Battery infiltration method, secondary battery and electric equipment
By adopting exponential attenuation pulse voltage charging processing in the battery, the problem that the pole-chip infiltration method in the prior art cannot take into account the infiltration rate and high capacity and high voltage characteristics, and the battery is quickly immersed and avoided the pole-chip overcharging and lithium excretion. The infiltration rate and battery performance of the pole sheet are significantly improved.
Patent Information
- Application Number
- CN202410932228.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-11
Smart Images

Figure CN119008830A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery manufacturing, and in particular to a battery impregnation method, a secondary battery and an electrical device. Background Art
[0002] Pole plate wetting refers to the process of electrolyte spreading on the surface of the electrode plate. The effect of pole plate wetting is directly related to the performance of the battery. Poor pole plate wetting may lead to a lack of internal electrolyte, which in turn causes negative electrode problems.
[0003] In the prior art, the wettability of the electrode is provided by increasing the thermal motion energy of the electrolyte molecules and changing the contact angle between the electrolyte and the electrode. However, the above methods have many restrictions and cannot effectively take into account the wetting rate and the high capacity and high voltage characteristics of the battery. Summary of the invention
[0004] The technical problem to be solved by the present application is to provide a battery infiltration method, a secondary battery and an electrical device to solve the problem that the existing electrode infiltration method cannot effectively take into account both the infiltration rate and the high capacity and high voltage characteristics of the battery.
[0005] In order to solve the above problems, the present application is implemented through the following technical solutions:
[0006] The present application proposes a battery impregnation method, which includes:
[0007] injecting electrolyte into a battery including a positive electrode sheet and a negative electrode sheet;
[0008] After the liquid injection is completed, the battery is subjected to an exponential decay pulse voltage charging process;
[0009] The DCR of the battery is monitored, and when the DCR is less than a preset resistance threshold, the exponential decay pulse voltage charging process for the battery is stopped.
[0010] Furthermore, in the battery infiltration method, the amplitude of the exponential decay pulse voltage satisfies: P(t)=P0(i)·et / τ;
[0011] Among them, P(t) is the amplitude of the pulse voltage at time t, in V; P0(i) is the i-th initial amplitude of the pulse voltage, in V, i is 1, 2, 3; e is the base of the natural logarithm; t is time, in s; τ is the decay time constant of the pulse voltage, in s.
[0012] Furthermore, in the battery infiltration method, the second initial amplitude is 3 to 48V.
[0013] Furthermore, in the battery infiltration method, the step of performing exponential decay pulse voltage charging treatment on the battery includes:
[0014] Using a first exponential decay pulse voltage to perform charging until the DCR of the battery is 50% of its initial DCR;
[0015] After the charging by the first exponential decay pulse voltage is completed, a second exponential decay pulse voltage is used for charging until the DCR of the battery is 25% of its initial DCR;
[0016] After the charging by the second exponential decay pulse voltage is completed, a third exponential decay pulse voltage is used for charging until the DCR of the battery is less than the preset resistance threshold.
[0017] Further, a first initial amplitude of the first exponentially decayed pulse voltage is smaller than a second initial amplitude of the second exponentially decayed pulse voltage, and the second initial amplitude is smaller than a third initial amplitude of the third exponentially decayed pulse voltage.
[0018] Furthermore, the capacity of the battery is 20-1000 Ah, and the first initial amplitude and the capacity of the battery satisfy:
[0019] z=(-3*10 -05 *x 2 +0.0723*x+4.3499)*3;
[0020] Wherein, x is the capacity of the battery, in Ah; z is the first initial amplitude, in V.
[0021] Furthermore, in the battery infiltration method, the first initial amplitude is 4 to 6V; the second initial amplitude is 10 to 15V; and the third initial amplitude is 25 to 37.5V.
[0022] Furthermore, the preset resistance threshold and the capacity of the battery satisfy: y=-5*10 -08 *x 3 +4*10 -05 *x 2 -0.014*x+2.6895;
[0023] Wherein, y is the preset resistance threshold, in mΩ.
[0024] Furthermore, in the battery impregnation method, during the process of exponential decay pulse voltage charging treatment of the battery, the ambient temperature is 25-70°C.
[0025] Furthermore, in the battery infiltration method, the preset resistance threshold is 0.2 to 5 mΩ.
[0026] The present application also proposes a secondary battery, which is obtained by processing the above method.
[0027] The present application also proposes an electrical device, comprising the above-mentioned secondary battery, wherein the secondary battery serves as a power supply for the electrical device.
[0028] Compared with the prior art, the embodiments of the present application have the following advantages:
[0029] In the embodiment of the present application, the provided battery infiltration method uses an exponentially decaying pulse voltage to form an electric field between the positive electrode plate and the negative electrode plate, and converts electrical energy into internal energy of the electrolyte, replenishes the energy dissipated by the dynamic advancement of the electrolyte in the electrode plate, helps the electrolyte overcome the interface energy between the electrode plate, and allows the electrolyte to quickly spread on the electrode plate, thereby achieving the purpose of accelerated infiltration, realizing rapid infiltration of the battery after liquid injection, and breaking through the bottleneck of difficult infiltration of thick electrode plates; at the same time, the energy of the exponentially decaying pulse voltage naturally decays, which can effectively avoid the phenomenon of overcharging and lithium precipitation of the electrode plate, so this method can effectively take into account the high infiltration rate of the battery and the high capacity and high voltage characteristics of the battery.
[0030] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a flow chart of the battery infiltration method provided in the embodiment of the present application.
[0032] Figure 2 It is a schematic diagram of exponentially decaying pulse voltage charging of the battery infiltration method provided in an embodiment of the present application. DETAILED DESCRIPTION
[0033] In order to make the above-mentioned objects, features and advantages of the present application more obvious and easy to understand, the present application is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0034] The applicant of this application found that the electrode wetting effect is directly related to the performance of the battery. Poor electrode wettability may lead to a lack of internal electrolyte, which in turn causes negative electrode problems. In order to improve the energy density of battery cells, the existing technology often uses large-size structures and high-capacity and high-voltage materials, but the above design easily affects the electrode wetting effect, resulting in a lack of internal electrolyte, which in turn causes serious negative electrode problems.
[0035] Although the wettability of the electrode can be improved by increasing the thermal motion energy of electrolyte molecules and changing the contact angle between the electrolyte and the electrode, the above methods have many restrictions and cannot effectively take into account the efficiency of the wetting rate and the high-capacity and high-voltage characteristics of the battery.
[0036] In order to solve the above problems, the present application embodiment provides a battery impregnation method, such as Figure 1 As shown, it includes steps 101 to 103:
[0037] Step 101: inject electrolyte into a battery including a positive electrode plate and a negative electrode plate.
[0038] In the above step 101, the above battery can be a square shell battery, a cylindrical battery, a soft pack battery or a special-shaped battery.
[0039] In the above step 101, the above battery may be a wound battery or a laminated battery.
[0040] In the above step 101, the above battery may be a sealed battery or an unsealed battery.
[0041] In the above step 101, the above battery can be a lithium ion battery or a sodium ion battery. The above method is applicable to various electrodes, the above positive electrode plate includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes one or more of lithium iron phosphate material, ternary material, lithium manganate material, and lithium cobalt oxide material.
[0042] In the above step 101, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer arranged on the negative electrode current collector, and the above negative electrode active material layer is selected from non-metallic negative electrode materials; the non-metallic negative electrode material is preferably any one of hard carbon, soft carbon, graphite, silicon monoxide, or a combination of at least two of them, or a graphite material, a silicon-carbon material, etc.
[0043] In practical applications, the negative electrode sheet, the separator and the positive electrode sheet are stacked in order and wound to obtain a winding core, and the winding core is packaged to obtain a bare cell. After the bare cell is baked, the above step 101 can be performed, that is, the liquid injection operation is performed.
[0044] Step 102: After the liquid injection is completed, the battery is subjected to exponentially decayed pulse voltage charging.
[0045] In the above step 102, after the electrolyte injection is completed, the positive / negative poles of the pulse current generating device are respectively connected to the above positive electrode plate / negative electrode plate, and then an exponential decay pulse voltage is continuously applied to the battery for charging. The exponential decay pulse voltage can construct an electric field inside the battery, and the lithium ions in the battery electrolyte move in the electric field to obtain kinetic energy. This kinetic energy can not only replenish the energy dissipation such as viscous dissipation and friction dissipation caused by the electrolyte in the process of wetting the electrode plate at the solid / liquid interface, but also directly promote the electrolyte to spread on the electrode plate, so that the electrode plate infiltration rate is greatly improved, and the infiltration of lithium ions into the electrode plate is accelerated, thereby shortening the infiltration time. At the same time, because the energy of the exponential decay pulse voltage will naturally decay, the energy of driving the lithium ions in the electrolyte to overcome the interface energy between the electrolyte and the electrode plate is gradually smaller, so the electrode plate overcharge and lithium precipitation can be effectively avoided.
[0046] Step 103: monitor the DCR of the battery, and when the DCR is less than a preset resistance threshold, stop performing exponential decay pulse voltage charging processing on the battery.
[0047] In the above step 103, since the DCR of the battery is directly related to its infiltration state, it is possible to determine whether the infiltration is complete by monitoring the DCR of the battery, and when it is determined that the infiltration is complete, stop the exponential decay pulse voltage charging process on the battery, that is, complete the battery infiltration process.
[0048] In the above step 103, the preset resistance threshold is used to characterize that the battery infiltration is complete, that is, the above preset resistance threshold is the DC internal resistance value when the battery infiltration is complete. Therefore, when the DCR of the battery is less than the preset resistance threshold, it can be determined that the electrolyte has completed the infiltration of the electrode, and thus the exponential decay pulse voltage charging process of the battery is stopped.
[0049] Optionally, in a specific embodiment, the preset resistance threshold is 0.2 to 5 mΩ, for example, it can be a range value of one or any two of 0.2 mΩ, 0.3 mΩ, 0.5 mΩ, 0.8 mΩ, 1.0 mΩ, 1.5 mΩ, 2.0 mΩ, 3.0 mΩ, 4.0 mΩ, and 5.0 mΩ.
[0050] Optionally, in another specific implementation manner, the above-mentioned preset resistance threshold and battery capacity satisfy: y = -5*10 -08 *x 3 +4*10 -05 *x 2 -0.014*x+2.6895;
[0051] Among them, y is the preset resistance threshold, the unit is mΩ; x is the battery capacity, and the value of x is 20~1000Ah.
[0052] In this specific implementation, the resistance threshold for completion of infiltration is determined in advance based on the actual capacity calibration of the battery, so that the infiltration state can be judged more accurately during subsequent electrolyte infiltration, and when it is determined that the electrolyte has completed infiltration of the electrode, the exponential decay pulse voltage charging treatment of the battery is stopped in time.
[0053] The method provided in the embodiment of the present application, the exponentially decaying pulse voltage can not only continuously form an electric field between the positive electrode plate and the negative electrode plate, so as to convert the electrical energy into the internal energy of the electrolyte under the action of the electric field force, and replenish the energy dissipated by the dynamic advancement of the electrolyte in the electrode plate, but also help the electrolyte to overcome the interface energy between the electrode plate and the electrode plate, so that the electrolyte can quickly spread on the electrode plate, thereby achieving the purpose of accelerated wetting, realizing rapid wetting of the battery after liquid injection, and breaking through the bottleneck of difficult wetting of thick electrode plates; at the same time, the energy of the exponentially decaying pulse voltage decays naturally, which can effectively avoid overcharging and lithium precipitation of the electrode plate.
[0054] The battery wetting method provided in the embodiment of the present application can significantly increase the wetting rate of the pole piece, reduce the aging waiting time after injection, and thus reduce the time cost. Therefore, the wetting method provided in the embodiment of the present application solves the problem that the existing pole piece wetting method cannot effectively take into account the wetting rate and the high capacity and high voltage characteristics of the battery.
[0055] Optionally, in one embodiment, the amplitude of the exponential decay pulse voltage satisfies: P(t)=P0(i)·et / τ;
[0056] Among them, P(t) is the amplitude of the pulse voltage at time t, in V; P0(i) is the i-th initial amplitude of the pulse voltage, in V, i is 1, 2, 3; e is the base of the natural logarithm; t is time, in s; τ is the decay time constant of the pulse voltage, in s.
[0057] In this embodiment, the battery is charged using an exponentially decaying pulse voltage with an amplitude P(t) satisfying P(t)=P0(i)·et / τ, which can not only match the actual energy demand of the battery, but also effectively avoid lithium deposition caused by overcharging of the electrode.
[0058] The decay time constant τ is determined by the product of the pulse capacitance and the resistance, reflecting the decay of the pulse voltage from the initial amplitude to e -1 The duration required for V.
[0059] Optionally, in one embodiment, the time constant τ satisfies 10 -3 ≤τ≤1, for example, it can be 0.1.
[0060] Optionally, in one embodiment, the above-mentioned initial amplitude is 3 to 48V, that is, during the entire pulse charging process, the initial amplitude of the exponentially decaying pulse voltage is in the range of 3 to 48V, for example, it can be one of 3V, 4V, 5V, 8V, 10V, 15V, 20V, 25V, 30V, 40V, 48V or any two of the range values.
[0061] Optionally, in one embodiment, the step of performing exponential decay pulse voltage charging on the battery includes steps 201 to 203:
[0062] Step 201, using a first exponential decay pulse voltage to perform charging processing until the DCR of the battery is 50% of its initial DCR;
[0063] Step 202: After the charging by the first exponential decay pulse voltage is completed, a second exponential decay pulse voltage is used for charging until the DCR of the battery is 25% of its initial DCR;
[0064] Step 203: After the charging by the second exponential decay pulse voltage is completed, a third exponential decay pulse voltage is used for charging until the DCR of the battery is less than the preset resistance threshold.
[0065] In some embodiments, a first initial amplitude of the first exponentially decayed pulse voltage is smaller than a second initial amplitude of the second exponentially decayed pulse voltage, and the initial amplitude is smaller than a third initial amplitude of the third exponentially decayed pulse voltage.
[0066] In step 201, the initial DCR is the DCR of the aging test directly formed after the battery is filled with liquid; before the DCR of the battery is reduced to 50% of its initial DCR, the interface resistance between the electrolyte and the electrode is relatively small, and the energy dissipated by the dynamic advancement of the electrolyte in the electrode is relatively small, so the first exponential decay pulse voltage with a relatively small initial amplitude is used for charging.
[0067] In step 202, after the DCR of the battery is reduced to 50% of its initial DCR, the interfacial resistance between the electrolyte and the electrode will increase significantly, so that the energy dissipated by the dynamic advancement of the electrolyte in the electrode will also increase significantly. Therefore, in order to maintain the infiltration rate, the required energy to be replenished also needs to increase rapidly, so a second exponential decay pulse voltage with a larger initial amplitude is used for charging.
[0068] In step 203, after the DCR of the battery is reduced to 25% of its initial DCR, the interfacial resistance between the electrolyte and the electrode will further increase, so that the energy dissipated by the dynamic advancement of the electrolyte in the electrode will also further increase. Therefore, in order to maintain the wetting rate, more energy needs to be replenished, and thus a third exponential decay pulse voltage with a larger initial amplitude is used for charging.
[0069] In this embodiment, considering that the interface resistance between the electrolyte and the electrode gradually increases with the infiltration, the energy dissipated by the dynamic advancement of the electrolyte in the electrode also gradually increases. In order to maintain the infiltration rate, the required energy to be replenished also gradually increases. Therefore, an exponentially decaying pulse voltage with an increasing initial amplitude is set to charge the battery in sequence, which can alleviate the problem of the gradual decrease in the infiltration rate due to the gradual increase in interface resistance.
[0070] Optionally, in one implementation, the ratio of the second initial amplitude to the first initial amplitude is a, and the ratio of the third initial amplitude to the second initial amplitude is b; wherein, 1 <a≤10,1<b≤10。
[0071] In this specific embodiment, taking into account that the interfacial resistance between the electrolyte and the electrode gradually increases with the infiltration, the energy dissipated by the dynamic advancement of the electrolyte in the electrode also gradually increases. In order to maintain the infiltration rate, the energy required to be replenished also gradually increases. Therefore, when two adjacent charging treatments are set, the initial amplitude of the exponentially decaying pulse voltage is increased by a factor of 1 to 10, which can effectively replenish the gradually increasing energy dissipation of the electrolyte in the dynamic advancement of the electrode, offset the problem of the gradual increase in the interfacial resistance between the electrolyte and the electrode due to the continuous increase in the infiltration range, resulting in a gradual decrease in the infiltration rate, thereby effectively promoting the dynamic advancement of the electrolyte in the electrode and accelerating the overall infiltration rate.
[0072] Optionally, in a specific implementation, the first initial amplitude is 4-6V, the second initial amplitude is 10-15V, and the third initial amplitude is 25-37.5V.
[0073] In this specific implementation manner, the first initial amplitude is set to 4-6V, the second initial amplitude is set to 10-15V, and the third initial amplitude is set to 25-37.5V.
[0074] Optionally, in another specific implementation, when the battery capacity is 20-1000 Ah, the first initial amplitude and the battery capacity satisfy:
[0075] z=(-3*10 -05 *x 2 +0.0723*x+4.3499)*3;
[0076] Wherein, x is the battery capacity in Ah; z is the first initial amplitude in V.
[0077] In this specific embodiment, the first initial amplitude of the first exponentially decaying pulse voltage for charging the battery is set in advance according to its designed capacity, and then the second initial amplitude of the second exponentially decaying pulse voltage and the third initial amplitude of the third exponentially decaying pulse voltage can be determined, so that the initial amplitude of each exponentially decaying pulse voltage matches the battery capacity, which can more quickly and effectively help the electrolyte overcome the interface energy between the electrolyte and the electrode, allowing the electrolyte to quickly spread on the electrode.
[0078] Optionally, in one embodiment, during the exponential decay pulse voltage charging process of the battery, the ambient temperature is 25-70°C, which can effectively improve the infiltration rate and ensure the infiltration effect, and can avoid high temperature damage to the battery. Optionally, the above ambient temperature can be one of 25°C, 27°C, 30°C, 35°C, 40°C, 45°C, 50°C, 60°C, 70°C, or any two of the range values.
[0079] Optionally, in one embodiment, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, and the negative electrode active material layer includes a negative electrode active material.
[0080] Optionally, in a specific embodiment, the negative electrode active material may be a carbon-silicon negative electrode material, graphite or hard carbon.
[0081] Optionally, in a specific embodiment, the negative electrode plate also includes a conductive agent and a binder; optionally, the conductive agent includes one or more of conductive carbon black, acetylene black, Ketjen black, carbon nanotubes, and graphene, and the binder includes a carboxymethyl cellulose-based binder and a resin binder.
[0082] Optionally, in one embodiment, the carboxymethyl cellulose-based binder includes one or more of sodium carboxymethyl cellulose and lithium carboxymethyl cellulose; and / or the resin-based binder includes one or more of styrene-butadiene rubber, polyacrylic acid, and polyacrylonitrile.
[0083] In some embodiments, the negative electrode sheet is prepared as follows: the components for preparing the negative electrode sheet, such as the negative electrode active material, binder and conductive agent, are dispersed in a solvent such as deionized water to form a negative electrode slurry; the negative electrode slurry is coated on both sides of a negative electrode collector such as copper foil; after baking, rolling, cutting and other processes, the negative electrode sheet can be obtained.
[0084] Optionally, in one embodiment, the positive electrode plate includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes a lithium ion transition metal oxide, a ternary positive electrode material, etc. The lithium ion transition metal oxide includes at least one of lithium cobalt oxide, lithium manganese oxide, and lithium iron phosphate, and the ternary positive electrode material can specifically be a high-nickel layered ternary positive electrode material.
[0085] Optionally, in one embodiment, the positive electrode plate further includes a conductive agent, and the conductive agent may include at least one of conductive carbon black, acetylene black, Ketjen black, carbon nanotubes, graphene, hard carbon, carbon fiber, and carbon microspheres.
[0086] In some embodiments, the positive electrode sheet is prepared as follows: the components for preparing the positive electrode sheet, such as the positive electrode active material including the positive electrode material, the binder and the conductive agent are dispersed in a solvent such as N-methylpyrrolidone to form a positive electrode slurry; the positive electrode slurry is coated on a positive electrode collector such as aluminum foil; after drying, rolling, die cutting and other processes, the positive electrode sheet can be obtained.
[0087] The electrolyte plays a role in conducting ions between the positive electrode and the negative electrode, and the electrolyte can be liquid, gel or all-solid. In some embodiments, the electrolyte uses the above-mentioned electrolyte, which includes an electrolyte salt and a solvent, and the electrolyte salt is a lithium salt.
[0088] Optionally, in one embodiment, the electrolyte includes a lithium salt, an organic solvent and an additive, the additive includes fluoroethylene carbonate, the organic solvent includes at least one of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, and the lithium salt includes one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide salt, lithium bis(trifluoromethylsulfonate), lithium tetrafluoroborate, lithium perchlorate and lithium trifluoromethylsulfonate.
[0089] Optionally, in a specific embodiment, in the above electrolyte, the mass percentage of the additive is 0.1% to 2%. Optionally, the mass percentage of the additive in the electrolyte can be in the range of 0.1%, 0.2%, 0.5%, 1%, 1.5%, 2% or any two of them.
[0090] Optionally, in a specific embodiment, in the above electrolyte, the concentration of lithium salt is 0.5 to 2 mol / L. Optionally, the concentration of lithium salt in the electrolyte can be in the range of 0.5 mol / L, 0.6 mol / L, 0.8 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L or any two of them.
[0091] It can be understood that the battery provided in the embodiment of the present application also includes a separator arranged between the positive electrode plate and the negative electrode plate.
[0092] In practical applications, the negative electrode sheet, the positive electrode sheet and the separator are wound to obtain a winding core, the winding core is packaged to obtain a dry cell, and the dry cell is baked and then injected with liquid to obtain the above-mentioned battery.
[0093] The present application also proposes a secondary battery, which includes a battery, and the battery is obtained by processing the above method.
[0094] The present application also proposes an electrical device, which includes the above-mentioned secondary battery, and the secondary battery serves as a power supply for the electrical device.
[0095] For the above-mentioned secondary battery embodiment and electrical equipment embodiment, they include the above-mentioned battery, which is obtained by the above-mentioned method and can achieve the same technical effect. In order to avoid repetition, they will not be described here. For relevant matters, please refer to the partial description of the method embodiment.
[0096] The present application is described in detail below through examples.
[0097] Performance Testing Methods
[0098] (1) DCR test steps:
[0099] Step 1: Adjust the battery's state of charge (SOC) to 50% SOC.
[0100] Step 2: Discharge the battery at a rate of 0.2C for 30 seconds to eliminate the surface charge of the battery and ensure that the battery is in a stable state during the test. Discharge the battery at a rate of 1C for 5 seconds and record the initial voltage (V1) of the battery at 1C rate and the final voltage (V2) of the battery at the end of discharge.
[0101] Step 3: Calculate the DCR: Use the following formula to calculate the battery’s discharge DCR: RDCR = (V1-V2) / I
[0102] Where I is the discharge current, V1 is the initial voltage of the battery before discharge, and V2 is the end voltage after 5s of discharge.
[0103] Example 1
[0104] (1) Preparation of positive electrode sheet: The positive electrode active material lithium iron phosphate (LFP), the conductive agent acetylene black (Super P) and the binder polyvinylidene fluoride (PVDF) are mixed uniformly in a mass ratio of 96:2:2, and uniformly dispersed in 1-methyl-2-pyrrolidone (NMP) to prepare a uniform black slurry. The mixed black slurry is coated on both sides of an aluminum foil, and then baked, rolled and cut into sheets to obtain a positive electrode sheet;
[0105] (2) Preparation of negative electrode sheet: The negative electrode active material graphite, the conductive agent acetylene black (Super P) and the binder SBR are mixed uniformly in a mass ratio of 94:3:3, and evenly dispersed in deionized water to form a uniform black slurry. The mixed slurry is coated on both sides of the copper foil, and then baked, rolled and cut into pieces to obtain the negative electrode sheet;
[0106] (3) Preparation of batteries: The prepared positive electrode sheet, separator (PP separator is used as separator), and negative electrode sheet are stacked in order, with the separator located between the positive and negative electrode sheets, and a bare cell is obtained by winding, hot pressing and shaping, and welding the tabs. The bare cell is placed in an outer packaging aluminum plastic film and baked in an oven at 85±10°C for 24h. The electrolyte is injected into the dried bare cell, wherein the lithium salt of the electrolyte is 1M LiPF6, the solvent is ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate in a volume ratio of 1:1:1, and the additive is 0.5% of the total mass of the electrolyte by fluoroethylene carbonate.
[0107] (4) Under the condition of an ambient temperature of 30° C., a first exponentially decaying pulse voltage is cyclically applied between the positive electrode plate and the negative electrode plate for charging until the DCR of the battery is 50% of its initial DCR;
[0108] Wherein, the amplitude of the first exponential decay pulse voltage satisfies: P(t) = P0(i)·et / τ; P(t) is the amplitude of the pulse voltage at time t, in V; P0(i) is 5V; e is the base of the natural logarithm; t is time, in s; τ is 10 -1 , unit is s;
[0109] (5) Under the condition of an ambient temperature of 30° C., a second exponentially decaying pulse voltage is cyclically applied between the positive electrode plate and the negative electrode plate for charging until the DCR of the battery is 25% of its initial DCR;
[0110] Wherein, the amplitude of the first exponential decay pulse voltage satisfies: P(t) = P0(i)·et / τ; P(t) is the amplitude of the pulse voltage at time t, in V; P0(i) is 12.5V; e is the base of the natural logarithm; t is time, in s; τ is 10 -1 , unit is s;
[0111] (6) Under the condition of an ambient temperature of 30° C., a third exponential decay pulse voltage is cyclically applied between the positive electrode plate and the negative electrode plate for charging treatment until the DCR of the battery is less than 5 mΩ, and then the exponential decay pulse voltage charging treatment of the battery is stopped;
[0112] Wherein, the amplitude of the first exponential decay pulse voltage satisfies: P(t) = P0(i)·et / τ; P(t) is the amplitude of the pulse voltage at time t, in V; P0(i) is 35V; e is the base of the natural logarithm; t is time, in s; τ is 10 -1 , unit is s;
[0113] (7) Calculate the total infiltration time.
[0114] Example 2
[0115] The difference between Example 2 and Example 1 is that:
[0116] In step (4), the initial amplitude P0(i) of the first exponential decay pulse voltage is adjusted to 4V;
[0117] In step (5), the initial amplitude P0(i) of the second exponential decay pulse voltage is 10V;
[0118] In step (6), the initial amplitude P0(i) of the third exponential decay pulse voltage is 25.
[0119] Example 3
[0120] The difference between Example 3 and Example 1 is that:
[0121] In step (4), the initial amplitude P0(i) of the first exponential decay pulse voltage is adjusted to 6V;
[0122] In step (5), the initial amplitude P0(i) of the second exponential decay pulse voltage is 15V;
[0123] In step (6), the initial amplitude P0(i) of the third exponential decay pulse voltage is 37.5V.
[0124] Embodiment 4-5
[0125] The difference between Examples 4 to 5 and Example 1 is that in steps (4) to (6), the ambient temperature is adjusted to 25° C. and 70° C., respectively.
[0126] Comparative Example 1
[0127] The difference between Comparative Example 1 and Example 1 is that in steps (4) to (6), no exponentially decaying pulse voltage is applied for charging treatment, and the battery is simply placed in a 30° C. warm room to stand until the DCR of the battery is less than 5 mΩ.
[0128] Comparative Example 2
[0129] The difference between Comparative Example 2 and Example 1 is that in steps (4) to (6), no exponential decay pulse voltage is applied for charging, and the battery is simply placed in a 45° C. warm room until the DCR of the battery is less than 5 mΩ.
[0130] The batteries prepared in each embodiment and comparative example were subjected to battery impedance test and diffusion impedance test. The test data are shown in Table 1.
[0131] Table 1
[0132] Group Total infiltration time (min) Example 1 60 Example 2 80 Example 3 58 Example 4 65 Example 5 59 Comparative Example 1 240h Comparative Example 2 120h
[0133] It can be seen from the test results in Table 1 that the infiltration method provided in the embodiment of the present application can effectively accelerate the infiltration of the electrolyte into the electrode, shorten the infiltration time, and improve production efficiency.
[0134] In summary, in this embodiment, the battery infiltration method, after injecting electrolyte into the battery including the positive electrode plate and the negative electrode plate, performs an exponential decay pulse voltage charging treatment on the battery until the DCR of the battery is less than the resistance threshold, and the resistance threshold is used to characterize the completion of battery infiltration. Among them, the exponential decay pulse voltage can not only continuously form an electric field between the positive electrode plate and the negative electrode plate, so as to convert the electrical energy of the lithium ions in the electrolyte into kinetic energy under the action of the electric field force, replenish the energy dissipated by the dynamic advancement of the electrolyte in the electrode plate, and help the electrolyte to overcome the interface energy between the electrode plate, so that the electrolyte can be spread on the electrode plate, so as to achieve the purpose of accelerating infiltration, realize the rapid completion of infiltration of the battery after injection, and break through the bottleneck of the difficulty of infiltration of thick electrode plates; at the same time, the energy of the exponential decay pulse voltage decays naturally, which can effectively avoid the situation of overcharging and lithium precipitation of the electrode plate, thereby solving the problem that the existing electrode plate infiltration method cannot effectively take into account the infiltration rate and the high capacity and high voltage characteristics of the battery.
[0135] Although the preferred embodiments of the present application have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concepts. Therefore, the claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present application.
[0136] The battery impregnation method, secondary battery and electrical equipment provided by the present application are introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for general technicians in this field, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A battery impregnation method, characterized in that: include: injecting electrolyte into a battery including a positive electrode sheet and a negative electrode sheet; After the liquid injection is completed, the battery is subjected to an exponential decay pulse voltage charging process; The DCR of the battery is monitored, and when the DCR is less than a preset resistance threshold, the exponential decay pulse voltage charging process for the battery is stopped.
2. The battery impregnation method according to claim 1, characterized in that: The amplitude of the exponential decay pulse voltage satisfies: P(t) = P0(i)·et / τ; Wherein, P(t) is the amplitude of the pulse voltage at time t, in V; P0(i) is the i-th initial amplitude of the pulse voltage, in V, i is 1, 2, 3; e is the base of the natural logarithm; t is time, in s; τ is the decay time constant of the pulse voltage, in s.
3. The battery impregnation method according to claim 2, characterized in that: The initial amplitude is 3-48V.
4. The battery impregnation method according to claim 1, characterized in that: The step of performing exponential decay pulse voltage charging on the battery comprises: Using a first exponential decay pulse voltage to perform charging until the DCR of the battery is 50% of its initial DCR; After the charging by the first exponential decay pulse voltage is completed, a second exponential decay pulse voltage is used for charging until the DCR of the battery is 25% of its initial DCR; After the charging by the second exponential decay pulse voltage is completed, a third exponential decay pulse voltage is used for charging until the DCR of the battery is less than the preset resistance threshold.
5. The battery impregnation method according to claim 4, characterized in that: A first initial amplitude of the first exponential decay pulse voltage is smaller than a second initial amplitude of the second exponential decay pulse voltage, and the second initial amplitude is smaller than a third initial amplitude of the third exponential decay pulse voltage.
6. The battery impregnation method according to claim 5, characterized in that: The capacity of the battery is 20-1000 Ah, and the first initial amplitude and the capacity of the battery satisfy: z=(-3*10 -05 *x 2 +0.0723*x+4.3499)*3; Wherein, x is the capacity of the battery, in Ah; z is the first initial amplitude, in V.
7. The battery impregnation method according to claim 4, characterized in that: The first initial amplitude is 4-6V; the second initial amplitude is 10-15V; and the third initial amplitude is 25-37.5V.
8. The battery impregnation method according to claim 1, characterized in that: During the process of performing exponential decay pulse voltage charging on the battery, the ambient temperature is 25-70°C.
9. The battery impregnation method according to claim 6, characterized in that: The preset resistance threshold and the capacity of the battery satisfy: y = -5*10 -08 *x 3 +4*10 -05 *x 2 -0.014*x+2.6895; Wherein, y is the preset resistance threshold, in mΩ.
10. The battery impregnation method according to claim 1, characterized in that: The preset resistance threshold is 0.2-5 mΩ.
11. A secondary battery, characterized in that: The secondary battery is obtained by processing according to any one of claims 1 to 10.
12. An electrical equipment, characterized in that: The secondary battery according to claim 11 is included, and the secondary battery is used as a power supply for the electrical device.
Citation Information
Patent Citations
Non-aqueous electrolyte secondary battery charging method, electronic device, battery pack, and charging device
CN101569052A
Separator for secondary battery and method of fabricating it
JP2001155706A
Manufacturing method for nonaqueous electrolyte secondary battery
JP2005235624A
Pulse charge method for nonaqueous electrolyte secondary battery and pulse charge control device
US20100219795A1
Cited By
Battery formation method, battery and electric device