Battery lossless fluid infusion capacity-increasing repair method and device
Through the non-destructive rehydration method of inert gas protection, vacuum impregnation, differential pressure injection and helium leakage detection, combined with the redox medium to activate 'dead lithium', the problems of low safety and short life of battery rehydration are solved, and the battery efficiency is achieved Lossless fluid replenishment and capacity repair improves the capacity and life of the battery.
Patent Information
- Application Number
- CN202411058001.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
The existing battery rehydration technology has the problems of high safety risks, easy internal short circuits, and short service life. It also lacks effective lossless rehydration methods to improve the capacity and life of retired batteries.
The method of inert gas displacement of air, insulated needle pierces blind holes, vacuum pumping, pressure differential liquid injection, helium filling and airtightness detection after sealing is integrated, and the battery is activated by combining redox medium. The 'dead lithium' realizes the battery's lossless rehydration and capacity repair.
It reduces the safety risks during the rehydration process, improves the capacity and life of the battery, ensures the airtightness and repair effect of the battery, avoids the risks of air introduction and short circuit, and enhances the reuse value of the battery.
Smart Images

Figure CN118983545A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery repair and recycling, and in particular to a method and device for non-destructive battery liquid replenishment. Background Art
[0002] In recent years, the amount of retired power batteries has increased year by year and the data is huge. If the retired power batteries are not properly handled, it will cause environmental pollution, safety hazards and waste of resources. my country has issued a number of policies and regulations on capacity expansion and repair of retired power batteries to promote the development of high-value reuse technology for retired batteries. At present, the performance consistency of large-scale retired power batteries is poor, the capacity is obviously low, and the reuse value is insufficient.
[0003] Increasing the capacity of retired batteries by increasing the capacity of batteries and increasing the active lithium content of batteries is the key to increasing the capacity of retired lithium-ion batteries. The inactive lithium in the battery (also called "dead lithium") can be activated by adding redox media to react with the "dead lithium" to increase the active lithium content in the positive electrode material, thereby increasing the battery capacity. Taking the redox media SnI4 as an example, the principle of activating dead lithium by redox media in the electrolyte is: by adding soluble SnI4 to the lithium-ion electrolyte, with the help of I 3- / I - The redox couple undergoes a redox reaction with the dead lithium, converting the dead lithium generated during the cycle into active lithium. The chemical reaction formula involved in the reaction is:
[0004] SnI4+4Li=4LiI+Sn (1)
[0005] 2Li 1-x Ni 0.5 Co 0.2 Mn 0.3 O2+2xLi+3xI - =2LiNi 0.5 Co 0.2 Mn 0.3 O2+xI3 - (2)
[0006] I3 - + 2Li = 3I - + 2Li + (3)
[0007] The added SnI4 reacts with dead lithium to generate soluble LiI through reaction formula (1); LiI diffuses to the positive electrode and the lithium-deficient positive electrode active material Li 1-x Ni 0.5 Co 0.2 Mn 0.3 O2 is oxidized to I3 -(As shown in reaction equation (2)), the lithium content of the active material itself increases; the I3 generated at the positive electrode - It will diffuse to the negative electrode and further react with the "dead lithium" to generate soluble LiI. The above reaction process will be repeated until the dead lithium is completely activated.
[0008] The use of redox media to increase the capacity of retired batteries requires the use of refilling technology. However, the current refilling technology is not very mature. The battery cells that are repaired by refilling through direct punching are prone to internal short circuits, low safety, and short service life during use. Patent document CN114976332A uses a method of drilling blind holes in the battery to be repaired, and then directly refilling and sealing the blind holes with a steel needle. This method effectively avoids the risk of metal debris falling into the battery during the punching process and causing a short circuit in the battery. However, this method easily introduces moisture from the air, thereby limiting its injection environment. At the same time, the controllable injection of the battery and the airtightness inspection of the battery after sealing are not reflected in the patent. These are key factors that affect the battery repair effect. Summary of the invention
[0009] The technical problem to be solved by the present invention is to provide a method and device for non-destructive battery refilling, capacity expansion and repair, so as to reduce the safety risk of refilling and increase the capacity and life of the battery.
[0010] In order to solve the above problems, the present invention provides a battery non-destructive fluid replenishment and capacity expansion repair method, comprising the following steps:
[0011] S01: Introduce inert gas into the fluid replenishment system to replace air;
[0012] S02: Use an insulated needle to pierce the blind hole on the battery cover;
[0013] S03: Turn on the vacuum switch to evacuate the battery and the injection bottle to the same vacuum degree;
[0014] S04: Turn on the gas filling switch and fill the liquid filling bottle with inert gas to form a pressure difference between the liquid filling bottle and the battery;
[0015] S05: Turn on the injection switch, inject electrolyte with repair function into the battery and adjust the injection amount through the flow meter, and then turn off the injection switch;
[0016] S06: Turn on the inflation switch to fill the battery with helium;
[0017] S07: Pull out the insulating needle and seal the battery;
[0018] S08: Check the air tightness of the battery with a helium detector; perform a capacity test on the repaired battery after it is charged.
[0019] This method can well integrate inert gas protection, vacuum infiltration, differential pressure injection and subsequent helium leak detection to achieve non-destructive rehydration and repair of retired batteries.
[0020] Preferably, the battery to be repaired is a hard shell lithium ion battery, and the hard shell is preferably made of an aluminum shell, or a steel shell or a plastic shell; the battery type can be a lithium ion battery or a lithium metal battery, preferably a lithium ion battery.
[0021] Preferably, after the battery is placed in the tooling and fixed in S01, the insulating zirconium oxide needle is inserted into the sealing pin in the blind injection hole, and vacuuming and filling with inert gas are repeated three times. Optionally, the number of vacuuming times can be more than three times.
[0022] Preferably, in S02, the press machine clamps the needle and pierces the blind hole with a thickness of 0.2 to 1 mm at a displacement speed of 0.1 to 0.5 mm / s.
[0023] Preferably, in S03, the battery and the liquid injection bottle are evacuated to an internal pressure of 10 to 90 kPa, and after maintaining the pressure for 2 to 10 minutes, the evacuation switch is turned off.
[0024] Preferably, after the switch 5 is turned on in S04, an inert gas is filled into the liquid injection bottle to maintain the liquid injection pressure difference at 0.2-1 kPa. Preferably, the inert gas is helium, or high-purity argon.
[0025] Preferably, S05 injects liquid into the battery to be repaired, and controls the volume of the injected liquid according to a flow meter, and allows the battery to stand for 40 to 120 seconds after the injection.
[0026] Preferably, the electrolyte is a solvent for the electrolyte of the battery to be repaired, or a solvent for the electrolyte containing a redox medium, or a mixture of a solvent for the electrolyte and an electrolyte, or a mixture of a solvent for the electrolyte containing a redox medium and an electrolyte.
[0027] More preferably, the concentration of the electrolyte is 0.5 to 1.5 mol / L; the concentration of the redox medium is 2 to 10 mmol / L.
[0028] More preferably, the oxidation potential of the redox medium is lower than the charging cut-off voltage of the repaired battery, and the reduction potential is higher than the reduction potential of the positive electrode material in the repaired battery. The redox medium can well activate the inactive lithium in the retired battery and improve the battery capacity.
[0029] Furthermore, when the battery is a lithium iron phosphate / graphite battery, the redox medium is any one of an iodine-based compound (such as SnI4) or an organic substance with a suitable redox potential (such as TEMPO).
[0030] Preferably, in S06, switch four is closed and switch three is opened to inject helium into the repair battery.
[0031] Preferably, after the insulating needle is pulled out in S07, a sealing pin is pressed in to seal the battery. Preferably, laser welding sealing is performed.
[0032] Preferably, a helium detector is used in S08 to perform airtightness test on the sealed battery. Preferably, the sealed battery is placed in a helium-free environment for 5 to 30 minutes before the test.
[0033] The repaired batteries that have passed the air-tightness test are placed at 25℃~45℃ for 4h~24h for formation, and the rated capacity of the repaired batteries is tested using charging and discharging equipment.
[0034] The present invention also provides a battery non-destructive fluid replenishment and capacity expansion repair device, which includes an exhaust pipeline, an air charging pipeline, and a liquid injection pipeline connected to a battery to be repaired through a four-way pipe joint, the liquid injection pipeline is connected to a liquid injection bottle, the air charging pipeline is connected to a helium bottle and a liquid injection bottle respectively through a three-way pipe joint, and the exhaust pipeline is connected to a vacuum pump and a liquid injection bottle respectively through a three-way pipe joint.
[0035] Preferably, switch one, switch two, switch three and switch four are respectively provided between the four-way pipe joint and the battery to be repaired, three-way pipe joint two, three-way pipe joint one and the liquid injection bottle; switch five is provided between the three-way pipe joint one and the liquid injection bottle; switch six is provided between the three-way pipe joint two and the liquid injection bottle.
[0036] Preferably, a flow meter is provided on the liquid injection pipeline.
[0037] Preferably, the battery to be repaired is provided with an insulating needle for connecting a four-way pipe joint. The insulating needle can effectively prevent the battery from short-circuiting due to excessive needle displacement when puncturing the blind hole. The insulating needle is made of zirconium oxide, with an outer diameter of 1 to 2 mm and an inner diameter of 0.5 to 1 mm, which has the effect of puncturing the blind hole and injecting liquid for ventilation. Preferably, under the protection of a mechanical limit fixture, the needle pierces the blind hole at a speed of 0.1 to 0.5 mm / s.
[0038] More preferably, a sealing nail is provided between the insulating needle and the battery to be repaired. The sealing nail is made of rubber, has a diameter of 1 to 2.5 mm, is 0.1 to 0.5 mm (preferably 0.1 to 0.4 mm) larger than the diameter of the blind hole, and plays a role in sealing the gap between the needle and the injection hole.
[0039] The exhaust pipeline and the filling pipeline are used in the inert gas protection, pressure differential injection, vacuum infiltration, and helium filling process of the entire system, and the injection pipeline and flow meter are used to monitor the injection volume. It has been verified that the device can reduce the safety risks during the injection process and realize the non-destructive refilling and capacity expansion repair of retired batteries.
[0040] The present invention provides a non-destructive refilling method for lithium-ion batteries, which can achieve effective inert gas protection for perforated batteries and avoid the introduction of air into the battery during the injection process; at the same time, the battery can be evacuated, and the injection bottle is filled with inert gas to inject the battery through the pressure difference between the battery and the injection bottle; after the injection is completed, the battery is filled with helium for protection, in preparation for helium leak detection of the sealed battery; at the same time, the supplemented redox medium electrolyte can well activate the "dead lithium" in the battery. It has been verified that this method can reduce the safety risks during the injection process and achieve non-destructive refilling and capacity expansion repair of retired batteries.
[0041] The present invention can well integrate the refilling process flows such as inert gas protection, vacuum infiltration, pressure difference injection, and helium leak detection of sealed batteries by designing a non-destructive refilling device, while taking advantage of the "dead lithium" activation and capacity expansion effect of the redox repair electrolyte to achieve non-destructive refilling and repair of retired batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 A schematic diagram of a battery non-destructive fluid replenishment and capacity expansion repair device provided by the present invention;
[0043] Figure 2 The present invention provides a flow chart of the battery non-destructive fluid replenishment and capacity expansion repair method. DETAILED DESCRIPTION
[0044] In order to make the present invention more clearly understood, preferred embodiments are described in detail below with reference to the accompanying drawings.
[0045] like Figure 1 As shown, a non-destructive battery refilling and capacity expansion repair device provided by the present invention comprises an exhaust pipeline, an air charging pipeline, and a liquid injection pipeline connected to the battery to be repaired (1) through a four-way pipe joint (4), the liquid injection pipeline is connected to the liquid injection bottle (13), the exhaust pipeline is connected to the helium bottle (14) and the liquid injection bottle (13) through a three-way pipe joint (11), and the exhaust pipeline is connected to the vacuum pump (15) and the liquid injection bottle (13) through a three-way pipe joint (12). A flow meter (16) is provided on the liquid injection pipeline.
[0046] A switch 1 (5), a switch 2 (6), a switch 3 (7), and a switch 4 (8) are respectively arranged between the four-way pipe joint (4) and the battery to be repaired (1), the three-way pipe joint 2 (12), the three-way pipe joint 1 (11), and the liquid injection bottle (13); a switch 5 (9) is arranged between the three-way pipe joint 1 (11) and the liquid injection bottle (13); and a switch 6 (10) is arranged between the three-way pipe joint 2 (12) and the liquid injection bottle (13).
[0047] The battery to be repaired (1) is provided with an insulating needle (3) for connecting to a four-way pipe joint (4). A sealing nail (2) is provided between the insulating needle (3) and the battery to be repaired (1). The press machine (17) is used to pierce the blind hole on the battery to be repaired (1) with the insulating needle (3).
[0048] Example 1
[0049] In this embodiment, the sealing pin is made of rubber material and has a diameter of 2.3 mm, which is 0.3 mm larger than the diameter of the blind hole, and serves to seal the gap between the needle head and the injection hole.
[0050] The insulating needle is made of zirconium oxide, with an outer diameter of 1 mm and an inner diameter of 0.5 mm, which can puncture the blind hole and inject liquid for ventilation. Preferably, under the protection of the mechanical limit fixture, the needle punctures the blind hole at a speed of 0.1 mm / s.
[0051] The present embodiment provides a method for non-destructive rehydration of a lithium-ion battery, which specifically comprises the following steps:
[0052] S01: Filling of inert gas into the liquid replenishment system;
[0053] S02: Insulated needle pierces the blind hole;
[0054] S03: Vacuum the battery and the liquid filling bottle;
[0055] S04: Fill the injection bottle with inert gas;
[0056] S05: injecting liquid into the battery under pressure difference;
[0057] S06: The battery is filled with helium;
[0058] S07: Remove the needle and seal the battery;
[0059] S08: Check the air tightness of the battery after refilling.
[0060] The battery to be repaired is an aluminum shell lithium-ion battery. Preferably, after the battery to be repaired is placed in the tooling and fixed in S01, the insulating zirconium oxide needle is inserted into the sealing nail in the injection blind hole, and switch 1, switch 2, and switch 3 are turned on, and switch 4, switch 5, and switch 6 are turned off, and then vacuuming and filling with inert gas are repeated 3 times, and then switch 1, switch 2, and switch 3 are turned off. Optionally, the number of vacuuming times can be more than 3 times.
[0061] Preferably, in S02, the press clamps the needle and pierces the 0.5 mm thick blind hole at a displacement speed of 0.2 mm / s.
[0062] Preferably, in S03, switch one, switch two and switch six are turned on, and the battery and the liquid injection bottle are evacuated to an internal pressure of 70 kPa. After maintaining for 5 minutes, switch one, switch two and switch six are turned off.
[0063] Preferably, after the switch 5 is turned on in S04, an inert gas is filled into the liquid injection bottle to maintain the liquid injection pressure difference at 0.3 kPa. Preferably, the inert gas is high-purity argon.
[0064] Preferably, in S05, switch 1 and switch 4 are turned on, and liquid is injected into the battery to be repaired, and the volume of the injection amount is regulated by a flow meter, and the battery is left to stand for 60 seconds after injection. Preferably, the injected electrolyte is an electrolyte solvent, or an electrolyte solvent containing a redox medium. Preferably, the redox medium may be SnI4 or TEMPO, and the concentration of the redox medium is 5 mmol / L.
[0065] Preferably, in S06, the switch 4 is closed and the switch 3 is opened to inject an inert gas into the repair battery. Preferably, the inert gas is helium.
[0066] Preferably, after the insulating needle is pulled out in S07, a sealing pin is pressed in to seal the battery. Preferably, laser welding sealing is performed.
[0067] Preferably, a helium detector is used in S08 to perform air tightness test on the sealed battery. Preferably, the sealed battery is placed in a helium-free environment for 10 minutes before the test.
[0068] The repaired batteries that passed the air-tightness test were placed at 30°C for 12 hours for formation, and the rated capacity of the repaired batteries was tested using charging and discharging equipment.
[0069] Example 2
[0070] This embodiment provides a method for non-destructive liquid replenishment and capacity expansion repair of lithium iron phosphate square aluminum shell batteries, and the specific steps are as follows:
[0071] 1. Place the battery to be repaired, insert the insulated zirconium oxide needle into the sealing nail in the battery liquid injection blind hole, turn on switch 1, switch 2, switch 3, and close switch 4, switch 5, and switch 6. Repeat the vacuuming and filling with inert gas 3 times, and then close switch 1, switch 2, and switch 3.
[0072] 2. The press clamps the needle and pierces a blind hole with a thickness of 0.5 mm and a diameter of 1.5 mm at a displacement speed of 0.2 mm / s.
[0073] 3. Turn on switch 1, switch 2, and switch 3, evacuate the battery and the liquid injection bottle to an internal pressure of 70 kPa, maintain for 5 minutes, and then turn off switch 1, switch 2, and switch 6.
[0074] 4. After turning on switch five, fill the injection bottle with high-purity argon gas to maintain the injection pressure difference between the injection bottle and the battery at 0.3 kPa.
[0075] 5. Turn on switch 1 and switch 4 to inject liquid into the battery to be repaired, and adjust the volume of the injection according to the flow meter. After injection, let it stand for 60 seconds. The injected electrolyte is a mixture of an electrolyte solvent containing a redox medium SnI4 and an electrolyte, with a SnI4 concentration of 5mmol / L and an electrolyte concentration of 1mol / L.
[0076] 6. Turn off switch 4 and turn on switch 3 to inject helium into the repair battery.
[0077] 7. After pulling out the insulating needle, press in a 1.7mm diameter sealing aluminum nail and seal the battery by laser welding.
[0078] 8. Use a helium detector to test the air tightness of the sealed battery. Place the sealed battery in a helium-free environment for 10 minutes before testing.
[0079] The repaired batteries that passed the air-tightness test were placed at 30°C for 12 hours for formation, and the rated capacity of the repaired batteries was tested using charging and discharging equipment.
Claims
1. A battery non-destructive fluid replenishment and capacity expansion repair method, characterized in that: The following steps are involved: Step 1): Introducing an inert gas into the liquid replenishment system to replace the air; Step 2): Use an insulating needle to pierce the blind hole on the battery cover; Step 3): Turn on the vacuum switch and evacuate the battery and the injection bottle to the same vacuum degree; Step 4): Turn on the gas filling switch and fill the liquid filling bottle with inert gas to form a pressure difference between the liquid filling bottle and the battery; Step 5): Turn on the injection switch, inject electrolyte with repair function into the battery and adjust the injection amount through the flow meter, and turn off the injection switch; Step 6): Turn on the inflation switch to fill the battery with helium; Step 7): Pull out the insulating needle and seal the battery; Step 8): Check the air tightness of the battery using a helium detector; perform a capacity test on the repaired battery after it is charged.
2. The battery non-destructive fluid replenishment and capacity expansion repair method according to claim 1, characterized in that: The electrolyte is a solvent for the electrolyte of the battery to be repaired, or a solvent for the electrolyte containing a redox medium, or a mixture of a solvent for the electrolyte and an electrolyte.
3. The battery non-destructive fluid replenishment and capacity expansion repair method according to claim 2, characterized in that: The concentration of the electrolyte is 0.5-1.5 mol / L; the concentration of the redox medium is 2-10 mmol / L.
4. The battery non-destructive fluid replenishment and capacity expansion repair method according to claim 2, characterized in that: The oxidation potential of the redox medium is lower than the charge cut-off voltage, and the reduction potential is higher than the reduction potential of the positive electrode material.
5. The battery non-destructive fluid replenishment and capacity expansion repair method according to claim 4, characterized in that: When the battery is a lithium iron phosphate / graphite battery, the redox medium is an iodine-based compound or any one of organic substances with a suitable redox potential.
6. A battery non-destructive fluid replenishment and capacity expansion repair device, characterized in that: The invention comprises an exhaust pipeline, an air charging pipeline and a liquid injection pipeline which are connected to the battery to be repaired (1) through a four-way pipe joint (4); the liquid injection pipeline is connected to a liquid injection bottle (13); the exhaust pipeline is connected to a helium bottle (14) and a liquid injection bottle (13) through a three-way pipe joint (11); and the exhaust pipeline is connected to a vacuum pump (15) and a liquid injection bottle (13) through a two-way pipe joint (12).
7. The battery non-destructive liquid replenishment and capacity expansion repair device according to claim 6, characterized in that: A switch 1 (5), a switch 2 (6), a switch 3 (7), and a switch 4 (8) are respectively arranged between the four-way pipe joint (4) and the battery to be repaired (1), the three-way pipe joint 2 (12), the three-way pipe joint 1 (11), and the liquid injection bottle (13); a switch 5 (9) is arranged between the three-way pipe joint 1 (11) and the liquid injection bottle (13); and a switch 6 (10) is arranged between the three-way pipe joint 2 (12) and the liquid injection bottle (13).
8. The battery non-destructive fluid replenishment and capacity expansion repair device according to claim 6, characterized in that: A flow meter (16) is provided on the liquid injection pipeline.
9. The battery non-destructive liquid replenishment and capacity expansion repair device according to claim 6, characterized in that: The battery to be repaired (1) is provided with an insulating needle (3) for connecting to a four-way pipe joint (4).
10. The battery non-destructive liquid replenishment and capacity expansion repair device according to claim 9, characterized in that: A sealing nail (2) is provided between the insulating needle (3) and the battery to be repaired (1).
Citation Information
Cited By
Method for repairing capacity of secondary battery, secondary battery, and electric device
CN120432685A
Secondary battery capacity repair method, secondary battery, and electrical equipment
CN120432685B