Preparation method of high-temperature alloy long in service life and difficult to deform and prepared turbine disc

By performing multi-stage heat treatment and process optimization on nickel-based high-temperature alloys, the grain size and internal structure are regulated, and the problem of the difficulty of nickel-based high-temperature alloys to have high long-lasting life and high room temperature tensile strength is solved, and the turbine disk of aero engine is realized efficient application in

CN118996300APending Publication Date: 2024-11-22GAONA AERO MATERIAL CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411108942.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing nickel-based high-temperature alloys are difficult to meet the comprehensive requirements of high-end life and high room temperature tensile strength at the same time, and cannot have high-temperature durability and tensile strength in strict aero engine hot-end components materials.

Method used

By homogenizing the nickel-based high-temperature alloy, forging, die-forging, solution treatment and aging treatment, the grain size and internal structure of the alloy are regulated, and alloy ingots are prepared by triple smelting technology, and multi-stage heat treatment process is passed Optimization, including solution treatment and aging treatment, improves the average grain size and internal deformation mechanism of the alloy.

Benefits of technology

The long-lasting life and room temperature tensile strength of nickel-based high-temperature alloys have been significantly improved, so that the long-lasting life of the turbine disc at high temperatures reaches ≥100h, and the room temperature tensile strength reaches ≥1550MPa, meeting the comprehensive requirements of hot-end components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996300A_ABST
    Figure CN118996300A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high-temperature alloys, in particular to a preparation method of a long-service-life and difficult-to-deform high-temperature alloy and a prepared turbine disc. A preparation method of a long-service-life and difficult-to-deform high-temperature alloy comprises the following steps that (a) a nickel-based high-temperature alloy ingot is subjected to homogenization treatment and then forged to obtain a forging stock, and then die forging forming is conducted to obtain a die forging piece; (b) the die forging is subjected to solution treatment and aging treatment; the solution treatment comprises the following steps: carrying out heat preservation treatment at 1000-1130 DEG C for more than 24 hours, and carrying out oil cooling; and the transfer time of oil cooling is 20-40s. According to the method, the heat treatment process of the nickel-based superalloy is regulated and controlled, so that the average grain size of the nickel-based superalloy reaches 25-35 microns, meanwhile, the interiors of the grains are changed, an extra deformation mechanism in the grains can be excited in the plastic deformation process, and the service life of the nickel-based superalloy is greatly prolonged under the condition that the endurance life of the nickel-based superalloy is greatly prolonged. And the room-temperature tensile strength is not reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-temperature alloys, and in particular to a method for preparing a long-life, hard-to-deform high-temperature alloy and a turbine disk prepared thereby. Background Art

[0002] Nickel-based deformable high-temperature alloys are widely used in the preparation of hot end components such as aircraft engine turbine disks due to their excellent high-temperature strength, corrosion resistance, oxidation resistance and fatigue resistance.

[0003] In recent years, with the increasing thrust ratio of advanced aircraft engines, the service environment of hot end component materials has become very harsh, seriously affecting service safety. Therefore, for hot end component materials, it is necessary to have both higher high temperature durability and room temperature tensile strength to ensure the service reliability of the material. However, most nickel-based high temperature alloys currently cannot meet the comprehensive requirements of high durability and excellent room temperature tensile strength.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] An object of the present invention is to provide a method for preparing a long-life, hard-to-deform high-temperature alloy, so as to solve the problem in the prior art that nickel-based high-temperature alloys are difficult to simultaneously meet the comprehensive requirements of components for high durability and high strength of the alloy.

[0006] Another object of the present invention is to provide a turbine disk manufactured by the above-mentioned manufacturing method.

[0007] In order to achieve the above-mentioned object of the present invention, the present invention provides a method for preparing a long-life hard-to-deform high-temperature alloy, comprising the following steps:

[0008] (a) homogenizing a nickel-based high-temperature alloy ingot, then forging it to obtain a forging blank, and then die forging it to obtain a die forging;

[0009] (b) subjecting the die forging to a solution treatment and an aging treatment;

[0010] The solution treatment includes: heat preservation treatment at 1000-1130°C for more than 24 hours, oil cooling; the oil cooling transfer time is 20-40 seconds;

[0011] The nickel-based high-temperature alloy includes the following components in mass percentage: Ti 4.75%-5.25%, Al 2.25%-2.75%, Co 14.0%-15.5%, Cr 15.5%-16.5%, Mo 2.75%-3.25%, W 1.0%-1.5%, C 0.01%-0.02%, B 0.01%-0.02%, and the balance Ni.

[0012] In a specific embodiment of the present invention, in the solution treatment, the time of heat preservation treatment at 1110-1130° C. is 24-28 hours.

[0013] In a specific embodiment of the present invention, the aging treatment comprises: heat preservation treatment at 600-660° C. for 22-26 hours, air cooling, and then heat preservation treatment at 700-760° C. for 14-18 hours, and air cooling.

[0014] In a specific embodiment of the present invention, the nickel-based high-temperature alloy includes the following components in mass percentage: Ti 4.95% to 5.2%, Al 2.25% to 2.52%, Co 14.5% to 15.5%, Cr15.5% to 16.5%, Mo2.75% to 3.05%, W 1.3% to 1.5%, C 0.01% to 0.02%, B0.01% to 0.02%, and the balance Ni.

[0015] In a specific embodiment of the present invention, the homogenization treatment includes: heat preservation treatment at 1150-1170°C for 30-40h, then heating to 1180-1250°C for 35-45h, furnace cooling to below 1100±10°C and then air cooling out of the furnace.

[0016] In a specific embodiment of the present invention, during the forging, the forging temperature is 1000-1150°C.

[0017] In a specific embodiment of the present invention, in the die forging, the die forging temperature is 1100-1140°C.

[0018] In a specific embodiment of the present invention, the nickel-based high-temperature alloy ingot is obtained by a triple smelting process; the triple smelting includes: vacuum induction melting, electroslag remelting and vacuum consumable remelting.

[0019] Another aspect of the present invention provides a turbine disk produced by any one of the above-mentioned production methods.

[0020] In a specific embodiment of the present invention, the average grain size of the turbine disk is 25-35 μm.

[0021] In a specific embodiment of the present invention, the durability of the turbine disk under the conditions of 680°C / 830MPa is ≥100h; the durability of the turbine disk under the conditions of 730°C / 530MPa is ≥321h.

[0022] In a specific embodiment of the present invention, the room temperature tensile strength of the turbine disk is ≥1550 MPa.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention regulates the heat treatment process of the nickel-based high-temperature alloy so that the average grain size of the nickel-based high-temperature alloy reaches 25 to 35 μm, and at the same time, changes occur inside the grains, so that additional deformation mechanisms inside the grains may be stimulated during the plastic deformation process, thereby greatly improving the long-term service life of the nickel-based high-temperature alloy while ensuring that its room temperature tensile strength is not reduced;

[0025] (2) The turbine disk obtained by the preparation method of the present invention has a room temperature tensile strength of more than 1550 MPa, and a durability life of ≥100 h at 680°C / 830 MPa, and a durability life of ≥321 h at 730°C / 530 MPa, which meets the comprehensive requirements of high durability and room temperature tensile strength, and broadens its application in hot end components. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 The organizational diagram of the nickel-based high-temperature alloy component provided in Example 1 of the present invention;

[0028] Figure 2 The organizational diagram of the nickel-based high-temperature alloy component provided in Example 2 of the present invention;

[0029] Figure 3 The organizational diagram of the nickel-based high-temperature alloy component provided in Example 3 of the present invention;

[0030] Figure 4 The organizational diagram of the nickel-based high-temperature alloy component provided in Example 4 of the present invention;

[0031] Figure 5 The organizational diagram of the nickel-based high-temperature alloy component provided for Comparative Example 1;

[0032] Figure 6 This is the organizational diagram of the nickel-based high-temperature alloy component provided for Comparative Example 2. DETAILED DESCRIPTION

[0033] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0034] The performance of an alloy is related to its structure. Generally, the smaller the grain size, the more grain boundaries there are, and the greater the hindrance of dislocation movement by grain boundaries, the higher the strength of the alloy, but at the same time the durability will be lower. If the alloy grain size is adjusted to be relatively coarse, although the durability of the alloy may be improved to a certain extent, the increase in grain size will generally lead to a decrease in the strength of the alloy. Therefore, most current nickel-based high-temperature alloys cannot meet the comprehensive requirements of both high durability and high room temperature strength.

[0035] Based on this, the present invention provides a method for preparing a long-life, hard-to-deform high-temperature alloy, comprising the following steps:

[0036] (a) homogenizing a nickel-based high-temperature alloy ingot, then forging it to obtain a forging blank, and then die forging it to obtain a die forging;

[0037] (b) subjecting the die forging to solution treatment and aging treatment;

[0038] The solution treatment includes: heat preservation treatment at 1000-1130℃ for more than 24h, oil cooling; the transfer time of oil cooling is 20-40s;

[0039] The nickel-based high-temperature alloy includes the following components in percentage by mass: Ti 4.75% to 5.25%, Al 2.25% to 2.75%, Co 14.0% to 15.5%, Cr 15.5% to 16.5%, Mo 2.75% to 3.25%, W 1.0% to 1.5%, C 0.01% to 0.02%, B 0.01% to 0.02%, and the balance Ni.

[0040] The present invention regulates the heat treatment process of the nickel-based high-temperature alloy so that the average grain size of the nickel-based high-temperature alloy increases from about 10 to 15 μm to 25 to 35 μm. The appropriate increase in the grain size reduces the volume fraction of the grain boundary to a certain extent, thereby significantly increasing the endurance of the nickel-based high-temperature alloy. At the same time, the regulation of the heat treatment process of the present invention causes changes in the interior of the obtained alloy grains, so that additional deformation mechanisms inside the grains may be stimulated during the plastic deformation process, forming twins and / or stacking faults, compensating for the loss of strength caused by the increase in grain size, thereby obtaining an alloy with high endurance and room temperature tensile strength.

[0041] The present invention regulates the appropriate solution treatment temperature, duration, and oil cooling transfer over time, on the one hand, cooperates with the subsequent process to make the average grain size of the obtained alloy within the range of 25 to 35 μm, and on the other hand, ensures that certain changes occur inside the grains, so that additional deformation mechanisms can be stimulated during the plastic deformation process to ensure its tensile properties. For example, in different embodiments, in the solution treatment, the insulation temperature can be 1000°C, 1020°C, 1050°C, 1080°C, 1100°C, 1120°C, 1130°C, or a range consisting of any two thereof, and the insulation treatment time can be 24h, 25h, 26h, 27h, 28h, 30h, or a range consisting of any two thereof. The oil cooling transfer time can be 20s, 22s, 25s, 28s, 30s, 32s, 35s, 38s, 40s or a range consisting of any two of them. The oil cooling transfer time is regulated within the above range to avoid stress concentration cracking caused by too fast transfer and to avoid too slow transfer affecting the microstructure of the alloy.

[0042] In the nickel-based high-temperature alloy of the present invention, the content of each element can be as follows:

[0043] The mass percentage of Ti may be 4.75%, 4.8%, 5%, 5.15%, 5.25% or a range consisting of any two thereof; the mass percentage of Al may be 2.25%, 2.4%, 2.6%, 2.7%, 2.75% or a range consisting of any two thereof; the mass percentage of Co may be 14.0%, 14.2%, 14.5%, 14.8%, 15%, 15.2%, 15.5% or a range consisting of any two thereof; the mass percentage of Cr may be 15.5%, 15.8%, 16%, 16.2%, 16.5% or a range consisting of any two thereof. The mass percentage of Mo may be 2.75%, 2.9%, 3%, 3.1%, 3.25% or a range consisting of any two thereof; the mass percentage of W may be 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5% or a range consisting of any two thereof; the mass percentage of C may be 0.01%, 0.012%, 0.015%, 0.018%, 0.02% or a range consisting of any two thereof; the mass percentage of B may be 0.01%, 0.012%, 0.015%, 0.018%, 0.02% or a range consisting of any two thereof.

[0044] In a specific embodiment of the present invention, during the solution treatment, the holding time at 1110-1130° C. is 24-28 hours. Further optimization of the temperature and holding time of the solution treatment is more conducive to ensuring or even improving the room temperature tensile strength while improving the durability.

[0045] In a specific embodiment of the present invention, the aging treatment comprises: heat preservation treatment at 600-660° C. for 22-26 hours, air cooling, and then heat preservation treatment at 700-760° C. for 14-18 hours, and air cooling.

[0046] Among them, in the aging treatment, the temperature can be kept at 600°C, 620°C, 640°C, 660°C or any two of them for 22h, 24h, 26h, etc., and then air-cooled; and then the temperature can be kept at 700°C, 720°C, 740°C, 760°C or any two of them for 14h, 16h, 18h, etc., and then air-cooled.

[0047] In a specific embodiment of the present invention, the nickel-based high-temperature alloy includes the following components by mass percentage: Ti 4.95% to 5.2%, Al 2.25% to 2.52%, Co 14.5% to 15.5%, Cr 15.5% to 16.5%, Mo 2.75% to 3.05%, W 1.3% to 1.5%, C 0.01% to 0.02%, B 0.01% to 0.02%, and the balance Ni. By further optimizing and regulating the composition of the nickel-based high-temperature alloy, it is more conducive to cooperating with the aforementioned solid solution treatment and other processes, and on the basis of ensuring the average grain size, a microstructure that can fully stimulate the deformation mechanism inside the grain is obtained, ensuring or even improving the room temperature tensile strength.

[0048] In a specific embodiment of the present invention, the homogenization treatment includes: heat preservation treatment at 1150-1170°C for 30-40 hours, then heating to 1180-1250°C for heat preservation treatment for 35-45 hours, cooling the furnace to below 1100±10°C and then air cooling out of the furnace.

[0049] The present invention adopts a multi-stage homogenization treatment, which ensures the homogenization of the ingot structure on the one hand, and first reaches the homogenization temperature and maintains it for a period of time, so that the phase distribution in the alloy is uniform, and the grain size does not grow significantly within the temperature range; then the temperature is further increased, and a certain cooling method is used to further eliminate element segregation, reduce the content of the eutectic phase, improve the hot working performance, and cooperate with the subsequent process steps to improve the durability and tensile strength. For example, in different embodiments, the homogenization treatment may include: heat preservation treatment at 1150°C, 1160°C, 1170°C for 30h, 32h, 35h, 38h, 40h, etc., and then heat preservation treatment at 1180°C, 1200°C, 1220°C, 1250°C for 35h, 38h, 40h, 42h, 45h, etc., and air cooling after furnace cooling to below 1100±10°C.

[0050] In a specific embodiment of the present invention, during forging, the forging temperature is 1000-1150° C. For example, in different embodiments, during forging, the forging temperature can be 1000° C., 1050° C., 1100° C., 1150° C., or a range consisting of any two thereof.

[0051] In a specific embodiment of the present invention, during die forging, the die forging temperature is 1100-1140° C. For example, in different embodiments, during die forging, the die forging temperature can be 1100° C., 1110° C., 1120° C., 1130° C., 1140° C., or a range consisting of any two of them.

[0052] In actual operation, the forging method and the corresponding forging process can be selected according to the actual requirements of the alloy component. For example, when preparing alloy disc forgings, the ingot can be conventionally forged to obtain a rod blank, and then die forged to obtain the corresponding disc forging. The present invention does not elaborate on the process operations of forging and die forging. It is sufficient to adjust the processing temperature within the above range and adopt conventional processing methods.

[0053] In a specific embodiment of the present invention, the nickel-based high-temperature alloy ingot is obtained by a triple smelting process; the triple smelting includes: vacuum induction melting, electroslag remelting and vacuum consumable remelting.

[0054] The specific ingot is produced by conventional triple smelting method.

[0055] Another aspect of the present invention provides a turbine disk produced by any one of the above-mentioned production methods.

[0056] In a specific embodiment of the present invention, the average grain size of the turbine disk is 25-35 μm.

[0057] In a specific embodiment of the present invention, the durable life of the turbine disk at 680°C / 830MPa is ≥75h, preferably ≥100h, and more preferably ≥130h; the durable life of the turbine disk at 730°C / 530MPa is ≥200h, preferably ≥321h, and more preferably ≥325h.

[0058] For example, in different embodiments, the durability of the turbine disk at 680°C / 830MPa can be 100h, 104h, 110h, 120h, 150h, 160h, 180h, 190h, 193h or a range consisting of any two of them; the durability of the turbine disk at 730°C / 530MPa can be 321h, 330h, 340h, 360h, 375h, 385h, 393h or a range consisting of any two of them.

[0059] In a specific embodiment of the present invention, the room temperature tensile strength of the turbine disk is ≥1550 MPa.

[0060] For example, in different embodiments, the room temperature tensile strength of the turbine disk may be 1550 MPa, 1560 MPa, 1570 MPa, 1580 MPa, 1590 MPa, or a range consisting of any two thereof.

[0061] The room temperature tensile strength of the turbine disk obtained by the existing preparation method is mostly between 1500 and 1600 MPa, but the endurance life is relatively low, such as the endurance life at 680℃ / 830MPa is less than 100h, and the endurance life at 730℃ / 530MPa is no more than 200h. The turbine disk obtained by the preparation method of the present invention meets the comprehensive requirements of both high endurance life and room temperature tensile strength, and broadens its application in hot end components.

[0062] Example 1

[0063] This embodiment provides a method for preparing a long-life, hard-to-deform high-temperature alloy, comprising the following steps:

[0064] (1) after performing vacuum induction melting, electroslag remelting and vacuum consumable melting according to the alloy ratio, casting to obtain an alloy ingot, the cross-sectional size of the ingot is Φ510 mm;

[0065] The element composition (mass percentage) of the nickel-based high-temperature alloy includes: Ti 5.05%, Al 2.48%, Co 15.2%, Cr 16.1%, Mo 3.02%, W 1.42%, C 0.016%, B 0.015%, and the balance Ni.

[0066] (2) homogenizing the alloy ingot obtained in step (1); the homogenizing treatment comprises: keeping the alloy ingot at 1160° C. for 35 hours, then heating the alloy ingot to 1200° C. and keeping the alloy ingot for 40 hours, then cooling the alloy ingot to 1100° C. and air cooling the alloy ingot out of the furnace.

[0067] (3) The alloy ingot after the homogenization treatment in step (2) is kept at 1180° C. for 70 hours and forged to obtain a rod with a diameter of 150 mm; then the rod is kept at 1120° C. for 3 hours and die-forged to obtain a disc forging.

[0068] (4) The disc forging obtained in step (3) is heat-treated at 1110° C. for 24 h and oil-cooled, and the oil-cooling transfer time is 30±1 s; then the disc forging is heat-treated at 650° C. for 24 h and air-cooled, and then heat-treated at 760° C. for 16 h and air-cooled.

[0069] Example 2

[0070] This example is prepared by referring to the preparation method of Example 1, with the only difference being that the process parameters of step (4) are different.

[0071] In this embodiment, step (4) includes: heat-treating the disc forging obtained in step (3) at 1130°C for 24 hours, oil cooling, and the oil cooling transfer time is 20 to 22 seconds; then heat-treating the disc forging at 650°C for 24 hours, air cooling, and then heat-treating at 760°C for 16 hours, and air cooling.

[0072] Example 3

[0073] This example is prepared by referring to the preparation method of Example 1, with the only difference being that the process parameters of step (4) are different.

[0074] In this embodiment, step (4) includes: heat-treating the disc forging obtained in step (3) at 1120°C for 24 hours, oil cooling, and the oil cooling transfer time is 30±1s; then heat-treating the disc forging at 650°C for 24 hours, air cooling, and then heat-treating at 760°C for 16 hours, and air cooling.

[0075] Example 4

[0076] This example is prepared by referring to the preparation method of Example 1, with the only difference being that the process parameters of step (4) are different.

[0077] In this embodiment, step (4) includes: heat-treating the disc forging obtained in step (3) at 1000°C for 24 hours, oil cooling, and the oil cooling transfer time is 38 to 40 seconds; then heat-treating the disc forging at 650°C for 24 hours, air cooling, and then heat-treating at 760°C for 16 hours, and air cooling.

[0078] Example 5

[0079] This example is prepared by referring to the preparation method of Example 1, with the only difference being that the process parameters of step (4) are different.

[0080] In this embodiment, step (4) includes: heat-treating the disc forging obtained in step (3) at 1080°C for 24 hours, oil cooling, and the oil cooling transfer time is 30±1s; then heat-treating the disc forging at 650°C for 24 hours, air cooling, and then heat-treating at 760°C for 16 hours, and air cooling.

[0081] Example 6

[0082] This example is based on the preparation method of Example 1, with the only difference being that the process parameters of step (2) are different.

[0083] In this embodiment, step (2) includes: homogenizing the alloy ingot obtained in step (1); keeping the alloy ingot at 1160°C for 35 hours, then heating the alloy ingot to 1200°C and keeping the temperature for 40 hours, and then removing the alloy from the furnace and air cooling the alloy.

[0084] Example 7

[0085] This example is based on the preparation method of Example 1, with the only difference being that the process parameters of step (2) are different.

[0086] In this embodiment, step (2) includes: homogenizing the alloy ingot obtained in step (1); the homogenizing treatment includes: keeping the alloy ingot at 1145°C for 30 hours, then heating it to 1175°C and keeping it for 30 hours, then cooling it in the furnace to 1100°C and air cooling it out of the furnace.

[0087] Example 8

[0088] This embodiment refers to the preparation method of embodiment 1, with the only difference being that the composition of the alloy ingot in step (1) is different.

[0089] The element composition (mass percentage) of the nickel-based high-temperature alloy includes: Ti 4.89%, Al 2.61%, Co 14.3%, Cr 16.0%, Mo 3.05%, W 1.39%, C 0.015%, B 0.014%, and the balance Ni.

[0090] Example 9

[0091] This embodiment refers to the preparation method of embodiment 1, with the only difference being that the composition of the alloy ingot in step (1) is different.

[0092] The element composition (mass percentage) of the nickel-based high-temperature alloy includes: Ti 5.02%, Al 2.51%, Co 15.1%, Cr 16.3%, Mo 3.14%, W 1.13%, C 0.014%, B 0.017%, and the balance Ni.

[0093] Comparative Example 1

[0094] Comparative Example 1 refers to the preparation method of Example 1, except that the process parameters of step (4) are different.

[0095] In comparative example 1, step (4) comprises: heat-treating the disc forging obtained in step (3) at 1110°C for 4 hours, oil cooling, and the oil cooling transfer time is 30±1s; then heat-treating the disc forging at 650°C for 24 hours, air cooling, and then heat-treating at 760°C for 16 hours, and air cooling.

[0096] Comparative Example 2

[0097] Comparative Example 2 refers to the preparation method of Example 1, except that the process parameters of step (4) are different.

[0098] In Comparative Example 2, step (4) includes: heat-treating the disc forging obtained in step (3) at 1110°C for 24 hours, oil cooling, and the oil cooling transfer time is 10 to 12 seconds; then heat-treating the disc forging at 650°C for 24 hours, air cooling, and then heat-treating at 760°C for 16 hours, and air cooling.

[0099] Comparative Example 3

[0100] Comparative Example 3 refers to the preparation method of Example 1, except that the process parameters of step (4) are different.

[0101] In comparative example 3, step (4) comprises: heat-treating the disc forging obtained in step (3) at 1110°C for 24 hours, oil cooling, and the oil cooling transfer time is 50 to 52 seconds; then heat-treating the disc forging at 650°C for 24 hours, air cooling, and then heat-treating at 760°C for 16 hours, and air cooling.

[0102] Comparative Example 4

[0103] Comparative Example 4 refers to the preparation method of Example 1, except that the process parameters of step (4) are different.

[0104] In comparative example 4, step (4) comprises: heat-treating the disc forging obtained in step (3) at 1110°C for 20 hours, oil cooling, and the oil cooling transfer time is 30±1s; then heat-treating the disc forging at 650°C for 24 hours, air cooling, and then heat-treating at 760°C for 16 hours, and air cooling.

[0105] Experimental example

[0106] In order to compare and illustrate the performance differences of the nickel-based high-temperature alloys prepared by the preparation methods of different embodiments and comparative examples, samples of the disc forgings after aging treatment of each embodiment and comparative example were sampled and characterized for mechanical property testing and microstructure characterization. The test results are shown in Table 1. Figure 1 to Figure 4 The organizational diagram of the nickel-based high-temperature alloy component provided in Examples 1 to 4 of the present invention, Figure 5-6 The organizational diagrams of the nickel-based high-temperature alloy components provided for Comparative Examples 1 and 2.

[0107] Table 1 Test results of alloy components of different embodiments and comparative examples

[0108]

[0109] It can be seen from the above test results that the heat treatment process of the nickel-based high-temperature alloy of the present invention is regulated so that the average grain size of the nickel-based high-temperature alloy reaches 25 to 35 μm. At the same time, changes occur inside the grains, which may stimulate additional deformation mechanisms inside the grains during the plastic deformation process, thereby greatly improving the long-lasting life of the nickel-based high-temperature alloy while ensuring that its room temperature tensile strength is not reduced.

[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a long-life, hard-to-deform high-temperature alloy. It is characterized in that The steps include: (a) homogenizing a nickel-based high-temperature alloy ingot, then forging it to obtain a forging blank, and then die forging it to obtain a die forging; (b) subjecting the die forging to a solution treatment and an aging treatment; The solution treatment includes: heat preservation treatment at 1000-1130°C for more than 24 hours, oil cooling; the oil cooling transfer time is 20-40 seconds; The nickel-based high-temperature alloy includes the following components in mass percentage: Ti 4.75%-5.25%, Al 2.25%-2.75%, Co 14.0%-15.5%, Cr 15.5%-16.5%, Mo 2.75%-3.25%, W 1.0%-1.5%, C 0.01%-0.02%, B 0.01%-0.02%, and the balance Ni.

2. The preparation method according to claim 1, It is characterized in that In the solution treatment, the time of heat preservation treatment at 1110-1130° C. is 24-28 hours.

3. The preparation method according to claim 1, It is characterized in that The aging treatment comprises: heat preservation treatment at 600-660° C. for 22-26 hours, air cooling, and then heat preservation treatment at 700-760° C. for 14-18 hours, and air cooling.

4. The preparation method according to claim 1, It is characterized in that The nickel-based high-temperature alloy includes the following components in mass percentage: Ti 4.95%-5.2%, Al 2.25%-2.52%, Co14.5%-15.5%, Cr 15.5%-16.5%, Mo 2.75%-3.05%, W 1.3%-1.5%, C 0.01%-0.02%, B 0.01%-0.02%, and the balance Ni.

5. The preparation method according to claim 1, It is characterized in that The homogenization treatment comprises: heat preservation treatment at 1150-1170° C. for 30-40 hours, then heating to 1180-1250° C. for heat preservation treatment for 35-45 hours, furnace cooling to below 1100±10° C. and then air cooling out of the furnace.

6. The preparation method according to claim 1, It is characterized in that In the forging, the forging temperature is 1000-1150°C; And / or, during the die forging, the die forging temperature is 1100-1140°C.

7. The preparation method according to claim 1, It is characterized in that The nickel-based high-temperature alloy ingot is obtained through a triple smelting process; the triple smelting includes: vacuum induction melting, electroslag remelting and vacuum consumable remelting.

8. Turbine disc, It is characterized in that The preparation method is described in any one of claims 1 to 7.

9. The turbine disk according to claim 8, It is characterized in that The average grain size of the turbine disk is 25-35 μm.

10. The turbine disk according to claim 8, It is characterized in that Satisfy at least one of the following characteristics: (1) The turbine disc has a lifespan of ≥100 h at 680°C / 830 MPa; (2) The turbine disk has a lifespan of ≥321 h at 730°C / 530 MPa; (3) The room temperature tensile strength of the turbine disk is ≥1550 MPa.

Citation Information

Cited By

  • Super-large ingot type high-temperature alloy forging material and preparation method thereof