Secondary battery electrolyte and lithium secondary battery

By designing an electrolyte system consisting of the first electrolyte and the second electrolyte, the solvent system and additives work together to form a stable solid electrolyte interface film, the wetting ability of the lithium secondary battery electrolyte on the electrode material is solved. The poor problem improves the battery's cycle performance and storage stability, and meets the requirements of high voltage and high performance.

CN119009111APending Publication Date: 2024-11-22XIANGHE KUNLUN NEW ENERGY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411278216.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing lithium secondary battery electrolyte has poor wetting properties on the electrode material, resulting in unstable high-temperature storage, poor low-temperature discharge performance and short cycle life.

Method used

The electrolyte system consisting of the first electrolyte solution and the second electrolyte solution is adopted, wherein the first electrolyte solution includes a cyclic carbonate solvent, a chain carbonate solvent, a chain carboxylic acid ester solvent, and a first film forming additive and lithium salt, the second electrolyte includes a cyclic carbonate solvent, a chain carbonate solvent, a fluorocarbonate solvent, a chain carboxylate solvent, a second film-forming additive and a lithium salt, through mutual coordination It acts to form a stable solid electrolyte interface mask, improving the wetting and cycling performance of the electrode.

Benefits of technology

The circulation performance, high-temperature storage stability and low-temperature electrical performance of lithium-ion batteries have been significantly improved. The capacity retention rate of 1,000 cycles in 25℃ is >80%, and the capacity retention rate after 21 days of high-temperature storage in 60℃ is >80%, and the capacity recovery rate is > 85%, the low-temperature discharge capacity of 0.2C at -0℃ is >1801mAh, extending the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009111A_ABST
    Figure CN119009111A_ABST
Patent Text Reader

Abstract

The invention provides a secondary battery electrolyte and a lithium secondary battery, and belongs to the technical field of secondary batteries. The electrolyte comprises a first electrolyte and a second electrolyte, the first electrolyte is used for carrying out primary liquid injection when the lithium ion battery is prepared, and the second electrolyte is used for carrying out secondary liquid injection on the battery. Through the design of a solvent system and an additive system of the first electrolyte and the second electrolyte and the compounding of components and additive amounts, the high-voltage stability and wettability of the electrolyte are enhanced, and the first electrolyte and the second electrolyte cooperate with each other, so that the stability of an SEI film can be maintained, stable interface modification and protection are formed for a positive electrode and a negative electrode, and the service life of the SEI film is prolonged. And excessive consumption of the conductive lithium salt and gas generation are avoided. The lithium ion battery prepared by using the electrolyte has the advantages of high long circulation retention rate, high storage capacity retention rate and recovery rate, small volume expansion and large low-temperature discharge capacity, and fully meets the requirements of high-voltage and high-performance batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of secondary batteries, and in particular relates to a secondary battery electrolyte and a lithium secondary battery. Background Art

[0002] With the development of science and technology, secondary batteries are widely used in various electronic devices, electric vehicles and other fields due to their advantages such as high energy density, long cycle life and environmental protection. Among them, lithium secondary batteries have become the main research direction of secondary batteries due to their high energy density and long cycle life. However, the performance of lithium secondary batteries is greatly affected by the electrolyte. The electrolyte is an important component of lithium secondary batteries, which directly affects the electrochemical properties, safety and service life of the battery. Therefore, the development of electrolytes with excellent performance is of great significance to improving the performance of lithium secondary batteries.

[0003] The existing lithium secondary battery electrolyte is mainly composed of lithium salt, non-aqueous organic solvent and electrolyte additive. Among them, the electrolyte additive can improve the electrochemical performance of the battery, such as improving the capacity, cycle life and safety of the battery. At present, commonly used electrolyte additives include vinylene carbonate (VC), fluoroethylene carbonate (FEC), etc. These additives can form a stable solid electrolyte interface film (SEI film) on the surface of the positive and negative electrodes of the battery, thereby improving the electrochemical performance of the battery. However, the existing secondary battery electrolyte has the problem of poor wettability to the electrode material, which leads to problems such as unstable high-temperature storage of the battery, poor low-temperature discharge performance, and short battery cycle life.

[0004] Therefore, how to develop an electrolyte that is both highly safe and can improve battery cycle life and service life is an important topic in the current field of lithium secondary batteries. Summary of the invention

[0005] In view of the deficiencies of the prior art, the present invention aims to provide a secondary battery electrolyte and a lithium secondary battery with excellent cycle performance, high temperature storage stability and low temperature discharge performance.

[0006] One of the objects of the present invention is to provide a secondary battery electrolyte, the electrolyte comprising a first electrolyte and a second electrolyte, the mass ratio of the first electrolyte to the second electrolyte being (80-90):(20:10).

[0007] Taking the total mass of the first electrolyte as 100%, the first electrolyte includes 5-25% cyclic carbonate solvent, 20-35% chain carbonate solvent, 20-35% chain carboxylate solvent, 5-10% first film-forming additive and 9-15% lithium salt.

[0008] Taking the total mass of the second electrolyte as 100%, the second electrolyte includes 10-25% of cyclic carbonate solvent, 10-20% of chain carbonate solvent, 5%-10% of fluorocarbonate, 10-35% of chain carboxylate solvent, 0.1%-5% of second film-forming additive and 10-20% of lithium salt.

[0009] The first film-forming additive includes a silicon-containing additive and a sulfur-containing additive.

[0010] The second film-forming additive includes a compound A as shown in Formula 1;

[0011]

[0012] Among them, the R 1 and R 2 are each independently selected from H, halogen, substituted or unsubstituted C 1 -C 6 Straight chain or branched alkyl, substituted or unsubstituted C 2 -C 6 Alkenyl, substituted or unsubstituted C 2 -C 6 Alkyne, sulfonyl halide, substituted or unsubstituted C 6 -C 20 Aryl, substituted or unsubstituted C 1 -C 6 Alkylsulfone, substituted or unsubstituted C 6 -C 20 Aryl, substituted or unsubstituted C 1 -C 6 Any one of a silyl group, a carbonyl group or a sulfonyl halide group;

[0013] And, the R 1 and R 2 At least one of them is a fluorine-containing group;

[0014] The R 3 -CH 2 -、-CH 2 CH 2 -or-CH 2 CH 2 CH 2 -.

[0015] Preferably, the R 1 and R 2 Each independently selected from H, -C 4 H 7 , -C 2 H 5 、-CH 3 、-CH 2 CF3 , CH 2 CHF 2 , CHF 2 , -CF 3 , -CF 2 Br, C 2 H 4 NH 2 , =O or Li.

[0016] Preferably, the compound A comprises one or more of the following compounds:

[0017]

[0018] Preferably, the cyclic carbonate solvent includes ethylene carbonate and propylene carbonate.

[0019] Preferably, the mass ratio of ethylene carbonate to propylene carbonate is 1:(0.2-1).

[0020] Preferably, the linear carbonate solvent includes one or more of ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, allyl methyl carbonate or diethyl pyrocarbonate, preferably ethyl methyl carbonate.

[0021] Preferably, the chain carboxylate solvent includes one or more of methyl propionate, methyl acetate, propyl propionate (PP), methyl butyrate, ethyl butyrate, propyl acetate, butyl butyrate, ethyl propionate or ethyl acetate, preferably propyl propionate.

[0022] Preferably, the fluorocarbonate solvent includes one or more of fluoroethylene carbonate, difluoroethylene carbonate, difluoropropylene carbonate, trifluoroethyl acetate, trifluoroethyl methyl carbonate, trifluoromethylethylene carbonate, 4-trifluoromethylethylene carbonate, chloroethylene carbonate, di(2,2,2-trifluoroethyl) carbonate, methyl trifluoropropionate, 3,3,3-trifluoroethyl acetate, methyl 2-(trifluoromethyl)benzoate, ethyl 4,4,4-trifluorobutyrate or 1,1,1,3,3,3-hexafluoroisopropyl acrylate, preferably difluorocarbonate.

[0023] Preferably, the sulfur-containing additive includes one or more of vinyl sulfate, 1,3-propane sultone, 1,3-propene sultone, propylene sulfate, 1,4-butane sultone, vinylene sulfite or methylene disulfonate, preferably propylene sulfate and 1,4-propane sultone.

[0024] Preferably, the silicon-containing additive includes one or more of tetravinylsilane, tristrimethylsilane phosphate or tristrimethylsilane borate, preferably tetravinylsilane.

[0025] Preferably, the mass ratio of the sulfur-containing additive to the silicon-containing additive is 4:0.5;

[0026] Preferably, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium perchlorate, lithium trifluoromethanesulfonate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethylsulfonyl imide), lithium difluorophosphate, lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), lithium iodide, lithium tetrafluorooxalatophosphate, bis(tetrafluorophosphoryl imide), lithium tetrafluoroborate or lithium bis(oxalatoborate).

[0027] A second object of the present invention is to provide a lithium secondary battery, wherein the lithium secondary battery comprises the secondary battery electrolyte as described above, wherein a first electrolyte is first injected into the battery, and after formation, a second electrolyte is injected.

[0028] Preferably, after injecting the first electrolyte, the formation is performed after soaking for 16-18 hours;

[0029] Preferably, the formation step includes first charging at 0.02C current for 30 min, then charging at 0.05C current for 30 min, then charging at 0.1C current for 120 min, and then charging at 0.2C current to a voltage of 3.85V. ;

[0030] Preferably, after the second electrolyte is injected, the final sealing is performed after soaking for 18-20 hours, and then the final sealing is performed again after aging for 24 hours.

[0031] Preferably, the positive electrode active material of the lithium secondary battery is LiNi x Co y Mn z L (1-x-y-z) O 2 、LiCo x1 L (1-x1) O 2 、LiNix 2 Ly 1 Mn (2-x2-y1 ) 4 and Li z1 MPO 4 One or more of the following;

[0032] Wherein, L is at least one of Co, Al, Sr, Mg, Ti, Ca, Zr, Zn, Si and Fe; M is at least one or two of Fe, Mn and Co; 0≤x≤1, 0≤y≤1, 0≤z≤1, 0≤x+y+z≤1, 0≤x1≤1, 0.3≤x2≤0.6, 0.01≤y1≤0.2, 0.5≤z1≤1;

[0033] Preferably, the negative electrode active material of the lithium secondary battery includes single-element lithium metal, lithium alloy, carbon material, a composite material of single-crystal silicon and carbon, or a composite material of silicon monoxide and carbon.

[0034] The beneficial effects of the present invention include:

[0035] The electrolyte of the present invention includes a first electrolyte and a second electrolyte, wherein the first electrolyte is used for primary injection when preparing a lithium-ion battery, and the second electrolyte is used for secondary injection of the battery. By designing the solvent system and additive system of the first electrolyte and the second electrolyte, as well as compounding the components and the addition amounts, on the one hand, the high-voltage stability of the electrolyte is enhanced, and the wettability to the electrode is enhanced; on the other hand, the first electrolyte and the second electrolyte cooperate with each other to maintain the stability of the SEI film, form a stable interface modification and protection for the positive and negative electrodes, avoid excessive consumption of conductive lithium salts and gas generation, thereby significantly improving the cycle performance, high-temperature storage stability and low-temperature electrical performance of the lithium-ion battery. The lithium-ion battery prepared by using the electrolyte of the present invention has a capacity retention rate of >80% after 1000 cycles at 25°C, a capacity retention rate of >80% after 21 days of high-temperature storage at 60°C, a capacity recovery rate of >85%, a volume expansion rate of ≤8%, and a low-temperature discharge capacity of 0.2C at -0°C of >1801mAh. It has the advantages of high long-cycle retention rate, high storage capacity retention rate and recovery rate, low volume expansion, and large low-temperature discharge capacity, and fully meets the requirements of high-voltage and high-performance batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The contact angle of the first electrolyte added to the surface of the graphite negative electrode sheet;

[0037] Figure 2 The contact angle of the first electrolyte and the second electrolyte mixed after the graphite negative electrode sheet is soaked in the first electrolyte;

[0038] Figure 3 The contact angle of the first electrolyte and the second electrolyte mixed and dropped onto the surface of the graphite negative electrode sheet. DETAILED DESCRIPTION

[0039] In the following description, certain specific details are included to provide a comprehensive understanding of each disclosed embodiment. However, one skilled in the relevant art will recognize that the embodiments can be implemented without one or more of these specific details, but with other methods, components, materials, etc.

[0040] Unless otherwise required herein, the words "include" and "comprising" should be interpreted as having an open and inclusive meaning, ie, "including but not limited to".

[0041] References to "one embodiment" or "an embodiment" or "a preferred embodiment" or "certain embodiments" throughout this specification mean that the specific referenced elements, structures or features described in connection with the embodiment are included in at least one embodiment. Therefore, the phrases "in one embodiment" or "in an embodiment" or "in a preferred embodiment" or "in certain embodiments" appearing in different places throughout the specification do not necessarily all refer to the same embodiment. In addition, the specific elements, structures or features may be combined in any appropriate manner in one or more embodiments.

[0042] According to a first aspect of the present invention, there is provided a secondary battery electrolyte, characterized in that the electrolyte comprises a first electrolyte and a second electrolyte, and the mass ratio of the first electrolyte to the second electrolyte is (50-90):(10-50).

[0043] Taking the total mass of the first electrolyte as 100%, the first electrolyte includes 5-25% cyclic carbonate solvent, 20-30% chain carbonate solvent, 20-35% chain carboxylate solvent, 5-10% first film-forming additive and 9-15% lithium salt.

[0044] Taking the total mass of the second electrolyte as 100%, the second electrolyte includes 10-25% of cyclic carbonate solvent, 10-20% of chain carbonate solvent, 5%-10% of fluorocarbonate, 10-35% of chain carboxylate solvent, 0.1%-5% of second film-forming additive and 10-20% of lithium salt.

[0045] The first film-forming additive includes a sulfur-containing additive and a silicon-containing additive;

[0046] The second film-forming additive includes a compound A as shown in Formula 1;

[0047]

[0048] Among them, the R 1 and R 2 are each independently selected from H, halogen, substituted or unsubstituted C 1 -C 6 Straight chain or branched alkyl, substituted or unsubstituted C 2 -C 6 Alkenyl, substituted or unsubstituted C 2 -C 6 Alkyne, sulfonyl halide, substituted or unsubstituted C 6 -C 20 Aryl, substituted or unsubstituted C 1 -C 6 Alkylsulfone, substituted or unsubstituted C 1 -C6 Any one of a silyl group, a carbonyl group or a sulfonyl halide group;

[0049] And, the R 1 and R 2 At least one of them is a fluorine-containing group;

[0050] The R 3 -CH 2 -、-CH 2 CH 2 -or-CH 2 CH 2 CH 2 -.

[0051] In the present invention, C 1 -C 6 Substituents of straight-chain or branched alkyl groups, C 2 -C 6 Substituents of olefin groups, C 2 -C 6 Substituents of alkynyl groups, C 6 -C 20 Substituents of aromatic groups, C 1 -C 6 Substituents of the alkylsulfone group, substituted or unsubstituted C 6 -C 20 Aryl and C 1 -C 6 The substituents of the silyl group are independently selected from one or more of halogen, sulfonyl halide or silyl group. The halogen includes one or more of F, Cl or Br.

[0052] In the present invention, the mass ratio of the first electrolyte to the second electrolyte is 5:5, 5.5:4.5, 6:4, 6.5:3.5, 7:3, 7.5:2.5, 8:2, 8.5:1.5 or 9:1.

[0053] Preferably, the mass ratio of the first electrolyte to the second electrolyte is 7:3.

[0054] In the first electrolyte, the percentage of the cyclic carbonate solvent is, for example, 5%, 7%, 10%, 12%, 15%, 17%, 20%, 22% or 25%, the percentage of the chain carbonate solvent is, for example, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34% or 35%, and the percentage of the chain carboxylate solvent is, for example, 20%. , 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34% or 35%, the percentage of the first film-forming additive is, for example, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5% or 10%, and the percentage of the lithium salt is, for example, 9%, 10%, 11%, 12%, 13%, 14% or 15%.

[0055] In the second electrolyte, the percentage of the cyclic carbonate solvent is, for example, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, or 25%, the percentage of the linear carbonate solvent is, for example, 10%, 11%, 12%, 13%, 14%, 15%, 6%, 17%, 18%, 19% or 20%, and the percentage of the fluorocarbonate is, for example, 5%, 6%, 7%, 8%, 9% or 10%. 0%, the percentage of the chain carboxylic acid ester solvent is, for example, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28% or 30%, the percentage of the second film-forming additive is, for example, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, and the percentage of the lithium salt is, for example, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%.

[0056] In the present invention, the cyclic carbonate solvent is compounded with the chain carboxylic acid ester solvent, and cooperates with the first additive to ensure that a stable solid electrolyte interface film is formed on the surface of the battery pole piece during formation, which can broaden the working temperature range of the electrolyte to -40°C to 60°C. The fluorinated carbonate and the second additive containing fluorine and nitrogen in the second electrolyte have better oxidation resistance. On the one hand, they can increase the oxidation decomposition potential of the electrolyte so that the working voltage of the electrolyte reaches more than 5V; on the other hand, the first additive, the second additive and the fluorinated carbonate cooperate with each other to form a stable organic and inorganic protective film containing N on the positive and negative electrodes during the operation of the battery, effectively inhibiting the side reactions on the positive and negative electrode surfaces and the degradation of the positive and negative electrodes, improving performance and preventing the dissolution of transition metal ions that may occur during high pressure and high temperature processes.

[0057] However, since the viscosity of the fluorocarbonate and the first additive greatly affects the wetting performance of the battery, the present invention designs the electrolyte to be a first electrolyte and a second electrolyte, wherein the first electrolyte is used for a primary injection into the battery, and the second electrolyte is used for a secondary injection into the battery. The battery is first injected with the first electrolyte to allow the electrolyte to completely infiltrate the battery, ensuring that the electrode material is in full contact with the electrolyte, improving the transmission efficiency of lithium ions in the electrode, and promoting the formation of a more stable solid electrolyte interface film; and then a secondary injection is performed to supplement and adjust the electrolyte and additives, further optimizing the electrolyte composition, so that the battery maintains good performance during long-term use, reduces problems such as capacity attenuation and increased internal resistance, and is beneficial to improving the cycle life and stability of the battery.

[0058] In the present invention, the sulfur-containing additive reacts preferentially on the electrode surface, combines with lithium ions, and reacts with the active sites on the electrode surface to inhibit the occurrence of side reactions. The silicon-containing additive can form a stable silicon-lithium compound with lithium ions, fill the pores in the membrane, make the membrane denser, and cooperate with other components to form a compound with a specific structure, enhance the stability of the SEI membrane, and improve the bonding force between the electrode and the SEI membrane.

[0059] In a preferred embodiment of the present invention, the R 1 and R 2 Each independently selected from H, -C 4 H 7 , -C 2 H 5 、-CH 3 、-CH 2 CF 3 , CH 2 CHF 2 , CHF 2 , -CF 3 , -CF 2 Br, C 2 H 4 NH 2 , =O or Li.

[0060] In a preferred embodiment of the present invention, the compound A comprises one or more of the following compounds:

[0061]

[0062]

[0063] Preferably, the compound A is compound A1 as shown in formula 1-1.

[0064] In a preferred embodiment of the present invention, the cyclic carbonate solvent includes ethylene carbonate (EC) and propylene carbonate (PC).

[0065] Preferably, the mass ratio of ethylene carbonate to propylene carbonate is 1:(0.2-1).

[0066] In the present invention, the ethylene carbonate and propylene carbonate are beneficial to balancing the dielectric constant and viscosity of the electrolyte and promoting the formation of a stable SEI film. The mass ratio of the ethylene carbonate to the propylene carbonate is, for example, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9 or 1:1.

[0067] In a preferred embodiment of the present invention, the linear carbonate solvent includes one or more of ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, allyl methyl carbonate or diethyl pyrocarbonate.

[0068] Preferably, the linear carbonate solvent is ethyl methyl carbonate, which can improve ion conductivity, reduce viscosity, optimize electrode compatibility, and improve battery safety performance.

[0069] In a preferred embodiment of the present invention, the chain carboxylic acid ester solvent includes one or more of methyl propionate, methyl acetate, propyl propionate (PP), methyl butyrate, ethyl butyrate, propyl acetate, butyl butyrate, ethyl propionate or ethyl acetate.

[0070] Preferably, the chain carboxylic acid ester solvent is propyl propionate, which can improve the compatibility of various components of the electrolyte.

[0071] In a preferred embodiment of the present invention, the fluorocarbonate solvent includes one or more of fluoroethylene carbonate, difluoroethylene carbonate, difluoropropylene carbonate, trifluoroethyl acetate, trifluoroethyl methyl carbonate, trifluoromethylethylene carbonate, 4-trifluoromethylethylene carbonate, chloroethylene carbonate, di(2,2,2-trifluoroethyl) carbonate, methyl trifluoropropionate, 3,3,3-trifluoroethyl acetate, methyl 2-(trifluoromethyl)benzoate, ethyl 4,4,4-trifluorobutyrate or 1,1,1,3,3,3-hexafluoroisopropyl acrylate.

[0072] Preferably, the fluorocarbonate solvent is a bisfluorocarbonate.

[0073] Preferably, the mass ratio of the sulfur-containing additive to the silicon-containing additive is (5-10):1, preferably 8:1.

[0074] Preferably, the sulfur-containing additive includes one or more of vinyl sulfate (DTD), 1,3-propane sultone (PS), 1,3-propene sultone (PST), propylene sulfate (TS), 1,4-butane sultone (BS), vinyl sulfite (ES) or methylene disulfonate (MMDS).

[0075] Preferably, the sulfur-containing additive is a combination of propylene sulfate and 1,4-butane sultone, and the mass ratio of propylene sulfate to 1,4-butane sultone is 4:3.

[0076] Preferably, the silicon-containing additive includes one or more of tetravinylsilane (TVSI), tristrimethylsilyl phosphate (TMSP) or tristrimethylsilyl borate (TMSB).

[0077] Preferably, the silicon-containing additive is tetravinylsilane.

[0078] In the present invention, in the primary electrode liquid, the sulfur-containing additive and the silicon-containing additive cooperate with the cyclic carbonate solvent, the chain carbonate solvent, and the chain carboxylate solvent to further improve the wettability of the battery and make the battery performance more stable.

[0079] Preferably, the lithium salt is selected from lithium hexafluorophosphate (LiPF 6) 、Lithium perchlorate (LiClO 4) , lithium trifluoromethanesulfonate (LiTFS), lithium bis(trifluoromethanesulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium difluorophosphate (LiPO 2 F 2) , lithium difluorooxalatoborate (LiODFB), lithium difluorobisoxalatophosphate (LiODFB), lithium iodide, lithium tetrafluorooxalatophosphate, bis tetrafluorophosphoramidite salt, lithium tetrafluoroborate (LiBF 4 ) or one or more of lithium bis(oxalatoborate).

[0080] According to a second aspect of the present invention, the lithium secondary battery comprises the secondary battery electrolyte as described above, and a first electrolyte is first injected into the battery, and after formation, a second electrolyte is injected.

[0081] Preferably, after the first electrolyte is injected, the formation is performed after immersion for 16-18 hours.

[0082] Preferably, the formation step includes first charging at 0.02C for 30 min, then charging at 0.05C for 30 min, then charging at 0.1C for 120 min, and then charging at 0.2C to a voltage of 3.85V.

[0083] Preferably, after the second electrolyte is injected, the final sealing is performed after soaking for 18-20 hours, and then the secondary sealing is performed after aging for 24 hours, and then the capacity test is performed to screen out qualified batteries.

[0084] Specifically, the injection method includes:

[0085] The injection process is carried out in a glove box;

[0086] First, inject the first electrolyte into the dry battery cell, seal it, reserve some air bags, and place it for 16-18 hours before forming. The forming process is to charge at 0.02C for 30 minutes, 0.05C for 30 minutes, 0.1C for 120 minutes, and then charge at 0.2C until the voltage reaches 3.85V.

[0087] Then, inject the second electrolyte into the formed battery, let it sit for 18-20 hours for infiltration, and then perform a final seal. Then, after aging in a 45℃ high temperature box for 24 hours, perform a second final seal, and then perform a capacity test. The capacity test steps are: 0.2C charge to 5V, 0.2C discharge to 2.75V, 0.5C charge to 5V, 0.5C discharge to 2.75V, 1C charge to 5V, 1C discharge to 2.75V, screen out qualified batteries, and then continue with a series of other tests.

[0088] Specifically, the lithium secondary battery includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte.

[0089] The positive electrode and the negative electrode include active materials, conductive agents, current collectors, and binders for combining the active materials with the conductive agents and current collectors.

[0090] The positive electrode active material of the lithium secondary battery is LiNi x Co y Mn z L (1-x-y-z) O 2 、LiCo x1 L (1-x1) O 2 、LiNix 2 Ly 1 Mn (2-x2-y1 ) 4 and Li z1 MPO 4 One or more of the following;

[0091] Among them, L is at least one of Co, Al, Sr, Mg, Ti, Ca, Zr, Zn, Si and Fe; M is at least one or two of Fe, Mn and Co; 0≤x≤1, 0≤y≤1, 0≤z≤1, 0≤x+y+z≤1, 0≤x1≤1, 0.3≤x2≤0.6, 0.01≤y1≤0.2, 0.5≤z1≤1.

[0092] The negative electrode active material of the lithium secondary battery includes single-substance lithium metal, lithium alloy, carbon material, composite material of single crystal silicon and carbon, or composite material of silicon monoxide and carbon.

[0093] In the present invention, the lithium alloy includes an alloy formed by lithium and any one or at least two of aluminum, zinc, silicon, tin, gallium or antimony.

[0094] The carbon material is any one of hard carbon, hard carbon-coated composite graphite, soft carbon, soft carbon-coated composite graphite, natural graphite, graphitized coke, graphitized MCMB, and graphitized mesophase pitch carbon fiber, or a combination of at least two thereof.

[0095] Optionally, a separator or a solid electrolyte layer is further provided between the positive electrode and the negative electrode.

[0096] The charging cut-off voltage of the lithium-ion battery is 4.8V-5.2V.

[0097] Example

[0098] The present invention is further described in detail below in conjunction with the embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other.

[0099] In the following examples, unless otherwise specified, all raw materials are commercially available products.

[0100] Example 1

[0101] A non-aqueous electrolyte and a preparation method thereof, wherein the non-aqueous electrolyte comprises the following components in terms of mass percentage: a first electrolyte comprising: lithium hexafluorophosphate (LiPF 6) 12.5%, ethylene carbonate (EC) 15%, propylene carbonate (PC) 7%, ethyl methyl carbonate (EMC) 30%, propyl propionate (PP) 30%, lithium difluorooxalatoborate (LiDFOB) 0.5%, lithium difluorophosphate (LiPO 2 F 2 )1%, propylene sulfate (TS) 2%, 1,4-propane sultone (BS) 1.5%, tetravinylsilane (TVSI) 0.5%.

[0102] The mass percentage composition of the second electrolyte is: lithium hexafluorophosphate (LiPF 6) 15%, ethylene carbonate (EC) 15%, propylene carbonate (PC) 10%, ethyl methyl carbonate (EMC) 20%, propyl propionate (PP) 30%, bisfluorocarbonate DFEC 9.9%, and compound A as shown in formula 1-1 10.1%.

[0103] The preparation method of the non-aqueous electrolyte is as follows: preparing and preparing in a glove box, wherein the nitrogen content in the glove box is 99.999%, the actual oxygen content in the glove box is less than 2ppm, and the water content is less than 0.1ppm; according to the formula, cyclic carbonate solvents (EC and PC), chain carbonate solvents (EMC), and chain carboxylate solvents (PP) are mixed uniformly to obtain a non-aqueous solvent; the fully dried lithium salt (LiPF 6) Add the non-aqueous solvent, add film-forming additives (TS and BS), and then add dry lithium salts (LiDFOB and LiPO 2 F 2 ) to obtain the first electrolyte; according to the formula, cyclic carbonate solvents (EC and PC), chain carbonate solvents (EMC), chain carboxylic acid ester solvents (PP), and fluorocarbonate (DFEC) are mixed uniformly to obtain a non-aqueous solvent; the fully dried lithium salt (LiPF 6) Add the non-aqueous solvent and add compound A1 as shown in formula 1-1 to obtain a second electrolyte.

[0104] The first electrolyte and the second electrolyte obtained in Example 1 are applied to a lithium secondary battery. The preparation method of the lithium secondary battery is as follows:

[0105] Positive electrode preparation: LiCoO 2 Powder, binder (polyvinylidene fluoride, PVDF), and conductive agent (CNT: acetylene black) are mixed in a mass ratio of 97.6:1:0.5:1.5, N-methylpyrrolidone (NMP) is added, and the mixture is stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode slurry with uniform fluidity; the positive electrode slurry is evenly coated on an aluminum foil with a thickness of 13 μm; the coated aluminum foil is baked in an oven with 5 different temperature gradients, and then dried in an oven at 140°C for 8 hours, and then rolled and cut to obtain the desired positive electrode sheet.

[0106] Negative electrode preparation: Graphite negative electrode material, conductive agent (conductive carbon black, SP), dispersant (sodium carboxymethyl cellulose, CMC), and binder (styrene-butadiene rubber, SBR) are prepared into negative electrode slurry by a wet process in a mass ratio of 95.7:1:1.3:2; the negative electrode slurry is evenly coated on a copper foil with a thickness of 10 μm; the coated copper foil is baked in an oven with 5 different temperature gradients, and then dried in an oven at 80°C for 48 hours, and then rolled and cut to obtain the required graphite negative electrode sheet.

[0107] Diaphragm preparation: PE porous polymer film (thickness of about 8 mm) is used as the diaphragm.

[0108] Preparation of lithium-ion batteries: The positive electrode sheet, separator, and negative electrode sheet prepared above are wound to obtain a bare battery cell without liquid injection; the bare battery cell is placed in an outer packaging aluminum foil, and the prepared electrolyte is injected into the dried bare battery cell. After vacuum packaging, standing, formation, shaping, sorting and other processes, the required lithium-ion battery is obtained. The discharge voltage range is set to 2.75-5V, and the battery capacity is 2Ah.

[0109] The injection method is: take 4.9g of the first electrolyte in the glove box and inject it into the dry battery cell, seal it, reserve some air bags, and place it aside for 24 hours before forming it. The formation steps are 0.02C charging for 30min, 0.05C charging for 30min, 0.1C charging for 120min, and then 0.2C charging to a voltage of 3.85V. Take 2.1g of the second electrolyte in the glove box and inject it into the formed battery. After placing it aside for 24 hours, perform a final seal. After aging in a high-temperature box at 45℃ for 24 hours, perform a second final seal and then perform a capacity separation test. The capacity separation test steps are: 0.2C charging to 5V, 0.2C discharging to 2.75V, 0.5C charging to 5V, 0.5C discharging to 2.75V, 1C charging to 5V, 1C discharging to 2.75V. The battery after capacity separation then continues with a series of other tests.

[0110] The electrolyte compositions of Examples 1-17 and Comparative Examples 1-4 are shown in Table 1, where Compound A as shown in Formula 1-2 is represented as Compound A2, Compound A as shown in Formula 1-3 is represented as Compound A3, Compound A as shown in Formula 1-4 is represented as Compound A4, Compound A as shown in Formula 1-5 is represented as Compound A5, and Compound A as shown in Formula 1-6 is represented as Compound A6, and a first electrolyte, a second electrolyte, and a lithium secondary battery are prepared in the same manner as in the Examples.

[0111] Table 1 Electrolyte compositions of Examples 1-17 and Comparative Examples 1-4

[0112]

[0113]

[0114]

[0115] Among them, m 1 :m 2 is the mass ratio of the first electrolyte to the second electrolyte.

[0116] After lithium secondary batteries were prepared using the electrolytes described in Examples 1-17 and Comparative Examples 1-4, safety performance tests, cycle performance tests and high-temperature storage performance tests were carried out. The test results are shown in Tables 2 to 23.

[0117] (1) Wettability test

[0118] The wettability test of the graphite negative electrode sheet using the first electrolyte and the second electrolyte obtained in Example 3 shows that the compaction density of the graphite negative electrode sheet is 1.6 g / cm 3 . Figure 1 is the contact angle at 0s and 10s when the first electrolyte is dropped on the surface of the graphite negative electrode sheet; Figure 2 The graphite negative electrode sheet is first soaked in the first electrolyte for 17 hours, and then the first electrolyte and the second electrolyte are added dropwise in a weight ratio of 7:3 to form a mixed electrolyte at 0s and 10s; Figure 3 The contact angle of the electrolyte mixed with the first electrolyte and the second electrolyte in a weight ratio of 7:3 at 0s and 10s is shown in Table 1. Figure 1-3 As shown, for the battery electrode, the wettability is much better if the electrolyte is injected twice than once.

[0119] (2) 55℃ Cycle Performance

[0120] The battery was placed in a 55°C environment, and the formed battery was charged to 5V with a 1C constant current and constant voltage, with a cut-off current of 0.02C, and then discharged to 2.75V with a 1C constant current. After such a charge / discharge cycle, the capacity retention rate after the 800th cycle was calculated to evaluate its cycle performance;

[0121] Capacity retention rate after 800 cycles at 55° C. (%)=100%×discharge capacity at the 800th cycle / discharge capacity at the first cycle.

[0122] Among them, the test results of the 55°C cycle capacity retention rate of the batteries containing the non-aqueous electrolytes of Examples 1-17 and Comparative Examples 1-4 are shown in Table 23. It can be seen that the capacity retention rate of Examples 1-17 is maintained at more than 80% after 800 cycles at 55°C, and that of Example 3 can reach 98.68%.

[0123] (3) 60℃ high temperature storage performance

[0124] The divided battery was charged to 5V at 25°C with 1C constant current and constant voltage, with a cut-off current of 0.02C, and then discharged to 2.75V with 1C constant current, and the initial discharge capacity of the battery was measured. Then, the battery was charged to 5V with 1C constant current and constant voltage, with a cut-off current of 0.02C, and the initial volume of the battery was measured. Then, the battery was stored at 65°C for 14 days, and the thickness of the battery after storage at 65°C was measured. Then, the battery was discharged to 2.75V with 1C constant current, and the retention capacity of the battery was measured. Then, the battery was charged to 5V with 1C constant current and constant voltage, with a cut-off current of 0.02C, and then discharged to 2.75V with 1C constant current, and the recovery capacity was measured. The calculation formulas for capacity retention rate, capacity recovery rate, and volume expansion are as follows:

[0125] Capacity retention rate (%) = 100% × retention capacity / initial capacity

[0126] Capacity recovery rate (%) = 100% × recovery capacity / initial capacity

[0127] Volume expansion rate (%) = 100% × (volume after 14 days - initial volume) / initial volume

[0128] Among them, the capacity retention rate test results of the batteries containing the non-aqueous electrolytes of Examples 1-17 and Comparative Examples 1-4 at 65°C high temperature storage are shown in Table 23. The non-aqueous electrolytes provided by Examples 3-15 and 17 have excellent high and low temperature performance. The capacity remaining rate and capacity recovery rate of the lithium-ion batteries containing them after 14 days of high temperature storage at 60°C are both greater than 90%, and Examples 1-2 and 16 both reach about 80%, and the battery volume change of each embodiment is small; while the capacity recovery rate and capacity recovery rate of Comparative Example 1-2 after high temperature storage are extremely low, and the volume expansion is very serious with the extension of storage time.

[0129] Tables 2 to 22 show the test results of the cycle performance and safety performance of lithium-ion batteries prepared using the electrolyte formulations of Examples 1-17 and Comparative Examples 1-4.

[0130] Table 23 shows the test results of the cycle performance and high temperature storage performance of Examples 1-17 and Comparative Examples 1-4.

[0131] Table 2 Cycle and safety performance test of lithium ion battery prepared by electrolyte of Example 1

[0132] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS NG NG Short Circuit PASS PASS NG NG NG NG acupuncture PASS PASS PASS PASS NG NG Low pressure PASS PASS PASS PASS PASS PASS

[0133] Table 3 Cycling and safety performance test of lithium ion batteries prepared by electrolyte of Example 2

[0134] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS NG NG Short Circuit PASS PASS PASS NG NG NG acupuncture PASS PASS PASS PASS NG NG Low pressure PASS PASS PASS PASS PASS PASS

[0135] Table 4 Cycle and safety performance test of lithium ion battery prepared by electrolyte of Example 3

[0136]

[0137]

[0138] Table 5 Cycling and safety performance test of lithium ion batteries prepared by electrolyte of Example 4

[0139] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS PASS PASS Short Circuit PASS PASS PASS PASS PASS PASS acupuncture PASS PASS PASS PASS PASS PASS Low pressure PASS PASS PASS PASS PASS PASS

[0140] Table 6 Cycle and safety performance test of lithium ion battery prepared by electrolyte of Example 5

[0141] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS PASS PASS Short Circuit PASS PASS PASS PASS PASS PASS acupuncture PASS PASS PASS PASS PASS PASS Low pressure PASS PASS PASS PASS PASS PASS

[0142] Table 7 Cycle and safety performance test of lithium ion battery prepared by electrolyte of Example 6

[0143] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS PASS PASS Short Circuit PASS PASS PASS PASS PASS PASS acupuncture PASS PASS PASS PASS PASS PASS

[0144] Table 8 Cycle and safety performance test of lithium ion batteries prepared by electrolyte in Example 7

[0145]

[0146]

[0147] Table 9 Cycle and safety performance test of lithium ion batteries prepared by electrolyte in Example 8

[0148] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS PASS PASS Short Circuit PASS PASS PASS PASS PASS PASS acupuncture PASS PASS PASS PASS PASS PASS Low pressure PASS PASS PASS PASS PASS PASS

[0149] Table 10 Cycle and safety performance test of lithium ion batteries prepared by electrolyte of Example 9

[0150] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS PASS PASS Short Circuit PASS PASS PASS PASS PASS PASS acupuncture PASS PASS PASS PASS NG NG Low pressure PASS PASS PASS PASS PASS PASS

[0151] Table 11 Cycling and safety performance test of lithium ion batteries prepared by electrolyte of Example 10

[0152] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS PASS PASS Short Circuit PASS PASS PASS PASS PASS NG acupuncture PASS PASS PASS NG NG NG Low pressure PASS PASS PASS PASS PASS PASS

[0153] Table 12 Cycle and safety performance test of lithium ion battery prepared by electrolyte of Example 11

[0154] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS PASS PASS Short Circuit PASS PASS PASS PASS PASS PASS acupuncture PASS PASS PASS PASS NG NG Low pressure PASS PASS PASS PASS PASS PASS

[0155] Table 13 Cycling and safety performance test of lithium ion batteries prepared by electrolyte of Example 12

[0156] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS PASS PASS Short Circuit PASS PASS PASS PASS PASS PASS acupuncture PASS PASS PASS PASS NG NG Low pressure PASS PASS PASS PASS PASS PASS

[0157] Table 14 Cycling and safety performance test of lithium ion batteries prepared by electrolyte of Example 13

[0158] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS PASS PASS Short Circuit PASS PASS PASS PASS PASS PASS acupuncture PASS PASS PASS PASS NG NG Low pressure PASS PASS PASS PASS PASS PASS

[0159] Table 15 Cycling and safety performance test of lithium ion batteries prepared by electrolyte of Example 14

[0160] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS PASS PASS Short Circuit PASS PASS PASS PASS PASS PASS acupuncture PASS PASS PASS PASS NG NG Low pressure PASS PASS PASS PASS PASS PASS

[0161] Table 16 Cycle and safety performance test of lithium ion battery prepared by electrolyte of Example 15

[0162] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS PASS PASS Short Circuit PASS PASS PASS PASS PASS NG acupuncture PASS PASS PASS NG NG NG Low pressure PASS PASS PASS PASS PASS PASS

[0163] Table 17 Cycle and safety performance test of lithium ion battery prepared by electrolyte of Example 16

[0164] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS NG NG Short Circuit PASS PASS PASS NG NG NG acupuncture PASS PASS PASS PASS NG NG Low pressure PASS PASS PASS PASS PASS PASS

[0165] Table 18 Cycle and safety performance test of lithium ion battery prepared by electrolyte of Example 17

[0166] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS PASS Transport vibration PASS PASS PASS PASS PASS PASS Heavy object impact PASS PASS PASS PASS PASS PASS Thermal shock PASS PASS PASS PASS PASS PASS Overcharge PASS PASS PASS PASS PASS PASS Short Circuit PASS PASS PASS PASS PASS PASS acupuncture PASS PASS PASS PASS NG NG Low pressure PASS PASS PASS PASS PASS PASS

[0167] Table 19 Cycle and safety performance test of lithium ion batteries prepared by electrolyte of comparative example 1

[0168] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS NG NG Transport vibration PASS PASS PASS PASS NG NG Heavy object impact PASS PASS PASS PASS NG NG Thermal shock NG NG NG NG NG NG Overcharge NG NG NG NG NG NG Short Circuit NG NG NG NG NG NG acupuncture NG NG NG NG NG NG Low pressure PASS PASS PASS PASS NG NG

[0169] Table 20 Cycle and safety performance test of lithium ion batteries prepared by electrolyte of comparative example 2

[0170] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS NG NG Transport vibration PASS PASS PASS PASS NG NG Heavy object impact PASS PASS PASS PASS NG NG Thermal shock NG NG NG NG NG NG Overcharge NG NG NG NG NG NG Short Circuit NG NG NG NG NG NG acupuncture NG NG NG NG NG NG Low pressure PASS PASS PASS PASS NG NG

[0171] Table 21 Cycle and safety performance test of lithium ion batteries prepared by electrolyte of comparative example 3

[0172] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS NG Transport vibration PASS PASS PASS PASS PASS NG Heavy object impact PASS PASS PASS PASS PASS NG Thermal shock PASS PASS PASS PASS PASS NG Overcharge NG NG NG NG NG NG Short Circuit NG NG NG NG NG NG acupuncture NG NG NG NG NG NG Low pressure PASS PASS PASS PASS PASS NG

[0173] Table 22 Cycle and safety performance test of lithium ion battery prepared by electrolyte of comparative example 4

[0174] Cycle times 1 200 300 400 500 600 Drop test PASS PASS PASS PASS PASS NG Transport vibration PASS PASS PASS PASS PASS NG Heavy object impact PASS PASS PASS PASS PASS NG Thermal shock NG NG NG NG NG NG Overcharge NG NG NG NG NG NG Short Circuit NG NG NG NG NG NG acupuncture NG NG NG NG NG NG Low pressure PASS PASS PASS PASS PASS NG

[0175] Table 23 Cyclic performance and high temperature storage performance test of Examples 1-17 and Comparative Examples 1-4

[0176]

[0177]

[0178] The embodiments described above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A secondary battery electrolyte, It is characterized in that The electrolyte includes a first electrolyte and a second electrolyte, and the mass ratio of the first electrolyte to the second electrolyte is (5-9): (1-5); Taking the total mass of the first electrolyte as 100%, the first electrolyte comprises 5-25% of a cyclic carbonate solvent, 20-35% of a chain carbonate solvent, 20-35% of a chain carboxylate solvent, 5-10% of a first film-forming additive and 9-15% of a lithium salt; Taking the total mass of the second electrolyte as 100%, the second electrolyte includes 10-25% of a cyclic carbonate solvent, 10-20% of a chain carbonate solvent, 5%-10% of a fluorocarbonate, 10-35% of a chain carboxylate solvent, 0.1%-5% of a second film-forming additive, and 10-20% of a lithium salt; The first film-forming additive includes a sulfur-containing additive and a silicon-containing additive; The second film-forming additive includes a compound A as shown in Formula 1; Among them, the R 1 and R 2 are each independently selected from H, halogen, substituted or unsubstituted C 1 -C 6 Straight chain or branched alkyl, substituted or unsubstituted C 2 -C 6 Alkenyl, substituted or unsubstituted C 2 -C 6 Alkyne, sulfonyl halide, substituted or unsubstituted C 6 -C 20 Aryl, substituted or unsubstituted C 1 -C 6 Alkylsulfone, substituted or unsubstituted C 6 -C 20 Aryl, substituted or unsubstituted C 1 -C 6 Any one of a silyl group, a carbonyl group or a sulfonyl halide group; And, the R 1 and R 2 At least one of them is a fluorine-containing group; The R 3 -CH 2 -、-CH 2 CH 2 -or-CH 2 CH 2 CH 2 -.

2. The secondary battery electrolyte according to claim 1, It is characterized in that The R 1 and R 2 Each independently selected from H, -C 4 H 7 , -C 2 H 5 、-CH 3 、-CH 2 CF 3 , CH 2 CHF 2 , CHF 2 , -CF 3 , -CF 2 Br, C 2 H 4 NH 2 , =O or Li.

3. The secondary battery electrolyte according to claim 1, It is characterized in that The compound A includes one or more of the following compounds:

4. The secondary battery electrolyte according to claim 1, It is characterized in that The cyclic carbonate solvents include ethylene carbonate and propylene carbonate; Preferably, the mass ratio of ethylene carbonate to propylene carbonate is 1:(0.2-1).

5. The secondary battery electrolyte according to claim 1, It is characterized in that The chain carbonate solvent includes one or more of ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, allyl methyl carbonate or diethyl pyrocarbonate, preferably ethyl methyl carbonate.

6. The secondary battery electrolyte according to claim 1, It is characterized in that The chain carboxylate solvent includes one or more of methyl propionate, methyl acetate, propyl propionate, methyl butyrate, ethyl butyrate, propyl acetate, butyl butyrate, ethyl propionate or ethyl acetate, preferably propyl propionate.

7. The secondary battery electrolyte according to claim 1, It is characterized in that The fluorocarbonate solvent includes one or more of fluoroethylene carbonate, difluoroethylene carbonate, bisfluoropropylene carbonate, trifluoroethyl acetate, trifluoroethyl methyl carbonate, trifluoromethylethylene carbonate, 4-trifluoromethylethylene carbonate, chloroethylene carbonate, di(2,2,2-trifluoroethyl) carbonate, methyl trifluoropropionate, 3,3,3-trifluoroethyl acetate, methyl 2-(trifluoromethyl)benzoate, ethyl 4,4,4-trifluorobutyrate or 1,1,1,3,3,3-hexafluoroisopropyl acrylate, preferably a bisfluorocarbonate.

8. The secondary battery electrolyte according to claim 1, It is characterized in that The sulfur-containing additive includes one or more of vinyl sulfate, 1,3-propane sultone, 1,3-propene sultone, propylene sulfate, 1,4-butane sultone, vinylene sulfite or methylene disulfonate, preferably propylene sulfate and 1,4-propane sultone; Preferably, the silicon-containing additive comprises one or more of tetravinylsilane, tristrimethylsilane phosphate or tristrimethylsilane borate, preferably tetravinylsilane; Preferably, the mass ratio of the sulfur-containing additive to the silicon-containing additive is (5-10):1, preferably 8:1; Preferably, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium perchlorate, lithium trifluoromethanesulfonate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethylsulfonyl imide), lithium difluorophosphate, lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), lithium iodide, lithium tetrafluorooxalatophosphate, bis(tetrafluorophosphoryl imide), lithium tetrafluoroborate or lithium bis(oxalatoborate).

9. A lithium secondary battery, It is characterized in that The lithium secondary battery comprises a secondary battery electrolyte as claimed in any one of claims 1 to 8, wherein a first electrolyte is first injected into the battery, and after formation, a second electrolyte is injected; Preferably, after injecting the first electrolyte, the formation is performed after soaking for 16-18 hours; Preferably, the formation step includes first charging at 0.02C for 30 min, then charging at 0.05C for 30 min, then charging at 0.1C for 120 min, and then charging at 0.2C to a voltage of 3.85V; Preferably, after the second electrolyte is injected, the final sealing is performed after soaking for 18-20 hours, and then the final sealing is performed again after aging for 24 hours.

10. The lithium secondary battery according to claim 9, It is characterized in that The positive electrode active material of the lithium secondary battery is LiNi x Co y Mn z L (1-x-y-z) O 2 、LiCo x 1L (1-x1) O 2 、LiNix 2 Ly 1 Mn (2-x2-y1 ) 4 and Li z1 MPO 4 One or more of the following; Wherein, L is at least one of Co, Al, Sr, Mg, Ti, Ca, Zr, Zn, Si and Fe; M is at least one or two of Fe, Mn and Co; 0≤x≤1, 0≤y≤1, 0≤z≤1, 0≤x+y+z≤1, 0≤x1≤1, 0.3≤x2≤0.6, 0.01≤y1≤0.2, 0.5≤z1≤1; Preferably, the negative electrode active material of the lithium secondary battery includes single-element lithium metal, lithium alloy, carbon material, a composite material of single-crystal silicon and carbon, or a composite material of silicon monoxide and carbon.