Composite current collector
By setting a base coating and conductive coating in the composite fluid collection and controlling its elongation under tensile conditions, the problem of increasing square resistance during the composite fluid collection process is solved, and efficient current collection and battery safety are achieved Performance improvement.
Patent Information
- Application Number
- CN202411146008.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-22
AI Technical Summary
The existing composite fluids tend to increase the surface resistance during the treatment process, affecting the conductivity and efficiency and stability of the battery system.
The composite fluid of the base coating and the conductive coating is provided on the support film. Under the tensile conditions, the total mass of the base coating is M1 and the total mass of the conductive coating is M2. After forming the base coating, it is stretched. The elongation amount is X, and the tensile elongation amount after forming a conductive coating is Y, which satisfies M1/X < M2/Y, ensuring that the square resistance of the composite fluid collector is within 20 millioohms-40 millioohms.
By controlling the mass dispersion of the primer and conductive coatings, the square resistance is reduced, the overcurrent capability and current convergence capability of the composite fluid are improved, the total mass of the battery is reduced, and the safety performance of the battery is enhanced.
Smart Images

Figure CN119008969A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of current collectors, and in particular to a composite current collector. Background Art
[0002] In lithium-ion batteries, current collectors mainly refer to metal foils, such as copper foil and aluminum foil, which carry the active materials of the positive and negative electrodes and collect current for external output. The main function of the current collector is to collect the current generated by the active materials of the battery in order to form a larger current for external output. Therefore, the current collector should be in full contact with the active material, and the internal resistance should be as small as possible.
[0003] The current collector usually has good electrical conductivity and mechanical strength. It is responsible for carrying the active materials of the positive and negative electrodes, and collects the current generated by the electrochemical reaction for external output. At the same time, the current collector can also effectively disperse and transfer the heat generated inside the battery cell, improve the heat dissipation effect of the battery cell, and help maintain the temperature stability of the battery cell. The physicochemical properties of the current collector greatly affect the performance of lithium batteries. The main physical indicators of the current collector include thickness, thickness uniformity, surface density, surface roughness, tensile strength, elongation and porosity, and the chemical indicators include oxidation resistance, corrosion resistance and heat resistance. In lithium-ion batteries, copper foil and aluminum foil are commonly used current collector materials. Copper foil is usually used as a negative electrode current collector because copper is easily oxidized at a higher potential, but copper foil remains stable with lithium ions, which is conducive to current transmission. Aluminum foil is often used as a positive electrode current collector because of its high oxidation potential and dense oxide film on the surface.
[0004] With the development of science and technology, composite current collectors have gradually attracted attention as a new generation of current collector materials. The composite current collector has a sandwich structure, with a polymer layer in the middle and metal films on the top and bottom, and has better safety performance and energy density. After the composite current collector is produced, it is necessary to perform coating, rolling and other operations on the composite current collector. The current composite current collector needs to stretch the film for operation during such processing, but in the process of doing so, it is easy to increase the surface resistance of the composite current collector. The increase in square resistance will not only affect the conductive properties of the composite current collector, but may also have a negative impact on the efficiency and stability of the entire battery system. Therefore, the existing technology needs to be improved and improved. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, an object of the present invention is to provide a composite current collector.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] The present invention provides a composite current collector, comprising a support film, a primer coating is arranged on the support film, a conductive coating is arranged on the primer coating, the total mass of the primer coating is M1, the total mass of the conductive coating is M2, the composite current collector, after the primer coating is formed and before the conductive coating is formed, under tension conditions, its tensile elongation is X; after the conductive coating is formed, under the same tension conditions, its tensile elongation is Y, wherein M1 / X <M2 / Y。
[0008] Furthermore, in the composite current collector, the conductive coating is a metal layer.
[0009] Furthermore, in the composite current collector, the mass of the conductive coating per unit area is smaller than the mass of the support film per unit area.
[0010] Furthermore, in the composite current collector, the mass of the primer coating per unit area is smaller than the mass of the support film per unit area.
[0011] Furthermore, for the composite current collector, the mass of the primer coating per unit area is M3, the mass of the conductive coating per unit area is M4, and the thermal shrinkage rate of the composite current collector after forming the primer coating and before forming the conductive coating under thermal shrinkage conditions is X1; the thermal shrinkage rate of the composite current collector after forming the conductive coating under the same thermal shrinkage conditions is Y1, and M3 / X1>M4 / Y1.
[0012] Furthermore, for the composite current collector, the transmittance of the primer coating is between 96% and 98%.
[0013] Furthermore, the composite current collector has a square resistance within 20 milliohms to 40 milliohms under tension. The primer coating is a magnetron sputtering layer or a vacuum evaporation layer.
[0014] Furthermore, in the composite current collector, the conductive coating is a magnetron sputtering layer, a vacuum evaporation layer or an electroplating layer.
[0015] Further, for the composite current collector, the support film is a film formed of one or more of polyamide, polyimide, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyethylene, polypropylene, polypropylene styrene, acrylonitrile-butadiene-styrene copolymer, polyvinyl alcohol, polystyrene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, sodium polystyrene sulfonate, polyacetylene, silicone rubber, polyoxymethylene, polyphenylene ether, polyphenylene sulfide, polyethylene glycol, sulfur nitride polymer materials, polyphenylene, polypyrrole, polyaniline, polythiophene, polypyridine, cellulose, starch, protein, epoxy resin, phenolic resin.
[0016] Further, for the composite current collector, the conductive coating is a nickel metal, copper metal, copper alloy, aluminum alloy or aluminum metal layer, and the primer coating is an alumina or silicon nitride layer.
[0017] Compared with the prior art, the present invention provides a composite current collector, including a support film, a primer coating is provided on the support film, a conductive coating is provided on the primer coating, the total mass of the primer coating is M1, the total mass of the conductive coating is M2. For the composite current collector, after forming the primer coating and before forming the conductive coating, under the condition of tension, its tensile elongation is X; for the composite current collector, after forming the conductive coating, under the same tension condition, its tensile elongation is Y, where M1 / X < M2 / Y. When being stretched, part of the mass M of the upper primer coating will be dispersed on the elongation X, and at the same time, the mass M2 of the metal layer on the primer coating will also be dispersed on Y. At this time, by M1 / X being less than M2 / Y, for the current collector at present, when being stretched, part of the mass of the metal layer can fill the part reduced when the primer coating is stretched, so as to achieve the purpose of maintaining the current-carrying capacity of the composite current collector and reducing the sheet resistance. Description of the Drawings
[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the following will briefly introduce the drawings required for the description of the embodiments or the prior art. Obviously, the following drawings are only some embodiments of the present invention. For those of ordinary skill in the art, without creative efforts, other drawings can be obtained based on the structures shown in these drawings.
[0019] Figure 1 It is a schematic structural diagram of the composite current collector provided by the present invention.
[0020] Explanation of the reference numerals in the drawings:
[0021] Support film 100
[0022] Primer coating 200
[0023] Conductive coating 300 DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0026] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0027] like Figure 1As shown in the figure, the present invention provides a composite current collector, which includes a support film 100, a primer coating 200 is provided on the support film 100, and a conductive coating 300 is provided on the primer coating 200. The total mass of the primer coating 200 is M1, and the total mass of the conductive coating 300 is M2. For the composite current collector, after the primer coating 200 is formed and before the conductive coating 300 is formed, under the condition of tension, its tensile elongation is X; for the composite current collector, after the conductive coating 300 is formed, under the same tension condition (the same tension magnitude, tension direction, and stretching time), its tensile elongation is Y, where M1 / X < M2 / Y. Further, for the composite current collector provided by the present invention, under the condition of tension, its sheet resistance is within 20 mΩ - 40 mΩ. The primer coating 200 is a magnetron sputtering layer or a vacuum evaporation coating layer. Further, for the composite current collector provided by the present invention, the conductive coating 300 is a magnetron sputtering layer, a vacuum evaporation coating layer, or an electroplating layer. Further, for the composite current collector provided by the present invention, the conductive coating 300 is a metal layer, and the primer coating 200 is an insulating layer.
[0028] Under the tension condition of the present invention, the tensile strength can be detected by a tensile testing machine. Any tension can be selected for the experiment. Generally speaking, it is a tension of 4 - 10 N. The inventor conducted the experiment using a tension of 5 N for detection (tested according to the tensile method in GB / T 228.1 - 2010, using an ordinary tensile testing machine. The tensile object is cut into a length of 200 mm and a width of 15 mm, and stretched in the length direction at a tensile speed of 50 mm / min. The distance between the clamping heads of the testing machine is 125 mm. The sample is stretched until it breaks and then the tensile elongation is calculated. The tensile elongation is the length at break minus the length before stretching divided by the length before stretching).
[0029] After finding a suitable film as the support film 100 in the present invention, the support film 100 is placed in a vacuum coating device to form the primer coating 200. The thickness of the primer coating 200 can be 30 nm - 60 nm. Here, the vacuum coating device can be physical or chemical deposition methods such as magnetron sputtering and vacuum evaporation, and then a metal layer is formed by physical or chemical deposition methods such as magnetron sputtering or vacuum evaporation.
[0030] During the subsequent processing of the product of the present invention, under the condition of tension, the square resistance of the composite current collector of the present application is ensured to be within 20 milliohms-40 milliohms, thereby maintaining high flow capacity, current gathering capacity, etc. This is because when the finished product is stretched, the mass M of the primer coating 200 on the semi-finished product will be partially dispersed on the elongation X, and the mass M2 of the metal layer on the primer coating 200 will also be dispersed on Y. At this time, M1 / X is less than M2 / Y. Relative to the current current collector, when stretched, part of the mass of the metal layer is to fill the part that is reduced when the primer coating 200 is stretched, thereby achieving the purpose of maintaining the flow capacity of the composite current collector and achieving the ability to reduce the square resistance.
[0031] Furthermore, in the composite current collector provided by the present invention, the mass per unit area of the conductive coating 300 is less than the mass per unit area of the support film 100. That is to say, the mass of the metal layer is less than the mass of the support film 100, so that the total mass of the composite current collector of the present invention is small, so that the electrical device using the present application, such as a lithium battery, can be lighter and have a higher energy density. Further, in the composite current collector provided by the present invention, the mass per unit area of the primer coating 200 is less than the mass per unit area of the support film 100. That is to say, the mass of the primer coating 200 is less than the mass of the support film 100, so that the total mass of the current collector of the present application can be reduced. A low-quality primer layer can also reduce the formation of holes in the support film 100 by the primer layer, and can also reduce the cost of the composite current collector of the present application, because the primer layer of the present application requires less amount and the production process consumes less energy.
[0032] Furthermore, in the composite current collector provided by the present invention, the mass per unit area of the primer coating 200 is M3, the mass per unit area of the conductive coating 300 is M4, and the composite current collector provided by the present invention, after forming the primer coating 200 and before forming the conductive coating 300, under thermal shrinkage conditions, has a thermal shrinkage rate of X1; in the composite current collector provided by the present invention, after forming the conductive coating 300, under the same thermal shrinkage conditions, has a thermal shrinkage rate of Y1, and M3 / X1>M4 / Y1.
[0033] In the present invention, the primer coating 200 formed on the support film 100 is a semi-finished product, and the metal layer formed on the primer coating 200 is a finished product. The heat shrinkage rate of the present invention is tested by the following method: the finished product or semi-finished product is placed in an oven at 150 degrees for 30 minutes, the difference between the length before the test and the length after the test is measured, and then divided by the length before the test to obtain the heat shrinkage rate.
[0034] The semi-finished product of the present invention has a heat shrinkage rate X1 in the length direction, the heat shrinkage rate of the finished product in the length direction is Y1, the mass of the semi-finished product in the width direction (the mass mean unit area mass in this application, that is, the primer coating 200 and the metal layer on the finished product or semi-finished product of a certain length and a certain width) is M3, and the mass of the metal layer in the finished film in the width direction is M4, wherein M3 / X1 is greater than M4 / Y1. Thus, when the composite current collector of the present invention is used in an electrical device such as a battery, when it is heated to the point of being punctured by a sharp object, its heat shrinkage will prevent the propagation of current in the metal layers on the upper and lower surfaces of the support layer, which is beneficial to improving the safety performance of the battery.
[0035] The primer coating 200 of the present invention is preferably made of a non-conductive material, and the primer coating 200 may be made of a coating such as aluminum oxide or silicon nitride. 2 O 3 ) materials, has the characteristics of high temperature resistance, inertness, good mechanical properties and chemical stability. Alumina is a white crystalline powder. When the powder particle size reaches the nanometer level, it will show optical, electrical, magnetic, thermal, mechanical and other properties that conventional materials do not have. The alumina coating can improve the high temperature resistance, acid resistance, liquid absorption and retention capacity and mechanical strength of the support film 100, thereby improving the performance and safety of the battery. The alumina coating can maintain stability in a high temperature environment and protect the substrate from high temperature oxidation. The coating can increase the mechanical strength of the substrate, improve wear resistance and corrosion resistance. The alumina coating has good chemical inertness and can resist corrosion from a variety of chemical substances. In lithium batteries, the alumina coating can absorb and retain electrolytes to improve the safety performance of the battery. Alumina has a high degree of ionicity in its crystal structure, and a stable ionic bond is formed between the oxygen ions and aluminum ions in its structure, making it difficult for electrons to conduct freely. The pure alumina coating is an insulating layer that does not have good electrical conductivity, which is beneficial to improving the safety performance of the battery.
[0036] The silicon nitride coating (Si 3 N 4 Silicon nitride coating (SiN) is a coating material widely used in many industrial fields with many excellent properties. Silicon nitride has high mechanical strength, and its flexural strength can reach 500-1200MPa, and it can maintain high strength even at high temperatures. The oxidation resistance temperature of silicon nitride reaches 1400℃, and it can work stably in high temperature environments. Silicon nitride is insoluble in any inorganic acid except hydrofluoric acid and has excellent corrosion resistance. Silicon nitride has good chemical stability and can maintain its performance in a variety of chemical environments. Silicon nitride has a low friction coefficient and is self-lubricating, which can reduce wear and frictional heat. Silicon nitride coating (Si 3 N 4The conductivity of silicon nitride coating is relatively special because it is an insulator with a large band gap and it is difficult for electrons to jump, so it is not conductive in its natural state. Silicon nitride coating can be used as a protective layer or functional layer to improve the performance and reliability of the product.
[0037] Furthermore, in the composite current collector provided by the present invention, the transmittance of the primer coating 200 is between 96% and 98%. This allows for better identification of unqualified products in subsequent production, because the transmittance in this range allows light to pass through better. After a metal layer is formed on the primer coating 200, its transmittance will decrease less, and its surface is more likely to allow light to pass through, making it easier to detect with a CCD. Furthermore, in the composite current collector provided by the present invention, the conductive coating 300 is nickel metal, copper metal, copper alloy, aluminum alloy or aluminum metal layer, wherein nickel-copper alloy is preferred, and nickel-copper alloy has better bonding with the support film 100.
[0038] Further, in the composite current collector provided by the present invention, the support film 100 shown is a film formed by one or more of polyamide, polyimide, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyethylene, polypropylene, polypropylene, acrylonitrile-butadiene-styrene copolymer, polyvinyl alcohol, polystyrene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, sodium polystyrene sulfonate, polyacetylene, silicone rubber, polyformaldehyde, polyphenylene oxide, polyphenylene sulfide, polyethylene glycol, polysulfur nitride polymer materials, polyphenylene, polypyrrole, polyaniline, polythiophene, polypyridine, cellulose, starch, protein, epoxy resin, and phenolic resin. The support film 100 can be a film made of any non-conductive material.
[0039] The inventors tested the composite current collector of the present invention, mainly testing the current flow capacity of the composite current collector of the present invention. After the composite current collector of the present invention is produced, the composite current collector is then processed for battery preparation, mainly coating, cold pressing, slitting, and die-cutting the composite current collector to obtain battery pole pieces, winding or laminating the flexible pole pieces to obtain bare cells, and then assembling, injecting, forming, and other processes to obtain a battery using the composite current collector.
[0040] The following is the experimental data. The comparative example uses a composite current collector with M1 / X greater than M2 / Y, specifically M1 is 4g / m 2 , while M2 is 3g / m 2 , X is 5%, and Y is 4%. The embodiment is the composite current collector claimed for protection in this application. The embodiment uses a composite current collector in which M1 / X is less than M2 / Y, specifically M1 is 3g / m 2 , and M2 is 4g / m 2 , the X value is 5% and the Y value is 4%.
[0041] The above comparative examples and embodiments are then prepared into batteries according to the above method, and then the current capacity is tested. The current capacity is measured according to the charging temperature rise. The lower the charging temperature rise, the stronger the current capacity of the composite current collector of the present application.
[0042] Comparative Example Overcurrent capability (charging temperature rise) Comparative Example 1 4.6℃ Comparative Example 2 4.3℃ Example 1 3.5℃ Example 2 3.1℃
[0043] This shows that the composite current collector of the present invention has a strong flow capacity.
[0044] In summary, the product of the present invention ensures that the square resistance of the composite current collector of the present application is within 20 milliohms-40 milliohms under tension during subsequent processing, thereby maintaining high flow capacity, current gathering capacity, etc. This is because when the finished product is stretched, the mass M of the primer coating on the semi-finished product will be partially dispersed on the elongation X, and the mass M2 of the metal layer on the primer coating will also be dispersed on Y. At this time, M1 / X is less than M2 / Y. Relative to the current current collector, when stretched, part of the mass of the metal layer fills the part that is reduced when the primer coating is stretched, thereby achieving the purpose of maintaining the flow capacity of the composite current collector and achieving the ability to reduce the square resistance.
[0045] In addition, the semi-finished product of the present invention has a thermal shrinkage rate X1 in the length direction, the finished product has a thermal shrinkage rate Y1 in the length direction, the mass of the semi-finished product in the width direction (the mass mean unit area mass in this application, that is, the primer coating and metal layer on the finished product or semi-finished product of a certain length and a certain width) is M3, and the mass of the metal layer in the finished film in the width direction is M4, wherein M3 / X1 is greater than M4 / Y1. Thus, when the composite current collector of the present invention is used in an electrical device such as a battery, when it is heated to the point of being punctured by a sharp object, its thermal shrinkage will prevent the propagation of current in the metal layers on the upper and lower surfaces of the support layer, which is beneficial to improving the safety performance of the battery.
[0046] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A composite current collector, characterized in that: The composite current collector comprises a supporting film, a primer coating is arranged on the supporting film, a conductive coating is arranged on the primer coating, the total mass of the primer coating is M1, the total mass of the conductive coating is M2, the composite current collector, after forming the primer coating and before forming the conductive coating, has a tensile elongation of X under tensile conditions; the composite current collector, after forming the conductive coating, has a tensile elongation of Y under the same tensile conditions, wherein M1 / X <M2 / Y。 2. The composite current collector according to claim 1, characterized in that: The conductive coating is a metal layer, and the primer coating is an insulating layer.
3. The composite current collector according to claim 2, characterized in that: The mass per unit area of the conductive coating is smaller than the mass per unit area of the support film.
4. The composite current collector according to claim 3, characterized in that: The mass per unit area of the primer coating is smaller than the mass per unit area of the support film.
5. The composite current collector according to claim 4, characterized in that: The mass of the primer coating per unit area is M3, the mass of the conductive coating per unit area is M4, and the thermal shrinkage rate of the composite current collector after forming the primer coating and before forming the conductive coating under thermal shrinkage conditions is X1; the thermal shrinkage rate of the composite current collector after forming the conductive coating under the same thermal shrinkage conditions is Y1, and M3 / X1>M4 / Y1.
6. The composite current collector according to claim 5, characterized in that: The light transmittance of the primer coating is 96%-98%.
7. The composite current collector according to claim 1, characterized in that: The composite current collector has a square resistance within 20 milliohms to 40 milliohms under tension conditions.
8. The composite current collector according to any one of claims 1 to 7, characterized in that: The primer coating is a magnetron sputtering layer or a vacuum evaporation layer, and the conductive coating is a magnetron sputtering layer, a vacuum evaporation layer or an electroplating layer.
9. The composite current collector according to claim 8, characterized in that: The support film shown is a film formed by one or more of polyamide, polyimide, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyethylene, polypropylene, polypropylene, acrylonitrile-butadiene-styrene copolymer, polyvinyl alcohol, polystyrene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, sodium polystyrene sulfonate, polyacetylene, silicone rubber, polyformaldehyde, polyphenylene ether, polyphenylene sulfide, polyethylene glycol, polysulfur nitride polymer materials, polyphenylene, polypyrrole, polyaniline, polythiophene, polypyridine, cellulose, starch, protein, epoxy resin, and phenolic resin.
10. The composite current collector according to claim 9, characterized in that: The conductive coating is a nickel metal, copper metal, copper alloy, aluminum alloy or aluminum metal layer, and the primer coating is an aluminum oxide or silicon nitride layer.