Solid core-shell-shaped diesel oil hydrotreating catalyst with active phase loaded on selective shell layer and preparation method of solid core-shell-shaped diesel oil hydrotreating catalyst
By using mesoporous carbon@molecular sieve material with solid core-shell structure and metal-organic chelate in diesel hydrotreatment catalyst, the orderly connection between hydrorefining and hydrocracking functions is achieved, and the existing technology is solved The problem of insufficient functional coordination has improved the efficiency and product quality of diesel hydrotreatment.
Patent Information
- Application Number
- CN202411330965.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-24
AI Technical Summary
In the existing diesel hydrotreatment catalysts, the hydrorefining and hydrocracking functions lack coordination on the microscopic scale, resulting in poor catalytic effect, and the acidic support mixed with other support in disorder, making it impossible to fully exert the coordination role of the two.
Using mesoporous carbon@molecular sieve material with solid core-shell structure as a carrier, metal-organic chelates are formed with Ni and Mo through 4-nitrophenyl thiol and ethylenediamine, and metal active components are selectively supported to mesoporous In the carbon pores, a selective shell-supported metal phase catalyst with clear functional boundaries and orderly connections are formed.
The orderly connection between hydrorefining and hydrocracking functions is achieved, the efficiency of diesel hydrotreatment is improved, excessive cracking caused by agglomeration of acid carriers is avoided, and liquid yield and diesel quality are improved.
Smart Images

Figure CN118988383A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of diesel hydrogenation catalysts, in particular to a solid core-shell diesel hydrogenation treatment catalyst with a selective shell layer loaded with a metal phase and a preparation method thereof. Background Art
[0002] The purpose of diesel hydroprocessing to prepare clean diesel is to remove sulfur, denitrogen and aromatize to the maximum extent and to improve the cetane number. The most critical thing is to select a targeted and efficient catalyst. At present, hydrodesulfurization, denitrogenation and aromatization and improving the cetane number are achieved through the hydrorefining function and hydrocracking function in the catalyst respectively. The former uses metal catalysts to hydrogenate and saturate aromatics to generate cycloalkanes while removing sulfur and denitrogen, and the latter uses acidic catalysts to open the ring and crack cycloalkanes.
[0003] At present, the three main processes used in industrial applications are to load two catalysts in separate beds in a single reactor (single-stage dual-dose), to load two catalysts in two reactors (dual-stage dual-dose), or to load a single catalyst in a single reactor (single-stage single-dose), but the disadvantages are obvious. In the first two processes, the catalyst and equipment costs are high, the process flow is complicated, and the hydrorefining function and hydrocracking function in the catalyst do not fully play a coordinated role at the microscopic scale. In the latter process, the acidic carrier (such as molecular sieve) and other carriers (such as alumina or carbon) in the catalyst are disorderly mixed, resulting in the hydrorefining function and hydrocracking function in the catalyst also being in disordered contact at the microscopic scale, and the coordination between the two cannot be fully exerted. Therefore, it is particularly urgent to develop a multifunctional coupling catalyst that orderly connects the hydrorefining and hydrocracking functions.
[0004] CN115646534B silanizes a microporous molecular sieve, forms a carbon coating on the outer surface of the molecular sieve using ethyl orthosilicate and dopamine, and further undergoes calcination, HF etching, and drying and calcination again to obtain a mesoporous carbon@molecular sieve material with a solid core-shell structure. The mesoporous carbon@molecular sieve material with a solid core-shell structure provided by the invention combines mesoporous carbon and molecular sieve in an orderly manner to form a core-shell single particle material with a uniform structure and a distinct inner and outer boundary.
[0005] The present invention is based on CN115646534B, and by virtue of the chemical reaction of 4-nitrobenzene mercaptan, ethylenediamine, Ni and Mo to form a metal-organic chelate, the molecular volume of the metal active component in the solution is increased, the active component is selectively loaded into the mesoporous channels of the mesoporous carbon, and the loading behavior in the microporous molecular sieve channels is restricted, thereby obtaining a solid core-shell diesel hydroprocessing catalyst with a selective shell-loaded metal phase, in which the functional domains of hydrorefining and hydrocracking are clearly distinguished and orderly connected. Summary of the invention
[0006] The invention provides a solid core-shell diesel hydroprocessing catalyst with a selective shell loaded metal phase and a preparation method thereof, which solves the problem of orderly connection between hydrofining and hydrocracking functions in a diesel hydroprocessing catalyst.
[0007] The technical solution of the present invention is as follows:
[0008] The invention provides a solid core-shell diesel hydroprocessing catalyst with a selective shell-loaded metal phase, wherein Ni-Mo is used as an active component, 4-nitrobenzene mercaptan and ethylenediamine are used as chelating agents, and a mesoporous carbon@molecular sieve material with a solid core-shell structure is used as a carrier, and the loading amount of the active component in the catalyst is 15-25%.
[0009] As a further technical solution, the mesoporous carbon@molecular sieve material with a solid core-shell structure is prepared by the following method: mixing a microporous molecular sieve, trimethylchlorosilane and toluene, reacting in a microwave, filtering, washing and drying to obtain a silanized molecular sieve, dispersing the silanized molecular sieve in a mixture of anhydrous ethanol, ammonia water and water, adding tetraethyl orthosilicate and dopamine, stirring with a microwave, centrifuging, washing, drying and calcining in nitrogen to obtain a solid powder, then treating the solid powder with an HF solution, filtering, washing, drying and calcining to obtain a mesoporous carbon@molecular sieve material with a solid core-shell structure.
[0010] As a further technical solution, the solution impregnation refers to: adding the nickel salt, 4-nitrobenzene mercaptan and ethylenediamine into water, stirring and dissolving to obtain solution A, adding the molybdenum salt, 4-nitrobenzene mercaptan and ethylenediamine into water, stirring and dissolving to obtain solution B, and impregnating the carrier in the solution A and solution B in order, filtering, drying and calcining.
[0011] As a further technical solution, the molar ratio of 4-nitrobenzenethiol to ethylenediamine is 2:1.
[0012] As a further technical solution, the calcination conditions of the carrier after impregnation, filtration and drying in the solution A are calcination at 400-450°C in the air for 1-2h, and the calcination conditions of the carrier after impregnation, filtration and drying in the solution B are calcination at 400-450°C in 10% H2S / nitrogen for 3-5h. The drying conditions are both drying at 80-100°C in the air for 3-5h.
[0013] As a further technical solution, the mass ratio of Ni to Mo in the active component is (2-4): (6-9).
[0014] The basic principle of the present invention is: the mesoporous carbon@molecular sieve carrier with a solid core-shell structure is a single core-shell particle with a uniform structure and a distinct inner and outer boundary. The core is a microporous molecular sieve with a pore size of about 0.65nm, and the shell is a mesoporous carbon with a pore size greater than 5nm. By means of the chemical reaction of metal-organic chelates formed between 4-nitrobenzene mercaptan, ethylenediamine, Ni and Mo, the molecular volume of the metal active component in the solution is increased, and the active component is selectively loaded into the mesoporous channels of the mesoporous carbon, limiting its loading behavior in the microporous molecular sieve channels, and obtaining a solid core-shell diesel hydroprocessing catalyst with a selective shell-loaded metal phase, in which the hydrorefining and hydrocracking functional domains are clearly distinguished and orderly connected. In the catalyst, the shell region of the mesoporous carbon loaded with active components performs the functions of hydrodesulfurization, denitrogenation and dearomatization on the sulfur-containing and nitrogen-containing compounds and aromatic compounds in diesel, and the molecular sieve core performs the isomerization and cracking effects on the desulfurized, denitrogenated and dearomatized alkanes and cycloalkanes transferred from the shell region to improve the cetane number.
[0015] Compared with the prior art, the solid core-shell diesel hydroprocessing catalyst with a selective shell-loaded metal phase provided by the present invention is a core-shell single catalyst that isolates the hydrorefining function and the hydrocracking function in different regions but connects them in an orderly manner. The use of the catalyst for diesel hydroprocessing reaction is conducive to further revealing the transmission mechanism of the probe molecule and the reaction relay mechanism in different functional zones, and is conducive to a deep understanding of the structure-activity relationship between the catalyst microstructure and the macroscopic performance of hydrogenation. The catalyst can also avoid the over-cracking phenomenon caused by the agglomeration of the acidic carrier, which is conducive to improving the liquid yield after diesel hydroprocessing. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a comparative evaluation result diagram of the catalytic effects of Catalyst 5 prepared in Example 5 and three control catalysts. DETAILED DESCRIPTION
[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] Example 1: A solid core-shell diesel hydroprocessing catalyst with a selective shell-loaded metal phase is prepared by the following method: (1) 1.0 g HY molecular sieve, 30 g trimethylchlorosilane, and 20 g toluene are mixed evenly, microwaved at 30°C for 4 h, filtered, washed with anhydrous ethanol until there is no chloride ion, and dried at 100°C to obtain a silanized HY molecular sieve. 0.12 g silanized HY molecular sieve is dispersed in a mixture of 10 ml anhydrous ethanol and 40 ml water, and stirred at room temperature for 20 min. 0.5 ml ammonia water is added dropwise and stirred for 10 min. 0.5 ml ethyl orthosilicate and 0.6 g dopamine are then added dropwise and microwaved for 12 h. Washed by centrifugation 3 times, dried at 60°C, and a brown powder is obtained. The temperature is increased to 200°C (constant temperature for 0.5 h) at 10°C / min under argon protection, and then increased to 800°C (constant temperature for 3 h) at 3°C / min to obtain a black powder. The above materials were added into 10 ml 2% HF solution and stirred for 10 min. Both sides were washed by centrifugation, dried at 100 °C, and calcined at 450 °C for 2 h to obtain a mesoporous carbon@molecular sieve carrier with a solid core-shell structure.
[0019] (2) Add 0.25 g of nickel acetate, 0.31 g of 4-nitrobenzene mercaptan and 0.06 g of ethylenediamine to 2.5 ml of water and stir to dissolve to obtain solution A. Add 0.28 g of ammonium molybdate, 0.44 g of 4-nitrobenzene mercaptan and 0.09 g of ethylenediamine to 2.5 ml of water and stir to dissolve to obtain solution B.
[0020] (3) 0.74 g of a mesoporous carbon@molecular sieve carrier with a solid core-shell structure was placed in solution A and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in air at 450°C for 2 h. The carrier was then placed in solution B and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in nitrogen with a hydrogen sulfide content of 10% by volume at 450°C for 4 h to obtain a solid core-shell diesel hydrotreating catalyst with a selective shell-loaded metal phase.
[0021] Example 2: A solid core-shell diesel hydroprocessing catalyst with a selective shell-loaded metal phase is prepared by the following method: (1) 1.0 g of Beta molecular sieve, 30 g of trimethylchlorosilane, and 20 g of toluene are mixed evenly, microwaved at 30°C for 4 h, filtered, washed with anhydrous ethanol until there is no chloride ion, and dried at 100°C to obtain silanized Beta molecular sieve. 0.12 g of silanized Beta molecular sieve is dispersed in a mixture of 10 ml of anhydrous ethanol and 40 ml of water, and stirred at room temperature for 20 min. 0.5 ml of ammonia water is added dropwise and stirred for 10 min. 0.5 ml of ethyl orthosilicate and 0.6 g of dopamine are added dropwise and microwaved for 12 h. Washed by centrifugation 3 times, dried at 60°C, and brown powder is obtained. Under argon protection, the temperature is increased to 200°C at 10°C / min (maintained at a constant temperature for 0.5 h), and then increased to 800°C at 3°C / min (maintained at a constant temperature for 3 h), to obtain black powder. The above materials were added into 10 ml 2% HF solution and stirred for 10 min. Both sides were washed by centrifugation, dried at 100 °C, and calcined at 450 °C for 2 h to obtain a mesoporous carbon@molecular sieve carrier with a solid core-shell structure.
[0022] (2) Add 0.25 g of nickel acetate, 0.31 g of 4-nitrobenzene mercaptan and 0.06 g of ethylenediamine to 2.5 ml of water and stir to dissolve to obtain solution A. Add 0.28 g of ammonium molybdate, 0.44 g of 4-nitrobenzene mercaptan and 0.09 g of ethylenediamine to 2.5 ml of water and stir to dissolve to obtain solution B.
[0023] (3) 0.74 g of a mesoporous carbon@molecular sieve carrier with a solid core-shell structure was placed in solution A and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in air at 450°C for 2 h. The carrier was then placed in solution B and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in nitrogen with a hydrogen sulfide content of 10% by volume at 450°C for 4 h to obtain a solid core-shell diesel hydrotreating catalyst with a selective shell-loaded metal phase.
[0024] Example 3: A solid core-shell diesel hydroprocessing catalyst with a selective shell-loaded metal phase is prepared by the following method: (1) 1.0 g HZSM-5 molecular sieve, 30 g trimethylchlorosilane, and 20 g toluene are mixed evenly, microwaved at 30°C for 4 h, filtered, washed with anhydrous ethanol until there is no chloride ion, and dried at 100°C to obtain a silanized HZSM-5 molecular sieve. 0.12 g of the silanized HZSM-5 molecular sieve is dispersed in a mixture of 10 ml anhydrous ethanol and 40 ml water, and stirred at room temperature for 20 min. 0.5 ml of ammonia water is added dropwise and stirred for 10 min. 0.5 ml of ethyl orthosilicate and 0.6 g of dopamine are added dropwise and microwaved for 12 h. Wash by centrifugation for 3 times, dry at 60℃ to obtain brown powder, and heat to 200℃ (maintain temperature for 0.5 h) at 10℃ / min under argon protection, and heat to 800℃ (maintain temperature for 3 h) at 3℃ / min to obtain black powder. Add the above materials to 10 ml 2% HF solution and stir for 10min. Wash both sides by centrifugation, dry at 100℃, and calcine at 450℃ for 2h to obtain a mesoporous carbon@molecular sieve carrier with a solid core-shell structure.
[0025] (2) Add 0.25 g of nickel acetate, 0.31 g of 4-nitrobenzene mercaptan and 0.06 g of ethylenediamine to 2.5 ml of water and stir to dissolve to obtain solution A. Add 0.28 g of ammonium molybdate, 0.44 g of 4-nitrobenzene mercaptan and 0.09 g of ethylenediamine to 2.5 ml of water and stir to dissolve to obtain solution B.
[0026] (3) 0.74 g of a mesoporous carbon@molecular sieve carrier with a solid core-shell structure was placed in solution A and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in air at 450°C for 2 h. The carrier was then placed in solution B and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in nitrogen with a hydrogen sulfide content of 10% by volume at 450°C for 4 h to obtain a solid core-shell diesel hydrotreating catalyst with a selective shell-loaded metal phase.
[0027] Example 4: A solid core-shell diesel hydroprocessing catalyst with a selective shell-loaded metal phase is prepared by the following method: (1) 1.0 g HY molecular sieve, 30 g trimethylchlorosilane, and 20 g toluene are mixed evenly, microwaved at 30°C for 4 h, filtered, washed with anhydrous ethanol until there is no chloride ion, and dried at 100°C to obtain silanized HY molecular sieve. 0.12 g silanized HY molecular sieve is dispersed in a mixture of 10 ml anhydrous ethanol and 40 ml water, and stirred at room temperature for 20 min. 0.5 ml ammonia water is added dropwise and stirred for 10 min. 0.5 ml ethyl orthosilicate and 0.6 g dopamine are added dropwise and microwaved for 12 h. Washed by centrifugation 3 times, dried at 60°C, and brown powder is obtained. Under argon protection, the temperature is increased to 200°C at 10°C / min (maintained at a constant temperature for 0.5 h), and then increased to 800°C at 3°C / min (maintained at a constant temperature for 3 h), to obtain black powder. The above materials were added into 10 ml 2% HF solution and stirred for 10 min. Both sides were washed by centrifugation, dried at 100 °C, and calcined at 450 °C for 2 h to obtain a mesoporous carbon@molecular sieve carrier with a solid core-shell structure.
[0028] (2) Add 0.21 g of nickel acetate, 0.29 g of 4-nitrobenzene mercaptan and 0.05 g of ethylenediamine to 2.5 ml of water and stir to dissolve to obtain solution A. Add 0.33 g of ammonium molybdate, 0.48 g of 4-nitrobenzene mercaptan and 0.10 g of ethylenediamine to 2.5 ml of water and stir to dissolve to obtain solution B.
[0029] (3) 0.74 g of a mesoporous carbon@molecular sieve carrier with a solid core-shell structure was placed in solution A and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in air at 450°C for 2 h. The carrier was then placed in solution B and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in nitrogen with a hydrogen sulfide content of 10% by volume at 450°C for 4 h to obtain a solid core-shell diesel hydrotreating catalyst with a selective shell-loaded metal phase.
[0030] Example 5: A solid core-shell diesel hydroprocessing catalyst with a selective shell-loaded metal phase is prepared by the following method: (1) 1.0 g HY molecular sieve, 30 g trimethylchlorosilane, and 20 g toluene are mixed evenly, microwaved at 30°C for 4 h, filtered, washed with anhydrous ethanol until there is no chloride ion, and dried at 100°C to obtain a silanized HY molecular sieve. 0.12 g silanized HY molecular sieve is dispersed in a mixture of 10 ml anhydrous ethanol and 40 ml water, and stirred at room temperature for 20 min. 0.5 ml ammonia water is added dropwise and stirred for 10 min. 0.5 ml ethyl orthosilicate and 0.6 g dopamine are added dropwise and microwaved for 12 h. Washed by centrifugation 3 times, dried at 60°C, and brown powder is obtained. The temperature is increased to 200°C (constant temperature for 0.5 h) at 10°C / min under argon protection, and then increased to 800°C (constant temperature for 3 h) at 3°C / min to obtain a black powder. The above materials were added into 10 ml 2% HF solution and stirred for 10 min. Both sides were washed by centrifugation, dried at 100 °C, and calcined at 450 °C for 2 h to obtain a mesoporous carbon@molecular sieve carrier with a solid core-shell structure.
[0031] (2) Add 0.25 g of nickel acetate, 0.31 g of 4-nitrobenzene mercaptan and 0.06 g of ethylenediamine to 2.5 ml of water and stir to dissolve to obtain solution A. Add 0.28 g of ammonium molybdate, 0.44 g of 4-nitrobenzene mercaptan and 0.09 g of ethylenediamine to 2.5 ml of water and stir to dissolve to obtain solution B.
[0032] (3) 0.74 g of a mesoporous carbon@molecular sieve carrier with a solid core-shell structure was placed in solution A and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in air at 400°C for 1 h. The carrier was then placed in solution B and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in nitrogen with a hydrogen sulfide content of 10% by volume at 400°C for 2 h to obtain a solid core-shell diesel hydrotreating catalyst with a selective shell-loaded metal phase.
[0033] Example 6: A control catalyst is prepared by the following method: (1) Add 0.25 g of nickel acetate to 2.5 ml of water, stir and dissolve to obtain solution A, and add 0.28 g of ammonium molybdate to 2.5 ml of water, stir and dissolve to obtain solution B.
[0034] (2) 0.74 g of mesoporous carbon CMK-3 was placed in solution A and stirred at room temperature for 12 h, filtered, dried in air at 100 °C for 3 h, and calcined in air at 400 °C for 1 h. The solution was then placed in solution B and stirred at room temperature for 12 h, filtered, dried in air at 100 °C for 3 h, and calcined in nitrogen with a hydrogen sulfide content of 10% by volume at 400 °C for 2 h to obtain control catalyst 1.
[0035] Example 7: A control catalyst is prepared by the following method: (1) Add 0.25 g of nickel acetate to 2.5 ml of water, stir and dissolve to obtain solution A, and add 0.28 g of ammonium molybdate to 2.5 ml of water, stir and dissolve to obtain solution B.
[0036] (2) 0.74 g of HY molecular sieve was placed in solution A and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in air at 400°C for 1 h. The solution was then placed in solution B and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in nitrogen with a hydrogen sulfide content of 10% by volume at 400°C for 2 h to obtain control catalyst 2.
[0037] Example 8: A control catalyst is prepared by the following method: (1) HY type molecular sieve and mesoporous carbon CMK-3 (mass ratio is 1:3) are carefully ground in an agate mortar and mixed evenly to obtain a mixed carrier.
[0038] (2) Add 0.25 g of nickel acetate to 2.5 ml of water and stir to dissolve to obtain solution A. Add 0.28 g of ammonium molybdate to 2.5 ml of water and stir to dissolve to obtain solution B.
[0039] (3) 0.74 g of the mixed carrier was placed in solution A and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in air at 400°C for 1 h. The mixed carrier was then placed in solution B and stirred at room temperature for 12 h, filtered, dried in air at 100°C for 3 h, and calcined in nitrogen containing 10% by volume of hydrogen sulfide at 400°C for 2 h to obtain control catalyst 3.
[0040] Example 9: This example evaluates the catalyst 5, the control catalyst 1, the control catalyst 2 and the control catalyst 3 provided in the above examples, and the device used is a 100mL small-scale kettle evaluation device. 1.4 g of catalyst was loaded into the reactor, and the temperature was gradually raised to 300 ° C under a hydrogen atmosphere. The feedstock oil is a toluene solution of dibenzothiophene, in which the mass ratio of dibenzothiophene is 5%. The reaction conditions are: reaction pressure 4.0 MPa, reaction temperature 300 ° C, reaction time 72h. The comparative evaluation results of the catalytic effects of catalyst 5, control catalyst 1, control catalyst 2 and control catalyst 3 are shown in Table 1. It can be seen from Table 1 that the conversion rate of dibenzothiophene provided by the catalyst of the present invention is higher than that of the control catalyst, and the yield and selectivity of cyclohexylbenzene (CHB) are also higher than those of the control catalyst, indicating that the catalyst provided by the present invention is more conducive to the removal of dibenzothiophene, more conducive to the hydrogenation path reaction of dibenzothiophene, and is conducive to improving the cetane number of diesel products and improving the quality of diesel products.
[0041] Table 1 Comparative evaluation results of the catalytic effects of the catalyst prepared in Example 5 and three control catalysts.
[0042] catalyst Conversion rate of dibenzothiophene CHB selectivity CHB yield Catalyst 5 90.4 95.4 80.2 Comparative Catalyst 1 57.2 63.2 57 Comparative Catalyst 2 63.9 11.3 6.4 Comparative Catalyst 3 83.5 89.1 72.5
Claims
1. A solid core-shell diesel hydroprocessing catalyst with a selective shell-loaded metal phase, It is characterized in that Ni and Mo are used as active components, 4-nitrobenzene mercaptan and ethylenediamine are used as chelating agents, and a mesoporous carbon@molecular sieve material with a solid core-shell structure is used as a carrier. The active components and the chelating agent are loaded on the carrier by a solution impregnation method, and the catalyst is obtained by filtering, drying, and roasting. The loading amount of the active components in the catalyst is 15%-25%. The solution impregnation method refers to: adding the nickel salt, 4-nitrobenzene mercaptan and ethylenediamine into water, stirring and dissolving to obtain solution A; The molybdenum salt, 4-nitrobenzene mercaptan and ethylenediamine are added into water, stirred and dissolved to obtain solution B; the carrier is immersed in solution A and solution B respectively in the order of immersion, filtration, drying and roasting.
2. The diesel hydrotreating catalyst according to claim 1, It is characterized in that The mass ratio of Ni to Mo in the active component is (2-4): (6-9).
3. The diesel hydrotreating catalyst according to claim 1, It is characterized in that The molar ratio of the 4-nitrobenzenethiol to ethylenediamine is 2:
1.
4. The diesel hydrotreating catalyst according to claim 1, It is characterized in that The carrier is immersed in the solution A, filtered, and dried, and then calcined at 400°C-450°C in air for 1-2 hours. The carrier is immersed in the solution B, filtered, and dried, and then calcined at 400°C-450°C in nitrogen with a hydrogen sulfide volume content of 10% for 3-5 hours. The drying conditions are both 80°C-100°C in air for 3-5 hours.
Citation Information
Patent Citations
A method for preparing a core-shell mesoporous carbon@molecular sieve composite material
CN115646534B
High activity supported distillate hydroprocessing catalysts
CN101563437A
Catalyst for hydro-denitrification of inferior heavy distillate oil and preparation method and application of catalyst
CN103212432A
Preparation method and application of efficient catalyst used for organic sulfur hydrogenation conversion
CN107486223A
Preparation method of core-shell mesoporous carbon-coated molecular sieve composite material
CN115646534A