Heat treatment method for realizing ultrahigh strength of aluminum bronze alloy
By adopting multi-stage heat treatment methods in aluminum bronze alloys, including high-temperature, low-temperature heat treatment and electrical pulse treatment, the problem that the prior art is difficult to improve plastic toughness while maintaining high strength and hardness, and QAl11-6-6 aluminum is realized The ultra-high strength and good plastic toughness of bronze alloys meet the material needs of special working conditions.
Patent Information
- Application Number
- CN202411117421.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The existing aluminum-bronze alloy heat treatment methods are difficult to improve their plastic toughness while maintaining high strength and hardness. Especially in QAl11-6-6 aluminum bronze, conventional solid solution + aging methods cannot achieve both yield strength and tensile strength. Ultra-high strength above 1000MPa and also has good plastic toughness.
A special heat treatment method is adopted, including two high-temperature heat treatment, one low-temperature heat treatment and one electrical pulse treatment. The specific steps are: the first high-temperature heat treatment is between 850 and 950℃, the second high-temperature heat treatment is between 750 and 850℃, and the low-temperature heat treatment is between 750 and 850℃, and the low-temperature The heat treatment is between 450 and 550°C and the electric pulse treatment is finally carried out at 500°C. Through these steps, the solid solution and phase change of elements in the alloy are promoted, and the strength and plasticity of the alloy are improved.
The yield strength and tensile strength of QAl11-6-6 aluminum bronze alloy are achieved above 1000MPa, and the elongation after break reaches more than 5.0%, which significantly improves the strength and toughness of the material and meets the material needs under special working conditions.
Smart Images

Figure CN118996298A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal processing of copper alloy materials, and in particular relates to a special heat treatment method for achieving ultra-high strength of aluminum bronze alloy. Background Art
[0002] High alloyed QAl11-6-6 aluminum bronze has the strength, hardness and wear resistance of high-strength steel, while its corrosion resistance, oleophilic lubrication, heat dissipation and other properties are better than those of high-strength steel. Ultra-high strength QAl11-6-6 aluminum bronze with yield strength and tensile strength of more than 1000MPa is usually used to replace imports and is used to manufacture key structural parts under special working conditions such as heavy load, heavy pressure, strong wear and strong corrosion, solving the problem of key materials. QAl11-6-6 aluminum bronze is a heat-treatable copper alloy, and the "solid solution + aging" heat treatment method is generally used to improve its strength and hardness. However, in order to make the yield strength and tensile strength of the alloy parts reach ultra-high strength of more than 1000MPa, and at the same time have good plastic toughness (elongation after fracture is not less than 3.5%), it is impossible to achieve this by conventional "solid solution + aging" heat treatment method. By further increasing the content of Al, Fe, and Ni alloy elements, the strength and hardness of the alloy can be improved, but its plasticity and toughness will be significantly reduced, which will bring great difficulties to hot working and machining. Therefore, my country still mainly relies on imports for ultra-high strength aluminum bronze materials required under some special working conditions. How to develop a special heat treatment based on the existing QAl11-6-6 aluminum bronze composition to achieve ultra-high strength performance and meet the needs of special working conditions has become a difficult problem that the industry urgently needs to solve. Summary of the invention
[0003] The purpose of the present invention is to provide a heat treatment method for achieving ultra-high strength of QAl11-6-6 aluminum bronze alloy, so as to solve key material problems under special working conditions in important fields of my country.
[0004] The present invention provides a heat treatment method for achieving ultra-high strength of QAl11-6-6 aluminum bronze alloy, which comprises four steps of two high-temperature heat treatments, one low-temperature heat treatment and one electric pulse treatment. The operation method is as follows:
[0005] Step 1: Cut the extruded or centrifugally cast QAl11-6-6 aluminum bronze alloy tube and rod into fixed lengths or machine them into parts, put them into a resistance furnace heated to 850-950℃ and keep them warm for 0.5-2.0 hours for the first high-temperature heat treatment, and immediately quench and cool them in room temperature water after taking them out of the furnace.
[0006] Step 2: Place the QAl11-6-6 aluminum bronze alloy tubes and bars or machined parts that have undergone the first high-temperature heat treatment in a resistance furnace heated to (750-850)°C for 2-4 hours for the second high-temperature heat treatment, and air cool after being taken out of the furnace;
[0007] Step 3: Place the QAl11-6-6 aluminum bronze alloy tubes and bars or machined parts that have undergone the second high-temperature heat treatment in a resistance furnace heated to (450-550)°C for 2-4 hours for low-temperature heat treatment, and air cool after being taken out of the furnace;
[0008] Step 4: The QAl11-6-6 aluminum bronze alloy tube, bar or machined parts that have undergone low temperature heat treatment are subjected to an electric pulse treatment at 500°C × (1-8) min, followed by air cooling.
[0009] Preferably, the first high-temperature heat treatment parameters in step 1 are: keeping warm in a resistance furnace at 880-920°C for 0.5-1.0 hour, and quenching and cooling in room temperature water immediately after taking out of the furnace.
[0010] Preferably, the second high temperature heat treatment parameters in step 2 are: keeping warm in a resistance furnace at 780-820° C. for 2.5-3.3 hours, and air cooling after exiting the furnace.
[0011] Preferably, the low temperature heat treatment parameters in step 3 are: keeping warm in a resistance furnace at 480-520° C. for 2-3 hours, and air cooling after exiting the furnace.
[0012] Preferably, the electric pulse treatment parameters in step 4 are: the QAl11-6-6 aluminum bronze alloy tube, rod or machined part that has undergone low-temperature heat treatment is subjected to another electric pulse treatment at 500°C × (3 to 5) min, followed by air cooling after treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0014] Figure 1 is the metallographic structure of the sample of Example 1 of the present invention;
[0015] Figure 2 This is the metallographic structure of the sample of Example 2 of the present invention;
[0016] Figure 3 This is the metallographic structure of the sample of Comparative Example 1 of the present invention;
[0017] Figure 4 This is the metallographic structure of the sample of Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0018] The technical principle of the present invention is briefly described as follows: the extruded or centrifugally cast QAl11-6-6 aluminum bronze alloy tube and bar is cut into fixed lengths or machined into parts, and a first high-temperature short-time heat treatment is performed at 850-950°C for 0.5-1.0 hours to promote the decomposition of the second phase in the alloy and make the solute atoms in the alloy solid-dissolve in the copper matrix; then a second high-temperature long-time heat treatment is performed at (750-850)°C for 2-4 hours to promote the full solid-dissolution of alloy elements such as Al, Fe, and Ni in the copper matrix; after solid-dissolution, the alloy is immediately taken out of the furnace and quenched in room temperature water to strongly inhibit the high-temperature precipitation of the second phase in the alloy, thereby obtaining a supersaturated solid solution. Subsequently, the alloy is subjected to a low-temperature heat treatment at (450-550)°C for 2-4 hours, which can not only eliminate the quenching stress in the alloy, but also make the strengthening phase in the alloy uniformly dispersed and fully precipitated, thereby improving the strength of the alloy. After the first three steps of treatment, the yield strength of the alloy can reach 950-1000MPa, while the elongation after fracture is less than 3%, failing to achieve the expected ultra-high strength and good plasticity and toughness. Therefore, the alloy needs to be subjected to a special electric pulse treatment. The alloy is treated with an electric pulse at 500℃×(1-8)min, which causes the alloy to undergo a phase change, and more iron-rich κ phase precipitates from the α phase and is arranged along the direction of the current, thereby increasing the tensile strength of the alloy and effectively improving the plasticity of the alloy, so that the tensile strength and yield strength of the alloy both reach more than 1000MPa, and the elongation after fracture reaches more than 5.0%.
[0019] The present invention provides a heat treatment method for achieving ultra-high strength of QAl11-6-6 aluminum bronze alloy. Compared with the existing heat treatment process of aluminum bronze alloy, the main features and advantages are: the process is simple and controllable, and the electric pulse treatment technology is introduced into the heat treatment of the alloy, so that the strengthening phase in the alloy is fully utilized, the alloy strength is effectively improved, and the strength and toughness matching of the alloy are improved. The QAl11-6-6 aluminum bronze tube bar or machined parts prepared by the special heat treatment method of the present invention have a tensile strength of 1116MPa, a yield strength of 1021MPa, and an elongation after fracture of 5.9%. It not only achieves ultra-high strength performance, but also has good strength and toughness matching, can replace imports, and provide materials for manufacturing key structural parts under special working conditions such as heavy load, heavy pressure, strong wear, and strong corrosion.
[0020] The following is a specific description of the principles and features of the present invention. The examples given are only used to explain the present invention to make the above and other purposes, features and other advantages of the present invention clearer, and are not used to limit the scope of application of the present invention.
[0021] Example 1
[0022] QAl11-6-6 aluminum bronze alloy, the mass percentage of each element is: Al: 10.80%, Fe: 6.07%, Ni+Co: 6.22%, inevitable impurities: <0.5%, balance: Cu. It is melted and extruded into rods according to conventional processes, and the extruded rod specification is φ16mm. The heat treatment process is as follows:
[0023] (1) The extruded QA11-6-6 aluminum bronze alloy rod was placed in a resistance furnace heated to 860°C for 1.5 hours for high temperature heat treatment, and immediately quenched and cooled in room temperature water after being taken out of the furnace.
[0024] (2) The QAl11-6-6 aluminum bronze alloy tubes and bars or machined parts that have undergone the first high-temperature heat treatment are placed in a resistance furnace heated to 750°C for 2 hours for a second high-temperature heat treatment, and then air-cooled after being taken out of the furnace;
[0025] (3) The QAl11-6-6 aluminum bronze alloy tube and rod that has undergone the second high-temperature heat treatment is placed in a resistance furnace heated to 500°C for 2.5 hours for low-temperature heat treatment, and then air-cooled after being taken out of the furnace.
[0026] (4) The QAl11-6-6 aluminum bronze alloy tube, bar or machined parts that have undergone low temperature heat treatment are subjected to an electric pulse treatment at 500°C for 3 min and then air-cooled.
[0027] The experiment shows that the microstructure of the QAl11-6-6 aluminum bronze alloy after the heat treatment process of Example 1 of the present invention is mainly β' phase matrix and KⅡ phase. The electric pulse treatment can change the distribution of KⅡ phase in the aluminum bronze alloy. Part of KⅡ is distributed along the direction of the electric pulse current, such as Figure 1 shown.
[0028] The mechanical properties test results are: tensile strength of 1116MPa, yield strength of 1021MPa, elongation after fracture of 5.9%, which meet the use requirements. In comparison, the mechanical properties of the extruded QAl11-6-6 aluminum bronze alloy are: tensile strength of 956MPa, elongation after fracture of 2.3%. It can be seen that the heat treatment of the present invention can improve the strength and plasticity of QAl11-6-6 aluminum bronze materials and parts.
[0029] Example 2
[0030] QAl11-6-6 aluminum bronze alloy, the mass percentage of each element is: Al: 10.80%, Fe: 6.07%, Ni+Co: 6.22%, inevitable impurities: <0.5%, balance: Cu. It is melted and extruded into rods according to conventional processes, and the extruded rod specification is φ16mm. The heat treatment process is as follows:
[0031] (1) The extruded QA11-6-6 aluminum bronze alloy rod was placed in a resistance furnace heated to 860°C for 1.5 hours for high temperature heat treatment, and immediately quenched and cooled in room temperature water after being taken out of the furnace.
[0032] (2) The QAl11-6-6 aluminum bronze alloy tubes and bars or machined parts that have undergone the first high-temperature heat treatment are placed in a resistance furnace heated to 750°C for 2 hours for a second high-temperature heat treatment, and then air-cooled after being taken out of the furnace;
[0033] (3) The QAl11-6-6 aluminum bronze alloy tube and rod that has undergone the second high-temperature heat treatment is placed in a resistance furnace heated to 500°C for 2.5 hours for low-temperature heat treatment, and then air-cooled after being taken out of the furnace.
[0034] (4) The QAl11-6-6 aluminum bronze alloy tube, bar or machined parts that have undergone low temperature heat treatment are subjected to an electric pulse treatment at 500°C for 5 min and then air-cooled.
[0035] The experiment shows that the microstructure of the QAl11-6-6 aluminum bronze alloy after the heat treatment process of Example 2 of the present invention is mainly composed of β' phase matrix and KⅡ phase, and part of KⅡ is distributed along the direction of the electric pulse current. Compared with Example 1, the KⅡ phase in the aluminum bronze alloy is aggregated and gathered into a larger "tadpole-shaped" phase, such as Figure 2 The mechanical properties test results are as follows: tensile strength reaches 1020MPa, yield strength reaches 1006MPa, and elongation after fracture reaches 6.63%. In comparison, the mechanical properties of the extruded QAl11-6-6 aluminum bronze alloy are as follows: tensile strength 956MPa, elongation after fracture 2.3%. Compared with Example 1, due to the extension of the electric pulse time to 5min, the plasticity is improved and the strength is slightly reduced, but it can still meet the use requirements.
[0036] Comparative Example 1
[0037] QAl11-6-6 aluminum bronze alloy, the mass percentage of each element is: Al: 10.80%, Fe: 6.07%, Ni+Co: 6.22%, inevitable impurities: <0.5%, balance: Cu. It is melted and extruded into rods according to conventional processes, and the extruded rod specification is φ16mm. The heat treatment process is as follows:
[0038] (1) The extruded QA11-6-6 aluminum bronze alloy rod was placed in a resistance furnace heated to 860°C for 1.5 hours for high temperature heat treatment, and immediately quenched and cooled in room temperature water after being taken out of the furnace.
[0039] (2) The QAl11-6-6 aluminum bronze alloy tubes and bars or machined parts that have undergone the first high-temperature heat treatment are placed in a resistance furnace heated to 750°C for 2 hours for a second high-temperature heat treatment, and then air-cooled after being taken out of the furnace;
[0040] (3) The QAl11-6-6 aluminum bronze alloy tube and rod that has undergone the second high-temperature heat treatment is placed in a resistance furnace heated to 500°C for 2.5 hours for low-temperature heat treatment, and then air-cooled after being taken out of the furnace.
[0041] The test shows that after the sample of comparative example 1 was subjected to solution aging heat treatment and no electric pulse treatment, the matrix of the QAl11-6-6 aluminum bronze alloy was α phase and β phase, and a large number of nearly spherical KⅡ phases (C-type phases) were distributed in the matrix. There were intermittent point-shaped or rod-shaped particles distributed on the grain boundaries, such as Figure 3 As shown. Compared with the extruded alloy, the martensitic characteristics of the microstructure in the heat treatment state are more obvious, the α phase size is smaller, and the distribution is more uniform. The mechanical properties test results are: the tensile strength is 970MPa, the yield strength is 950MPa, and the elongation after fracture is 2%. The mechanical properties of the extruded QAl11-6-6 aluminum bronze alloy are: tensile strength 956MPa, elongation after fracture 2.3%. In comparison, the strengthening effect produced by the heat treatment of comparative example 1 is not obvious.
[0042] Comparative Example 2
[0043] QAl11-6-6 aluminum bronze alloy, the mass percentage of each element is: Al: 10.80%, Fe: 6.07%, Ni+Co: 6.22%, inevitable impurities: <0.5%, balance: Cu. It is melted and extruded into rods according to conventional processes, and the extruded rod specification is φ16mm. The heat treatment process is as follows:
[0044] (1) The extruded QA11-6-6 aluminum bronze alloy rod was placed in a resistance furnace heated to 860°C for 1.5 hours for high temperature heat treatment, and immediately quenched and cooled in room temperature water after being taken out of the furnace.
[0045] (2) The QAl11-6-6 aluminum bronze alloy tubes and bars or machined parts that have undergone the first high-temperature heat treatment are placed in a resistance furnace heated to 750°C for 2 hours for a second high-temperature heat treatment, and then air-cooled after being taken out of the furnace;
[0046] (3) The QAl11-6-6 aluminum bronze alloy tube and rod that has undergone the second high-temperature heat treatment is placed in a resistance furnace heated to 500°C for 2.5 hours for low-temperature heat treatment, and then air-cooled after being taken out of the furnace.
[0047] (4) The QAl11-6-6 aluminum bronze alloy tube, bar or machined parts that have undergone low temperature heat treatment are subjected to an electric pulse treatment at 500°C for 7 min and then air-cooled.
[0048] The test shows that after the solution aging heat treatment, the sample in comparative example 2 was subjected to an electric pulse treatment for 7 minutes. Due to the long electric pulse treatment time, the KⅡ phase in the QAl11-6-6 aluminum bronze alloy aggregated and grew to form large particles, short rods, and tadpoles, with a maximum size of 15μm, which is not conducive to the strengthening and toughening of the alloy. Figure 4 The mechanical properties test results are: tensile strength is 1015MPa, yield strength is 970MPa, and elongation after fracture is 2.69%. In comparison, the mechanical properties of the extruded QAl11-6-6 aluminum bronze alloy are: tensile strength is 956MPa, and elongation after fracture is 2.3%.
[0049] The above embodiments are used to explain the present invention rather than to limit the present invention. Several improvements and modifications may be made without departing from the principles of the present invention, and these improvements and modifications are also considered to be within the protection scope of the present invention.
Claims
1. A heat treatment method for achieving ultra-high strength of aluminum bronze alloy, characterized in that: Follow these steps: Step 1: Cut the extruded or centrifugally cast QAl11-6-6 aluminum bronze alloy tube and rod into fixed lengths or machine them into parts, put them into a resistance furnace heated to 850-950℃ and keep them warm for 0.5-2.0 hours for the first high-temperature heat treatment, and immediately quench and cool them in room temperature water after taking them out of the furnace. Step 2: Place the QAl11-6-6 aluminum bronze alloy tubes and bars or machined parts that have undergone the first high-temperature heat treatment in a resistance furnace heated to (750-850)°C for 2-4 hours for the second high-temperature heat treatment, and air cool after being taken out of the furnace; Step 3: Place the QAl11-6-6 aluminum bronze alloy tubes and bars or machined parts that have undergone the second high-temperature heat treatment in a resistance furnace heated to (450-550)°C for 2-4 hours for low-temperature heat treatment, and air cool after being taken out of the furnace; Step 4: The QAl11-6-6 aluminum bronze alloy tube, bar or machined parts that have undergone low temperature heat treatment are subjected to an electric pulse treatment at 500°C × (1-8) min, followed by air cooling.
2. The heat treatment method for achieving ultra-high strength of aluminum bronze alloy according to claim 1, characterized in that: The first high temperature heat treatment parameters in step 1 are: keeping in a resistance furnace at 880-920°C for 0.5-1.0 hour, and immediately quenching and cooling in room temperature water after being taken out of the furnace; The second high temperature heat treatment parameters in step 2 are: keeping in a resistance furnace at 780-820°C for 2.5-3.3 hours, and air cooling after leaving the furnace; The low temperature heat treatment parameters in step 3 are: keeping in a resistance furnace at 480-520°C for 2-3 hours, and air cooling after leaving the furnace; The electric pulse treatment parameters in step 4 are: the QAl11-6-6 aluminum bronze alloy tube, bar or machined parts that have undergone low-temperature heat treatment are subjected to another electric pulse treatment at 500°C × (1 to 5) min, followed by air cooling.
Citation Information
Patent Citations
Grain refining method of aluminium bronze
CN101307419A
Method for improving cavitation corrosion resistance of nickel-aluminum bronze workpiece
CN114318196A
High-hardness corrosion-resistant nickel-aluminum bronze welding wire, preparation method thereof and application of high-hardness corrosion-resistant nickel-aluminum bronze welding wire in alloy cladding
CN115537596A
Preparation method of ultrahigh-strength elastic copper alloy material
CN118222950A
Manufacture of copper alloy casting
JP1986023754A