called a sample or a shielding film substrate 8;

[0071] 2. Place the wiped sample on the sample rack of the coating machine and evacuate the vacuum chamber. When the vacuum degree reaches 3.0×10 -4 When Pa, turn on the radio frequency ion source to perform ion cleaning pretreatment on the sample. The radio frequency ion source parameter voltage is 1200V, current is 950mA, and cleaning takes 5-10 minutes.

[0072] 3. After cleaning, wait until the vacuum degree stabilizes at 2.0×10 -4 Pa, thin film deposition begins, and a 10nm to 15nm thick SiO2 film is deposited as the connecting layer 9 at a rate of 0.7nm / s.

[0073] 4. Start preparing the ultra-thin Ag-Al film 10, and turn on the electron guns corresponding to the Ag material and the Al material at the same time, pre-melt the Ag and Al materials, and after sufficient pre-melting, open the baffles of Ag and Al at the same time to co-evaporate and prepare the Ag-Al thin film, and adjust the electron gun power so that the monitoring rate of Ag, that is, the rate monitored by the first monitoring probe 1, is controlled at about 0.5nm / s, and the monitoring rate of Al, that is, the rate monitored by the second monitoring probe 2, is controlled at about 0.03nm / s. At this time, the rate of Ag-Al, that is, the rate monitored by the third monitoring probe 3, is about 0.42nm / s~0.44nm / s. When the thickness of the third monitoring probe 3 shows 8nm, turn off the electron gun, baffle and other systems to stop film deposition.

[0074] 5. After the film deposition is completed, continue to evacuate until the vacuum degree reaches 2.0×10 -4Pa, start the vacuum annealing process.

[0075] 6. Control the heating rate at about 15℃ / min, heat to 200℃, maintain for 5 minutes, then stop vacuuming and heating, start cooling naturally, and take out the sample when it reaches room temperature.

[0076] 7. The transmittance of Ag-Al film in the visible light range was measured by UV-Vis-NIR spectrophotometer. Figure 3 As shown, the transmittance at 550 nm is about 88.4%, and the thickness of the Ag-Al film 10 under this process is measured to be 8.7 nm. Figure 3 In the figure, Wavelength represents wavelength and Transmittance represents transmittance.

[0077] 8. The surface morphology of Ag-Al samples was measured by scanning electron microscopy (SEM). Figure 4 As shown in the figure, it can be seen that the particles on the surface of the film layer are uniform and flat, and the uniformity is good.

[0078] 9. The surface of Ag-Al samples was measured by energy dispersive spectrometer (EDS). Figure 5 As shown, the proportions of Ag and Al in the film layer of the Ag—Al film 10 are 95.36 Atomic % and 4.64 Atomic % respectively, and the Ag particles and the Al particles are all evenly distributed in the film layer of the Ag—Al film 10 . Figure 5 The Element in represents an element.

[0079] 10. Using an electromagnetic shielding tester, it was measured that the average electromagnetic shielding of the Ag-Al film 10 in the 20MHz~5GHz frequency band is 27dB.

[0080] Therefore, the ultra-thin Ag—Al film 10 can meet the requirements of both high transmittance and strong electromagnetic shielding effect.

[0081] The materials and methods of the present application can achieve strong electromagnetic shielding effect while maintaining high visible transmittance. The film with high transparency and good electromagnetic shielding performance and its preparation method can be widely used in various transparent electromagnetic shielding windows.

[0082] In this specification, the same or similar parts between the various embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the embodiments described later, the description is relatively simple, and the relevant parts can be referred to the partial description of the previous embodiments.

[0083] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A method for preparing an ultra-thin transparent electromagnetic shielding film, characterized in that: include: Using silver material and aluminum material as raw materials, the silver material and the aluminum material are respectively subjected to co-evaporation deposition treatment on a shielding film substrate in a vacuum coating machine to obtain an electromagnetic shielding film containing silver particles and aluminum particles; wherein the silver material and the aluminum material are separated by a partition and placed inside the vacuum coating machine, so that the silver material and the aluminum material are respectively co-evaporated and deposited on the shielding film substrate under the separation of the partition; In the co-evaporation deposition process, according to the electromagnetic shielding requirements and transmittance requirements of the electromagnetic shielding film, the first rate of the silver material in the co-evaporation deposition is controlled, and the second rate of the aluminum material in the co-evaporation deposition is controlled, so that the proportion of silver particles and the proportion of aluminum particles in the electromagnetic shielding film meet the electromagnetic shielding requirements and transmittance requirements.

2. The method for preparing an ultra-thin transparent electromagnetic shielding film according to claim 1, characterized in that: The first rate of the silver material in the co-evaporation deposition is monitored by a first monitoring probe, and the second rate of the aluminum material in the co-evaporation deposition is monitored by a second monitoring probe; wherein the first monitoring probe and the silver material are arranged on one side of the partition, the second monitoring probe and the aluminum material are arranged on the other side of the partition, and the connection line between the first monitoring probe and the evaporation source of the aluminum material passes through the partition, and similarly, the connection line between the second monitoring probe and the evaporation source of the silver material passes through the partition, so that in the co-evaporation deposition, the first monitoring probe does not collect the deposition parameters corresponding to the aluminum material, and the second monitoring probe does not collect the deposition parameters corresponding to the silver material.

3. The method for preparing an ultra-thin transparent electromagnetic shielding film according to claim 2, characterized in that: The first rate monitored by the first monitoring probe is 0.4 nm / s to 0.6 nm / s, and / or the second rate monitored by the second monitoring probe is 0.02 nm / s to 0.05 nm / s.

4. The method for preparing an ultra-thin transparent electromagnetic shielding film according to claim 1, characterized in that: The method for preparing the electromagnetic shielding film further comprises: monitoring the deposition rate and / or deposition thickness of the electromagnetic shielding film by means of a third monitoring probe.

5. The method for preparing an ultra-thin transparent electromagnetic shielding film according to claim 4, characterized in that: The deposition rate monitored by the third monitoring probe is 0.42 nm / s to 0.44 nm / s; and / or the deposition thickness monitored by the third monitoring probe is 7 nm to 10 nm, wherein when the monitored deposition thickness exceeds 10 nm, the co-evaporation process is stopped.

6. The method for preparing an ultra-thin transparent electromagnetic shielding film according to claim 1, characterized in that: The silver material is evaporated in co-evaporation deposition to form the silver particles, and the aluminum material is evaporated in co-evaporation deposition to form the aluminum particles; By correcting the baffle to block most of the silver particles and most of the aluminum particles, a small portion of the silver particles and a small portion of the aluminum particles are deposited onto the shielding layer substrate, so that the first rate is lower than the evaporation rate at the evaporation source of the silver material, and the second rate is lower than the evaporation rate at the evaporation source of the aluminum material.

7. The method for preparing an ultra-thin transparent electromagnetic shielding film according to claim 6, characterized in that: The correction baffle is divided into guide plates located on both sides of the plate surface where the partition is located. The guide plates on both sides can be distributed obliquely upward in the direction of the plate surface where the partition is located, and a gap is formed between the guide plates on both sides. The formed gap is located above the partition, so that the silver particles and the aluminum particles contacting the guide plates can flow into the formed gap.

8. The method for preparing an ultra-thin transparent electromagnetic shielding film according to claim 1, characterized in that: The method for preparing the electromagnetic shielding film further comprises: after the co-evaporation deposition, performing a vacuum annealing process on the electromagnetic shielding film.

9. The method for preparing an ultra-thin transparent electromagnetic shielding film according to claim 8, characterized in that: The vacuum annealing process is as follows: the vacuum degree is 2.0×10 -4 Pa, the heating rate is controlled within 20℃ / min, the maximum temperature is 180℃-220℃, the holding time is 3-8min, and then it is naturally cooled to room temperature.

10. The method for preparing an ultra-thin transparent electromagnetic shielding film according to claim 1, characterized in that: The shielding film substrate is any one of the following: K9, JGS1, JGS2, JGS3 and sapphire; and / or, the co-evaporation deposition process uses electron beam co-evaporation; And / or, before the co-evaporation process, the electron guns corresponding to the silver material and the aluminum material are fully pre-melted, and the deposition process is started when the error between the power of the electron gun and the power during deposition falls within a preset range; and / or, before the co-evaporation treatment, the shielding film substrate is cleaned and wiped with an alcohol-ether mixture; And / or, before the co-evaporation treatment, the vacuum chamber is evacuated, and when the vacuum degree reaches a first vacuum degree, the shielding film substrate is pre-treated by ion cleaning, and the ion source parameters used for ion cleaning are voltage of 1200V, current of 950mA, and cleaning for 5-10 minutes.

11. The method for preparing an ultra-thin transparent electromagnetic shielding film according to claim 1, characterized in that: The method for preparing the electromagnetic shielding film further comprises: before the co-evaporation deposition, depositing a connection layer on the shielding film substrate to serve as a connection between the shielding film substrate and the electromagnetic shielding film.

12. The method for preparing an ultra-thin transparent electromagnetic shielding film according to claim 11, characterized in that: When the vacuum degree reaches the second vacuum degree, a connection layer of 10 nm to 15 nm is deposited on the shielding film substrate at a preset rate, and / or the connection layer is made of SiO2 or Al2O3.

13. An ultra-thin transparent electromagnetic shielding film, characterized in that: The electromagnetic shielding film is prepared by the method for preparing an ultra-thin transparent electromagnetic shielding film as described in any one of claims 1 to 12.

14. The ultra-thin transparent electromagnetic shielding film according to claim 13, characterized in that: The electromagnetic shielding film has a transmittance of more than 85% at a wavelength of 550nm; and / or an average electromagnetic shielding of 26dB to 35dB in a frequency band of 20MHz to 5GHz.

15. The ultra-thin transparent electromagnetic shielding film according to claim 13, characterized in that: The electromagnetic shielding film is a film in which aluminum particles are doped in silver particles. The content of the silver particles in the electromagnetic shielding film is 96Atomic% to 92Atomic%, and / or the content of the aluminum particles is 4Atomic% to 8Atomic%.

16. The ultra-thin transparent electromagnetic shielding film according to claim 13, characterized in that: The electromagnetic shielding film is connected to the shielding film substrate via a connecting layer.

17. An ultra-thin transparent electromagnetic shielding film preparation device, characterized in that: include: A partition is erected at the bottom of the vacuum coating machine; Dual electron guns are respectively located on both sides of the partition, each electron gun correspondingly serving as an evaporation source for evaporating silver material or an evaporation source for evaporating aluminum material; A controller is connected to the electron gun and is used to control a first rate of the silver material in the co-evaporation deposition and a second rate of the aluminum material in the co-evaporation deposition according to the electromagnetic shielding requirements and the transmittance requirements of the electromagnetic shielding film, so that the proportion of the silver particles and the proportion of the aluminum particles in the electromagnetic shielding film meet the electromagnetic shielding requirements and the transmittance requirements.

18. The ultra-thin transparent electromagnetic shielding film preparation device according to claim 17, characterized in that: The electromagnetic shielding film preparation device also includes: a first monitoring probe and a second monitoring probe connected to the controller; The first monitoring probe monitors a first rate of the silver material in the co-evaporation deposition, and the second monitoring probe monitors a second rate of the aluminum material in the co-evaporation deposition; The first monitoring probe and the silver material are arranged on one side of the partition, and the second monitoring probe and the aluminum material are arranged on the other side of the partition, and the connection line between the first monitoring probe and the evaporation source of the aluminum material passes through the partition, and similarly, the connection line between the second monitoring probe and the evaporation source of the silver material passes through the partition, so that during co-evaporation deposition, the first monitoring probe does not collect deposition parameters corresponding to the aluminum material, and the second monitoring probe does not collect deposition parameters corresponding to the silver material.

19. The ultra-thin transparent electromagnetic shielding film preparation device according to claim 18, characterized in that: The first rate monitored by the first monitoring probe is 0.4 nm / s to 0.6 nm / s, and / or the second rate monitored by the second monitoring probe is 0.02 nm / s to 0.05 nm / s.

20. The ultra-thin transparent electromagnetic shielding film preparation device according to claim 17, characterized in that: The electromagnetic shielding film preparation device further comprises: a third monitoring probe connected to the controller, wherein the third monitoring probe monitors the deposition rate and / or deposition thickness of the electromagnetic shielding film.

21. The ultra-thin transparent electromagnetic shielding film preparation device according to claim 20, characterized in that: The deposition rate monitored by the third monitoring probe is 0.42 nm / s to 0.44 nm / s; and / or the deposition thickness monitored by the third monitoring probe is 7 nm to 10 nm, wherein when the monitored deposition thickness exceeds 10 nm, the co-evaporation process is stopped.

22. The ultra-thin transparent electromagnetic shielding film preparation device according to claim 17, characterized in that: The electromagnetic shielding film preparation device also includes: a correction baffle; The silver material is evaporated in co-evaporation deposition to form the silver particles, and the aluminum material is evaporated in co-evaporation deposition to form the aluminum particles; The correction baffle blocks most of the silver particles and most of the aluminum particles, allowing a small portion of the silver particles and a small portion of the aluminum particles to be deposited onto the shielding layer substrate, so that the first rate is lower than the evaporation rate at the evaporation source of the silver material, and the second rate is lower than the evaporation rate at the evaporation source of the aluminum material.

23. The ultra-thin transparent electromagnetic shielding film preparation device according to claim 22, characterized in that: The correction baffle is divided into guide plates located on both sides of the plate surface where the partition is located. The guide plates on both sides can be distributed obliquely upward in the direction of the plate surface where the partition is located, and a gap is formed between the guide plates on both sides. The formed gap is located above the partition, so that the silver particles and the aluminum particles contacting the guide plates can flow into the formed gap.

24. The ultra-thin transparent electromagnetic shielding film preparation device according to claim 17, characterized in that: The vacuum coating machine includes a 1300 type vacuum coating machine.

Citation Information

Patent Citations

  • Double-source metal codeposition method capable of suppressing silver agglomeration

    CN104593725A

  • Ultra-thin silver base thin film, multi-layer composite transparent electric conduction thin film and preparing method and application thereof

    CN107254664A

  • Preparation device and preparation method for metal composite material

    CN108060393A

  • Electromagnetic shielding curved-surface optical window based on ultrathin doped metal / medium composite structure

    CN112888288A

  • Film system with selective electromagnetic shielding and high transmittance and preparation method thereof

    CN115867008A