Method for manufacturing semiconductor member
Through photoelectrochemical etching technology, precision fin-shaped or island-shaped gate convex parts are formed on semiconductor wafers, which solves the problems of shape accuracy and error control of semiconductor components in the prior art, improves the yield rate and reduces damage to semiconductor materials. risk.
Patent Information
- Application Number
- CN202410588330.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-22
AI Technical Summary
It is difficult to effectively manufacture semiconductor components with precision shapes, especially in semiconductor components, which affect the action characteristics of the components, and the existing processes have challenges to the etching accuracy and error control of semiconductor materials.
By using photoelectrochemical etching (PEC) method, by forming a mask on a semiconductor wafer, applying voltage and irradiating light to the etching solution, the gate convex portions in a fin-shaped or island-shaped manner are gradually etched, and the carrier concentration and etching are used. The pH controls the etching process of the liquid to achieve precise width control of the gate convex portion.
The precise shape formation of gate convex parts in the semiconductor element is realized, the yield is improved, the width error is reduced, the damage to semiconductor crystals is avoided, and the etching process can be automatically stopped, ensuring the normally closed state of the element.
Smart Images

Figure CN119008409A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a semiconductor component. Background Art
[0002] Semiconductor components formed of semiconductor materials with structures are widely used in semiconductor devices and the like. For example, a fin field effect transistor formed with a fin structure as a gate portion is known (see, for example, Patent Document 1). For example, the structure used in a semiconductor device may affect the operating characteristics of the device, and therefore, it is preferably formed in a precise shape.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 2017 / 047286 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] An object of the present invention is to provide a novel method for manufacturing a semiconductor member used in a semiconductor element or the like.
[0008] Solutions for solving problems
[0009] According to one embodiment of the present invention, there is provided a method for manufacturing a semiconductor component, comprising the following steps:
[0010] a step of preparing a processing object, the processing object comprising a wafer made of a conductive semiconductor and a mask arranged on an upper surface of the wafer,
[0011] a step of performing photoelectrochemical etching on the wafer by immersing the object to be processed in an etching solution and irradiating light from the upper surface side of the wafer,
[0012] In the process of photoelectrochemically etching the wafer,
[0013] The outer portion of the mask of the wafer is etched to form a convex portion below the mask.
[0014] The etching of the first side surface and the second side surface of the protrusion facing each other is automatically stopped by etching until the entire width between the first side surface and the second side surface is exhausted.
[0015] Effects of the Invention
[0016] A new method for manufacturing a semiconductor member used in a semiconductor element or the like can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 (a) and Figure 1 (b) are a cross-sectional view and a top view schematically showing the FET 100 according to the embodiment of the present invention, respectively.
[0018] Figure 2 (a) is a cross-sectional view schematically showing an object 150 to be processed in PEC etching according to an embodiment. Figure 2 (b) is a cross-sectional view schematically showing the PEC etching device 200 according to the embodiment.
[0019] Figure 3 (a)~ Figure 3 (c) is a schematic cross-sectional view showing the wafer 10a and the vicinity of the mask 160 of the semiconductor component 10 during PEC etching according to the embodiment.
[0020] Figure 4 (a) and Figure 4 (b) are a cross-sectional view and a top view schematically showing the FET 100 according to the first modification example, respectively.
[0021] Figure 5 FIG. 1 is a plan view schematically showing a FET 100 according to a second modification example.
[0022] Figure 6 (a) represents the Schottky barrier Φ B The depletion layer width W at each carrier concentration n when the current is 1 eV D Table showing the dependence of the 2-fold value on the applied voltage V. Figure 6 (b) is a table showing the allowable error of the width W of the gate protrusion 16 when the allowable error of the threshold value is ±50 mV and when the allowable error of the threshold value is ±100 mV.
[0023] Description of Reference Numerals
[0024] 10 ... semiconductor member, 10a ... wafer, 10D ... depletion layer, 11 ... substrate, 12 ... drift layer, 13 ... semiconductor layer, 15 ... gate recess, 16 ... gate protrusion, 16a ... side surface, 16b ... side surface, 20 ... gate electrode, 21 ... gate pad, 30 ... source electrode, 31 ... source pad, 40 ... drain electrode, 100 ... FET, 150 ... object to be processed, 160 ... mask, 200 ... PEC etching device, 210 ... container, 220 ... etching liquid, 230 ... light source, 231 ... light, 240 ... voltage source, 241 ... electrode on the side of the object to be processed, 242 ... wiring, 243 ... electrode on the side of the etching liquid, 244 ... covering member DETAILED DESCRIPTION
[0025] The manufacturing method of the semiconductor component described in the embodiment of the present invention is described. Here, as an example of the semiconductor component described in the embodiment, a field effect transistor (FET) as a semiconductor element is cited for description. It should be noted that the semiconductor component described in the embodiment may have only a semiconductor component, or may have other components such as a semiconductor component and an electrode as in this example. In addition, the use of the semiconductor component manufactured by the manufacturing method of the embodiment is not limited to FET.
[0026] The structure and operation of the FET 100 described in the embodiment will be exemplified. Figure 1 (a) and Figure 1 (b) are schematic cross-sectional views and plan views of the FET 100 according to the embodiment. The FET 100 includes a semiconductor member 10, a gate electrode 20, a source electrode 30, and a drain electrode 40. It should be noted that the FET 100 may include other members such as an insulating film as required.
[0027] The semiconductor component 10 is composed of a semiconductor material having conductivity by containing n-type conductive impurities (hereinafter also referred to as impurities) at a specified concentration. As a semiconductor material constituting the semiconductor component 10, a material that can be etched by photoelectrochemical (PEC) etching can be appropriately used, and for example, gallium nitride (GaN), silicon carbide (SiC), etc. can be used. It should be noted that it is not limited to wide bandgap semiconductors such as GaN, and existing compound semiconductors such as gallium arsenide (GaAs) and indium phosphide (InP) can be used. Here, as a semiconductor material constituting the semiconductor component 10, GaN containing n-type impurities such as silicon (Si) is used as an example for explanation.
[0028] The semiconductor component 10 used in the FET 100 of this example includes a substrate 11 and a layer 12 (hereinafter referred to as the drift layer 12) epitaxially grown on the substrate 11. The drift layer 12 is formed with a protrusion 16 (hereinafter referred to as the gate protrusion 16) by the manufacturing method (processing method) described in the embodiment, specifically by PEC etching. The gate protrusion 16 has a width W (refer to Figure 3 (c)). As will be described later, the width W of the gate protrusion 16 is determined according to the carrier concentration of the drift layer 12. In other words, the carrier concentration of the drift layer 12, in other words, the concentration of impurities added to the drift layer 12, is set in such a way as to obtain a predetermined width W.
[0029] For example, by setting the carrier concentration of the drift layer 12 to 1×10 16 / cm 3 The width W of the gate protrusion 16 can be set to 600 nm (refer to Figure 6By reducing the carrier concentration of the drift layer 12, the width W of the gate protrusion 16 can be widened, and by increasing the carrier concentration of the drift layer 12, the width W of the gate protrusion 16 can be narrowed (refer to Figure 6 (a)). The width W of the gate protrusion 16 (more specifically, the width W of the narrowest part of the gate protrusion 16) is preferably greater than 200 nm and less than 2000 nm. The carrier concentration of the drift layer 12 is set in such a way that the width W of the gate protrusion 16 is within this range. It should be noted that (since the width of the depletion layer depends on the dielectric constant of the semiconductor material,) the relationship between the carrier concentration of the drift layer 12 and the width W of the gate protrusion 16 will vary to some extent depending on the semiconductor material used. The precise relationship between the carrier concentration of the drift layer 12 and the width W of the gate protrusion 16 in the semiconductor material used can be obtained, for example, by preliminary experiments, and the carrier concentration of the drift layer 12 can be set based on the precise relationship obtained.
[0030] A gate protrusion 16 is formed on the upper surface of the semiconductor component 10 , in other words, on the upper surface of the drift layer 12 , and a recess 15 (hereinafter referred to as gate recess 15 ) is formed outside the gate protrusion 16 (in plan view).
[0031] The gate protrusion 16 functions as a gate portion of the FET 100. In this example, the FET 100 is a fin FET, such as Figure 1 As shown in (b) of FIG. 8 , the gate protrusion 16 (the shaded portion rising toward the upper right) has a fin-like (linear) shape.
[0032] The height of the gate protrusion 16 (in other words, the depth of the gate recess 15) can be appropriately set, for example, to about 1 μm. It should be noted that the height of the gate protrusion 16 is the thickness of the gate portion in the current flow direction. If it is too thin (too low), it is not preferred from the perspective of current control. Therefore, the height of the gate protrusion 16, in other words, the depth of PEC etching when forming the gate protrusion 16, is preferably 500 nm or more.
[0033] A gate electrode 20 is disposed on the inner surface of the gate recess 15, at least on the side surface of the gate protrusion 16. The gate electrode 20 is disposed on the side surface of one side of the gate protrusion 16 and the side surface of the other side opposite to the side surface in a manner of sandwiching the side portion of the gate protrusion 16 from both sides. The gate electrode 20 is connected to a gate pad 21 disposed on the upper surface of the semiconductor component 10, and is connected to an external circuit via the gate pad 21.
[0034] The gate electrode 20 is used to apply a gate voltage to the side of the gate protrusion 16. By controlling the gate voltage, the carrier distribution in the gate protrusion 16 changes, and the on state and the off state of the FET 100 can be switched. As described later, the gate protrusion 16 formed by the manufacturing method of the embodiment is completely depleted, so that the FET 100 becomes a normally closed type. In other words, by applying a predetermined positive voltage to the gate electrode 20, the electrons in the gate protrusion 16 can be increased, and the FET 100 is set to the on state.
[0035] It should be noted that Figure 1 (a) and Figure 1 (b) shows an example of a Schottky-type gate electrode structure in which the gate electrode 20 is directly arranged on the side of the gate protrusion 16, but if necessary, a MOS-type gate electrode structure in which the gate electrode 20 is arranged on the side of the gate protrusion 16 through a gate insulating film may also be used.
[0036] A source electrode 30 is disposed on the upper surface of the gate protrusion 16 (on one side in the vertical direction of the gate protrusion 16). The source electrode 30 is connected to a source pad 31 disposed on the upper surface of the semiconductor component 10, and is connected to an external circuit via the source pad 31. A drain electrode 40 is disposed on the lower surface of the semiconductor component 10, in other words, on the lower surface of the substrate 11 (on the other side in the vertical direction of the gate protrusion 16).
[0037] When a predetermined voltage is applied between the source electrode 30 and the drain electrode 40 , a gate voltage is applied to the gate electrode 20 to turn on the FET 100 , thereby operating the FET 100 so that a drain current flows in the thickness direction (vertical direction) of the semiconductor component 10 .
[0038] An exemplary method for manufacturing FET 100 is described. A gate protrusion 16 is formed on the upper surface portion (on the upper surface portion of the drift layer 12) of a flat semiconductor component 10a (hereinafter referred to as a wafer 10a) on which the gate protrusion 16 has not yet been formed. By forming the gate protrusion 16 on the wafer 10a, the semiconductor component 10 is obtained. The method for manufacturing FET 100 described in the embodiment has a feature of forming the gate protrusion 16 by PEC etching, as described in detail below.
[0039] Thereafter, by appropriately using a known technique for patterning a metal film or an insulating film, other members such as the gate electrode 20 , the source electrode 30 , the drain electrode 40 and an insulating film are formed on the semiconductor member 10 , thereby manufacturing the FET 100 .
[0040] The step of forming the gate protrusion 16 by PEC etching will be described in detail. Figure 2(a) is a cross-sectional view schematically showing an object 150 to be processed in the PEC etching described in the embodiment. The object 150 to be processed has a wafer 10a and a mask 160. As described above, the wafer 10a has a substrate 11 and a drift layer 12. The mask 160 is arranged on the upper surface of the wafer 10a (the upper surface of the drift layer 12) in an area where the gate protrusion 16 is to be formed. As the mask 160, a resist mask, a hard mask, etc. can be used appropriately. The mask 160 is preferably a light-shielding property that does not allow the light 231 irradiated by the PEC etching described later to pass through.
[0041] Figure 2 (b) is a cross-sectional view schematically showing a PEC etching apparatus 200 according to an embodiment. An etching solution (electrolyte) 220 is contained in a container 210, and the object 150 is immersed in the etching solution 220. An object-side electrode 241 is arranged on the lower surface of the wafer 10a (on the lower surface of the substrate 11), and the object-side electrode 241 and the lower surface and side surface of the wafer 10a are covered by a covering member 244 such as an anti-etching layer so that they are not exposed to the etching solution 220 (so that they are not in electrical contact with the etching solution 220), and the object 150 is immersed in the etching solution 220. As a result, the opening area of the mask 160 on the upper surface of the wafer 10a (the upper surface of the drift layer 12) is selectively exposed to the etching solution 220.
[0042] As the etching liquid 220, an etching liquid (potassium hydroxide aqueous solution, phosphoric acid aqueous solution, etc.) that can perform PEC etching on the semiconductor material constituting the wafer 10a (more specifically, the semiconductor material constituting the drift layer 12) can be appropriately used. The etching liquid 220 can be alkaline or acidic as needed. As described later, the pH of the etching liquid 220 is appropriately adjusted according to the width W of the gate protrusion 16, and the etching liquid 220 corresponding to the appropriate pH is used.
[0043] One end of a wiring 242 (covered with insulation) is connected to the object-side electrode 241. An etchant-side electrode 243 is attached to the other end of the wiring 242, and the etchant-side electrode 243 is immersed in the etchant 220. A voltage source 240 is disposed in the middle of the wiring 242. A predetermined etching voltage for PEC etching is applied between the object-side electrode 241 and the etchant-side electrode 243, in other words, between the wafer 10a and the etchant 220 by the voltage source 240.
[0044] With etching voltage applied between wafer 10a and etching solution 220, light 231 for PEC etching is irradiated from light source 230 onto the upper surface of wafer 10a, in other words, onto the upper surface of drift layer 12 to be etched. In this way, PEC etching is performed on wafer 10a.
[0045] Figure 3 (a)~ Figure 3 (c) is a schematic cross-sectional view showing the wafer 10a and the vicinity of the mask 160 of the semiconductor component 10 during PEC etching according to the embodiment. Figure 3 As the etching voltage, a voltage is applied that is positive on the wafer 10a side and negative on the etching liquid 220 side. As the light 231, light having a wavelength corresponding to energy greater than the band gap of the semiconductor material constituting the upper surface of the wafer 10a as the region to be etched is irradiated.
[0046] A depletion layer 10D (the shadow portion rising to the upper right) is formed on the upper surface of the wafer 10a. Photoexcitation is achieved by irradiating the upper surface of the wafer 10a with light 231, so that electrons and holes are generated in pairs in the surface layer of the upper surface. By applying a negative voltage to the etching solution 220, the holes are induced to the upper surface side of the wafer 10a (the etching solution 220 side). The semiconductor material is oxidized by the holes, and the oxide is dissolved in the etching solution, thereby etching. In the example where the wafer 10a is composed of GaN, GaN is decomposed into gallium (Ga) and nitrogen (N) due to the holes, and gallium is oxidized by the oxygen contained in the etching solution 220 to generate gallium oxide, which is dissolved in the acidic or alkaline etching solution 220, thereby etching. The electrons generated in pairs with the holes are induced to the lower surface side of the wafer 10a.
[0047] Reference Figure 3 (b). The gate recess 15 is formed by etching the outer portion of the mask 160 (when viewed from above) of the wafer 10a, thereby forming the gate protrusion 16 below the mask 160 (the gate protrusion 16 remains below the mask 160). As the etching of the bottom surface of the gate recess 15 progresses (the gate recess 15 becomes deeper), the etching of the side surfaces of the gate protrusion 16, which are the side surfaces of the gate recess 15, also progresses. In other words, as the etching of the side surfaces 16a and 16b of the gate protrusion 16 that are opposite to each other progresses, the width of the gate protrusion 16 becomes narrower.
[0048] In order to easily irradiate the side 16a and the side 16b of the gate protrusion 16 with light 231, the light 231 preferably has a light component that is incident obliquely with respect to the upper surface of the wafer 10a. In addition, by etching the side 16a and the side 16b, the width of the gate protrusion 16 becomes narrower than the width of the mask 160. Therefore, it is preferable to form the mask 160 slightly wider than the width W of the gate protrusion 16 to be finally obtained.
[0049] Holes move by diffusing in the undepleted region of the wafer 10a. When the width of the gate protrusion 16 is sufficiently wide, specifically, when an undepleted region remains between the depletion layer 10D formed on the side 16a and the depletion layer 10D formed on the side 16b in the gate protrusion 16, the holes move in this region, thereby etching the side 16a and the side 16b.
[0050] Reference Figure 3 (c) When the width of the gate protrusion 16 is narrowed until the total width of the gate protrusion 16 reaches the width W of the depletion layer 10D, holes cannot move, and etching of the side surfaces 16a and 16b stops automatically.
[0051] After the width of gate protrusion 16 reaches width W and etching of side surfaces 16a and 16b is stopped, if etching proceeds until the depth of gate recess 15 reaches a predetermined depth, irradiation with light 231 is stopped and PEC etching is terminated.
[0052] The FET 100 of this example is a fin FET, and the mask 160 includes a linear portion (in plan view). In the PEC etching step, the gate protrusion 16 including a linear portion having a narrowest width W of 200 nm to 2000 nm (in plan view) is formed.
[0053] As described above, the process of forming the gate protrusion 16 by PEC etching (the manufacturing method of the semiconductor component 10 described in the embodiment) includes: a process of preparing the processing object 150; and a process of immersing the processing object 150 in the etching liquid 220 and irradiating the light 231 from the upper surface side of the wafer 10a, thereby performing PEC etching on the wafer 10a.
[0054] In the process of PEC etching the wafer 10a, the outer portion of the mask 160 of the wafer 10a is etched to form a gate protrusion 16 under the mask 160, and the side 16a and the side 16b are etched until the total width between the side 16a and the side 16b opposite to each other of the gate protrusion 16 is exhausted, thereby automatically stopping the etching of the side 16a and the side 16b.
[0055] The width W of the gate protrusion 16 formed by the embodiment is determined by the width of the depletion layer 10D. As described below, the width of the depletion layer 10D is determined by the carrier concentration of the semiconductor component 10, more specifically, the portion (the drift layer 12 in this example) where the gate protrusion 16 is to be formed, and the pH of the etching solution 220. Therefore, even if there is an error in the size of the mask 160, the width W of the gate protrusion 16 can be precisely controlled according to the carrier concentration and the pH of the etching solution 220.
[0056] In a fin FET type power device, a threshold voltage for switching on / off is determined by the width W of the gate protrusion 16 as a gate portion. Therefore, it is preferable to precisely control the width W. A preferable width W is estimated as follows.
[0057] The semiconductor member 10 is made of GaN and the gate electrode 20 is made of gold (Au). The depletion layer width W in the Schottky junction is D It is expressed by the following mathematical formula 1:
[0058]
[0059] Here, ε r is the relative dielectric constant of GaN, 9.5, and ε0 is the dielectric constant of vacuum, 8.85×10- 12 F / m, Φ bi is the built-in potential, V is the applied voltage, and q is the elementary charge 1.60×10- 19 C,n is the carrier concentration of GaN.
[0060] Built-in potential Φ bi It is expressed by the following mathematical formula 2:
[0061] Φ=ΦB-kt·log(Nc / n)···(2)
[0062] Here, Φ B is the Schottky barrier at the contact between GaN and Au, 1 eV, and k is the Boltzmann constant, 1.38 × 10 -23 J / K, t is the absolute temperature 300K, N C The effective state density of the conduction band of GaN is 2.59×10 24 / m 3 .
[0063] The depletion layer width W D The width W of the gate protrusion 16 is formed to be twice of that of the gate electrode 20 , so that when a voltage V is applied to the gate electrode 20 , the total width of the gate protrusion 16 is depleted. Figure 6 (a) represents the Schottky barrier Φ B The depletion layer width W at each carrier concentration n at 1 eV D A table showing the dependence of the value twice of (in other words, the value of the width W of the fully depleted gate protrusion 16) on the applied voltage V.
[0064] The carrier concentration n is changed to 5×10 15 / cm 3 , 8×10 15 / cm 3 , 1×10 16 / cm 3and 2×10 16 / cm 3 The applied voltage V changes from +0.2V to -0.35V in 0.05V (50mV) increments. The width W is expressed in nm. A carrier concentration n of 5×10 15 / cm 3 And 2.5kV withstand voltage, 1×10 16 / cm 3 And 1.5kV voltage-resistant GaN power device.
[0065] For a specific carrier concentration n, when the width W of the gate protrusion 16 is the value in the table, the fin FET is just turned off at the applied voltage V. In other words, the applied voltage V becomes the threshold. For example, when the carrier concentration n is 1×10 16 / cm 3 By setting the width W to 600 nm, when the applied voltage V is 0, the entire width W is depleted and the fin FET is in an off state.
[0066] Consider the case of a design that is exactly in the off state (open) when the applied voltage V is 0. Figure 6 (b) is a table showing the allowable error of the width W of the gate protrusion 16 when the allowable error of the threshold voltage is ±50mV and when the allowable error of the threshold voltage is ±100mV. When the allowable error of the threshold voltage is ±50-100mV, the allowable error of the width W of the gate protrusion 16 becomes ±10-50nm. It is very difficult to suppress the allowable error of the width W of the gate protrusion 16 to such a low level in conventional photolithography.
[0067] In the embodiment, as described above, the gate protrusion 16 is formed by PEC etching. The barrier height of the semiconductor component 10 in contact with the etching solution 220 is controlled by the pH of the etching solution 220. Therefore, the depletion layer width W in PEC etching is D In other words, the width W of the formed gate protrusion 16 is controlled according to the pH of the etching solution 220 .
[0068] More specifically, by using the Schottky barrier Φ in the Schottky electrode structure to be fabricated B By adjusting the pH of the etching solution 220 in a similar manner, the depletion layer width W in the PEC etching can be reduced to D The depletion layer width W when the applied voltage V = 0 in the Schottky electrode structure D In this way, it is possible to form a gate protrusion 16 having a width W that is just enough to be in an off state when the applied voltage V is 0 when the Schottky electrode structure is formed.
[0069] As described above, the width W of the gate protrusion 16 described in the embodiment can be precisely controlled according to the carrier concentration n and the pH of the etching solution 220. It should be noted that in the existing growth technology, the deviation of the carrier concentration n within the wafer surface can be set to an average of about ±2%. For example, when the carrier concentration n is 1×10 16 / cm 3 In the case of ±2%, the error of the width W within the wafer surface is ±6 nm, and can be set to ±10 nm or less.
[0070] For example, in a comparative embodiment in which ultraviolet lithography using a stepper and dry etching are combined to form the gate protrusion 16, the yield of the element remains at about 50%. In contrast, in the gate protrusion 16 formed by PEC etching in the above-mentioned embodiment, the error of the width W can be suppressed to less than ±10 nm, thereby achieving an improvement in the yield.
[0071] In the comparative embodiment using dry etching, there is a concern about damage to the semiconductor crystal caused by dry etching. In contrast, in the embodiment, the gate protrusion 16 is formed by PEC etching which is wet etching, so the damage to the semiconductor crystal is suppressed. In addition, in the embodiment, the width W can be determined by automatically stopping the etching related to the width direction of the gate protrusion 16. Furthermore, in the embodiment, the fully depleted gate protrusion 16 can be formed, so the obtained FET 100 can be set to a normally closed type.
[0072] Next, a FET 100 according to a modified example of the above-described embodiment will be described. Figure 4 (a) and Figure 4 (b) are a cross-sectional view and a top view schematically showing the FET 100 according to the first modification example, respectively.
[0073] In the above embodiment, the FET 100 having a Schottky type (or MOS type) gate electrode structure is exemplified. The gate electrode structure is not limited to these. As a first modification, the FET 100 having a pn type gate electrode structure is exemplified.
[0074] In the first modification, a semiconductor layer 13 (a shadow portion rising to the left) having a conductivity type opposite to that of the drift layer 12 (in other words, p-type) is filled in the gate recess 15. The gate electrode 20 is formed on the semiconductor layer 13. The gate voltage is applied to the pn junction formed by the semiconductor layer 13 and the gate protrusion 16 via the semiconductor layer 13.
[0075] The manufacturing method of the FET 100 described in the first modification is the same as that of the above embodiment until the step of forming the gate protrusion 16. After the gate protrusion 16 is formed, the semiconductor layer 13 is formed by, for example, regrowth. It should be noted that, if necessary, polishing can be performed to flatten the upper surface of the semiconductor component 10 on which the semiconductor layer 13 is grown. Thereafter, by forming other components such as the gate electrode 20, the source electrode 30, the drain electrode 40 and the insulating film on the semiconductor component 10, the FET 100 described in the first modification is manufactured.
[0076] Figure 5 : is a schematic top view of the FET 100 described in the second variant. In the above embodiment, the FET 100 having a fin-shaped (linear) gate protrusion 16 is exemplified. The shape of the gate protrusion 16 is not limited thereto. As a second variant, the FET 100 (nanorod transistor) having a rod-shaped (island-shaped) gate protrusion 16 is exemplified. In the nanorod transistor, a gate electrode 20 is formed that surrounds the entire circumference of the gate protrusion 16 (when viewed from above).
[0077] Regarding the manufacturing method of the FET 100 described in the second variant, the process of forming the gate protrusion 16 is different from that in the above embodiment. In this example, the mask 160 includes an island-shaped portion (when viewed from above). In the PEC etching process, a gate protrusion 16 including an island-shaped portion is formed, and the width W of the narrowest part of the island-shaped portion (when viewed from above) is greater than 200nm and less than 2000nm. After the gate protrusion 16 is formed, other components such as the gate electrode 20, the source electrode 30, the drain electrode 40 and the insulating film are formed on the semiconductor component 10, thereby manufacturing the FET 100 described in the second variant.
[0078] The FET 100 according to the first and second modified examples also has the same advantages as in the above-described embodiment, such as forming the fully depleted gate protrusion 16 by PEC etching, and being able to precisely control the width W.
[0079] <Preferred Mode of the Invention>
[0080] Hereinafter, preferred embodiments of the present invention will be described.
[0081] (Note 1)
[0082] A method for manufacturing a semiconductor component comprises the following steps:
[0083] a step of preparing a process object, the process object comprising a wafer made of a conductive semiconductor and a mask arranged on an upper surface of the wafer; and
[0084] a step of performing photoelectrochemical etching on the wafer by immersing the object to be processed in an etching solution and irradiating light from the upper surface side of the wafer,
[0085] In the process of photoelectrochemically etching the wafer,
[0086] The outer portion of the mask of the wafer is etched to form a convex portion below the mask.
[0087] The etching of the first side surface and the second side surface of the protrusion facing each other is automatically stopped by etching until the total width between the first side surface and the second side surface is exhausted.
[0088] (Note 2)
[0089] The method for manufacturing a semiconductor component according to Supplement 1, wherein the mask includes a linear portion,
[0090] In the step of performing photoelectrochemical etching on the wafer, the convex portion including a linear portion is formed, wherein the width of the narrowest portion of the linear portion is greater than or equal to 200 nm and less than or equal to 2000 nm.
[0091] (Note 3)
[0092] The method for manufacturing a semiconductor component according to Supplement 1, wherein the mask includes an island-shaped portion,
[0093] In the step of performing photoelectrochemical etching on the wafer, the convex portion including an island-shaped portion is formed, and the width of the narrowest portion of the island-shaped portion is greater than or equal to 200 nm and less than or equal to 2000 nm.
[0094] (Note 4)
[0095] The method for manufacturing a semiconductor component according to any one of Supplementary Notes 1 to 3, further comprising the following step:
[0096] A gate electrode for applying a gate voltage is formed on the side surface of the protrusion, a source electrode is arranged on one side of the protrusion in the vertical direction, and a drain electrode is arranged on the other side of the protrusion in the vertical direction.
Claims
1. A method for manufacturing a semiconductor component, comprising the following steps: a step of preparing a process object, the process object including a wafer made of a conductive semiconductor and a mask arranged on an upper surface of the wafer; and a step of performing photoelectrochemical etching on the wafer by immersing the object to be processed in an etching solution and irradiating light from the upper surface side of the wafer, In the process of photoelectrochemically etching the wafer, The outer portion of the mask of the wafer is etched to form a convex portion below the mask, The etching of the first side surface and the second side surface of the protrusion that are opposite to each other is automatically stopped by etching until the total width between the first side surface and the second side surface is exhausted.
2. The method for manufacturing a semiconductor component according to claim 1, wherein: The mask comprises a linear portion, In the step of performing photoelectrochemical etching on the wafer, the convex portion including a linear portion is formed, and the width of the narrowest portion of the linear portion is greater than or equal to 200 nm and less than or equal to 2000 nm.
3. The method for manufacturing a semiconductor component according to claim 1, wherein: The mask comprises an island-shaped portion, In the process of performing photoelectrochemical etching on the wafer, the convex portion including an island-shaped portion is formed, and the width of the narrowest portion of the island-shaped portion is greater than or equal to 200 nm and less than or equal to 2000 nm.
4. The method for manufacturing a semiconductor component according to any one of claims 1 to 3, further comprising the following step: A gate electrode for applying a gate voltage to the side surface of the protrusion, a source electrode arranged on one side of the protrusion in the vertical direction, and a drain electrode arranged on the other side of the protrusion in the vertical direction are formed.