Production process of sodium ion battery
By using materials such as NMP and PVDF in the production process of sodium ion batteries, the problems of low gas production and energy density of the negative electrode of sodium ion batteries are solved, and the circulation and safety performance are improved, achieving higher charge and discharge cycle times and safety sex.
Patent Information
- Application Number
- CN202411094856.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-11
- Publication Date
- 2024-11-22
AI Technical Summary
The negative electrode gas production phenomenon occurs during the charging and discharging process of sodium ion batteries, and the energy density is low and the safety performance is insufficient, limiting their large-scale application.
Using N-methylpyrrolidone (NMP) as solvent and polyvinylidene fluoride (PVDF) as binder, the glue solution is made by stirring, conductive agent and hard carbon are added, viscosity is adjusted, and the slurry is prepared and passed through roll Sodium ion batteries are made by winding, assembling, injecting liquid and sealing, avoiding gas production during moisture absorption and volatility.
The cycling performance, capacity performance and safety performance of sodium ion batteries have been improved, the gas production problem of negative electrodes has been solved, the 0.5C charge and discharge cycle performance and the first-effect capacity of the positive electrode material have been improved, and the ignition combustion phenomenon has been avoided.
Smart Images

Figure CN119009153A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of secondary batteries and relates to a production process of a sodium ion battery. Background Art
[0002] With the continuous development of secondary batteries, lithium-ion batteries have become the mainstream of secondary batteries. With the development of lithium-ion batteries and the current vigorous development of new energy and energy storage, the storage of lithium materials is scarce, resulting in a substantial increase in lithium materials.
[0003] As sodium is a widely used material resource, the transformation of lithium-ion batteries into sodium-ion batteries has become a market trend. Since sodium-ion batteries produce gas at the negative electrode during the charge and discharge process, and sodium ions are subject to the technical bottleneck of negative electrode materials, the positive electrode material has low initial efficiency, resulting in low energy density of sodium-ion batteries. In addition, sodium-ion batteries have the phenomenon of catching fire and burning during needle puncture tests, which limits their large-scale application.
[0004] Based on this, it is necessary to develop a production process for sodium ion batteries to solve the above problems. Summary of the invention
[0005] In view of the above problems existing in the prior art, the purpose of the present invention is to provide a production process for sodium ion batteries, solve the problem of gas production at the negative electrode, and improve the cycle performance, gram capacity and safety performance of sodium ion batteries.
[0006] The present invention provides a production process for a sodium ion battery, comprising:
[0007] The solvent used in the negative electrode batching process is N-methylpyrrolidone (NMP), and the binder is polyvinylidene fluoride (PVDF). NMP and PVDF are mixed and stirred in proportion to form a glue solution;
[0008] The conductive agent and the negative electrode active material are sequentially added to the glue solution, mixed evenly, and the viscosity is adjusted to obtain a slurry, which is then coated on a current collector, rolled and cut to obtain a negative electrode sheet, and the negative electrode sheet and the positive electrode sheet are wound, assembled, injected with electrolyte, and sealed to obtain a sodium ion battery.
[0009] As a preferred embodiment of the present invention, the interval time between the introduction of the slurry into the feeding system and the completion of coating is controlled within 60 minutes, and the interval time between slitting and winding is controlled within 1 to 2 hours.
[0010] As a preferred embodiment of the present invention, the negative electrode active material is hard carbon.
[0011] As a preferred embodiment of the present invention, the conductive agent is one or more of conductive carbon black, carbon nanotubes and graphene.
[0012] As a preferred embodiment of the present invention, the solid content of the slurry is 50-54wt%.
[0013] As a preferred embodiment of the present invention, the mass ratio of the negative electrode active material, the binder and the conductive agent is 96-98:1-2:1-2.
[0014] As a preferred embodiment of the present invention, two stirring steps are adopted in both the preparation of the glue solution and the mixing step, the first stirring rate is 800-900 r / min, and the second stirring rate is 1500-1600 r / min.
[0015] As a preferred embodiment of the present invention, the active material of the positive electrode sheet is sodium nickel iron manganese oxide.
[0016] The principle of the present invention is that: in the aqueous process, deionized water is used as the solvent in the stirring process. Its physical principle is to coat the hard carbon with water, adhesive and conductive agent through high-speed stirring to form a sticky slurry, so that the slurry can be attached to the aluminum foil during the coating process to form the electrode; and the hard carbon itself easily absorbs moisture. Although the drying process is carried out in the coating process, the moisture absorbed in the hard carbon structure cannot be completely removed through the drying process, which leads to the decomposition of moisture in the hard carbon structure into gas during the circulation process after the battery is made, as the ions move back and forth, resulting in gas production in the battery. The new process uses NMP as the solvent in the stirring process. NMP is an oily organic solvent and does not contain moisture itself. There is no moisture in the hard carbon coating during the stirring process. Secondly, NMP is a volatile organic solvent. All NMP can be volatilized through the drying process. Since the hard carbon does not absorb moisture inside, the battery will not produce gas during the circulation process.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The present invention provides a production process for a sodium ion battery, which solves the problem of negative electrode gas production and improves the cycle performance, gram capacity and safety performance of the sodium ion battery. The negative electrode gas production problem is solved by adjusting the negative electrode batching process, and at the same time, the first effective gram capacity of the positive electrode material is improved from 105 mAh / g to 118 mAh / g, and the first effective gram capacity of the positive electrode material is improved by 12%, and the 0.5C charge and discharge cycle performance is improved from 80% of the capacity retention rate of 2000 cycles to 80% of the capacity retention rate of 8000 cycles. The safety performance is better than that of water-based batteries. There is a fire phenomenon in the needle puncture test of water-based batteries, while there is no fire phenomenon in the needle puncture test of the new process. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The capacity retention curve of the sodium ion battery in Example 1 after 8000 charge and discharge cycles at 0.5C;
[0020] Figure 2The capacity retention curve of the sodium ion battery in Comparative Example 1 after 2000 charge and discharge cycles at 0.5C;
[0021] Figure 3 This is a picture of the acupuncture test of the sodium ion battery in Example 1;
[0022] Figure 4 This is a picture of the needle puncture test of the sodium ion battery in Comparative Example 1. DETAILED DESCRIPTION
[0023] In order to better explain the present invention, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings, but the following embodiments do not limit the protection scope of the claims.
[0024] The active material in the following examples is hard carbon, and its physical properties are shown in Table 1:
[0025] Table 1 Physical properties of hard carbon
[0026]
[0027]
[0028] The stirring involved below uses a mixer, revolution refers to the speed of the stirring paddle in the mixer, and dispersion refers to the speed of the dispersion disk in the mixer.
[0029] The present invention will be further described below through specific embodiments and drawings.
[0030] Comparative Example 1
[0031] In an environment with humidity ≤10%, the negative electrode stirring process is a conventional water-based process, and its production process is as follows: deionized water is used as a solvent in the negative electrode preparation process, and the binder is carboxymethyl cellulose (CMC for short). CMC and deionized water are mixed and stirred in proportion to form a glue solution, and conductive carbon black (SP for short) and active substances are added to the glue solution in sequence, mixed evenly, and the viscosity is adjusted to obtain a slurry, which is coated on a current collector, rolled and cut to obtain a negative electrode sheet, and the negative electrode sheet and the positive electrode sheet are wound, assembled, injected, and sealed to obtain a sodium ion battery.
[0032] Example 1
[0033] A sodium ion battery production process, at a humidity of ≤10%, comprising:
[0034] S1. Under a temperature of 25±3°C, the solvent used in the negative electrode batching process is N-methylpyrrolidone (NMP), and the binder is polyvinylidene fluoride (PVDF). NMP and PVDF are mixed and stirred in proportion to form a glue solution;
[0035] S2. Add the conductive agent and hard carbon to the glue solution in turn, mix them evenly, adjust the viscosity, and prepare a slurry with a solid content of 52wt%. Apply the slurry on the current collector, roll and cut it to obtain a negative electrode sheet, and then wind, assemble, inject and seal the negative electrode sheet and the positive electrode sheet to obtain a sodium ion battery.
[0036] Specifically, the conductive agent is carbon nanotube (CNT) and graphene, and the mass ratio thereof is 0.6:0.6; the mass ratio of hard carbon, PVDF, and conductive agent is 97:1.8:1.2.
[0037] Specifically, the active material of the positive electrode sheet is layered oxide sodium nickel iron manganese oxide, and the electrolyte is sodium hexafluorophosphate.
[0038] In step S2, after the mixing is completed, the slurry is transferred into the storage tank through the feed port of the automatic feeding system for stirring and storage, and the slurry is automatically fed into the coating head from the discharge port. The coating head material tank is equipped with a liquid level sensor. When the slurry level in the material tank is lower than the sensing position of the sensor, the slurry is automatically added to the position that the sensor can sense, ensuring that the slurry amount in the coating head material tank is in a stable state for coating, and the coating humidity is controlled at ≤10% and the temperature is 25±3℃. After coating, the coated electrode is placed in the oven for vacuum baking. The baking parameters are as follows: temperature 85±5℃, vacuum ≥80%, and baking time 4h. Nitrogen needs to be filled in every 1h of baking and then vacuumed for ventilation. After ventilation 4 times, the baking temperature is turned off and vacuumed for storage. After the surface temperature of the electrode drops to room temperature, the electrode is taken out for rolling. The humidity in the rolling workshop is controlled at ≤10% and the temperature is 25±3℃. After rolling, the electrode is transferred to the slitting process and cut into the electrode width required by the process. After slitting, the electrode is transferred to the production workshop. The humidity in the production workshop is controlled at ≤10% and the temperature is 25±3℃. The new process negative electrode is obtained by welding the pole ears and sticking protective tape in the production workshop. The obtained negative electrode is rolled into a cylinder with the positive electrode diaphragm through winding. The core is wound and loaded into the steel shell. The semi-finished battery cells are put into a vacuum oven for baking. The baking process is as follows: temperature 85±℃, baking time 48h, vacuum degree ≥90%. Nitrogen needs to be filled in for 1h of baking and then vacuumed for ventilation. After 48 times, the baking is stopped. The surface temperature of the battery cells is reduced to below 45℃ through nitrogen filling and vacuuming cycles. The nitrogen filling cycle is repeated for 10s, pressure maintenance for 30s, vacuuming for 3min, and vacuum maintenance for 10min for 30 times. After the battery cells are cooled, the battery cells are taken out and transferred to the liquid filling and sealing workshop in batches. The dew point of the liquid filling and sealing workshop is controlled below -35℃. The liquid filling workshop performs bottom welding, groove rolling, cap welding, liquid injection, and sealing the cap on the upper end of the steel shell to obtain a sodium ion battery.
[0039] Example 2
[0040] The sodium ion battery prepared in Example 1 is activated by formation, and then a capacity division process is performed after activation. The battery capacity is tested in the capacity division process to obtain the battery capacity. The first effective gram capacity of the positive electrode material is calculated by the battery capacity and the amount of the positive electrode material active substance, as shown in Table 2:
[0041] Table 2 First effective gram capacity of positive electrode materials
[0042]
[0043] When the same positive electrode sheet is matched with negative electrodes of different processes, the capacity of the positive electrode material is significantly different. The gram capacity of the new process is significantly higher than that of the aqueous gram capacity. The new process can bring the capacity of the positive electrode material to the material design capacity. The material design gram capacity is 118mAh / g, and the new process can achieve it. Only the aqueous process can bring the capacity of the positive electrode material to 87.5%.
[0044] Example 3
[0045] The sodium ion batteries prepared in Example 1 and Comparative Example 1 were subjected to cycle performance tests: the same positive electrode sheet was matched with negative electrode sheets of different processes, and the new process had a capacity retention rate of more than 80% after 8000 charge and discharge cycles at 0.5C (see Figure 1 ), while the water-based process 0.5C charge and discharge cycle 2000 times capacity retention rate of more than 80% (see Figure 2 ); It can be seen that the new process cycle performance is better than the water cycle performance.
[0046] Example 4
[0047] The sodium ion batteries prepared in Example 1 and Comparative Example 1 were tested for safety performance: when the same positive electrode sheet was matched with negative electrodes of different processes, the battery made by the aqueous process still had a flash spark phenomenon during the needle puncture test (see Figure 3 ), while no obvious sparks were found in the needle puncture test of the new process, only white smoke appeared (see Figure 4 ), it can be seen that the new process will not cause fire and combustion during the needle puncture experiment, while the water-based process will cause sparks and fire and combustion during the needle puncture experiment.
[0048] Example 5
[0049] The sodium ion batteries prepared in Example 1 and Comparative Example 1 were subjected to gas production detection: the sodium ion batteries made with the same positive electrode matched with different negative electrodes were disassembled after 500 cycles, and it was found that the batteries made with the new process did not produce gas, while the batteries made with the aqueous process produced gas during dissection, and the gas pressure was relatively high.
[0050] The difference between the water-based process and the new process is that the water-based process uses deionized water as the solvent in the stirring process. Its physical principle is to use high-speed stirring to coat the hard carbon with water, adhesive and conductive agent to form a sticky slurry, so that the slurry can be attached to the aluminum foil during the coating process to make the electrode; hard carbon itself easily absorbs moisture. Although the drying process is carried out in the coating process, the moisture absorbed in the hard carbon structure cannot be completely removed through the drying process, resulting in the moisture in the hard carbon structure being decomposed into gas during the circulation process after the battery is made. As a result, the battery produces gas during the cycle. The new process uses NMP as the solvent in the stirring process. NMP is an oily organic solvent, which does not contain moisture itself. There is no moisture in the hard carbon coating during the stirring process. Secondly, NMP is a volatile organic solvent. All NMP can be volatilized through the drying process. Since the hard carbon does not absorb moisture inside, the battery will not produce gas during the circulation process.
[0051] Example 6
[0052] A sodium ion battery production process, at a humidity of ≤10%, comprising:
[0053] S1. Under a temperature of 25±3°C, the solvent used in the negative electrode batching process is N-methylpyrrolidone (NMP), and the binder is polyvinylidene fluoride (PVDF). NMP and PVDF are mixed and stirred in proportion to form a glue solution;
[0054] S2. Add the conductive agent and hard carbon to the glue solution in turn, mix them evenly, adjust the viscosity, and prepare a slurry with a solid content of 54wt%. Apply the slurry on the current collector, roll and cut to obtain a negative electrode sheet, and then wind, assemble, inject and seal the negative electrode sheet and the positive electrode sheet to obtain a sodium ion battery.
[0055] Specifically, the conductive agent is conductive carbon black SP and graphene, and the mass ratio thereof is 0.8:0.8; the mass ratio of hard carbon, PVDF, and conductive agent is 97:1.4:1.6.
[0056] Specifically, the active material of the positive electrode sheet is layered oxide sodium nickel iron manganese oxide, and the electrolyte is sodium hexafluorophosphate.
[0057] Specifically, two stirring steps are used in the steps of preparing the glue solution and mixing, with the first stirring rate being 900 r / min and the second stirring rate being 1500 r / min.
[0058] Example 7
[0059] A sodium ion battery production process, at a humidity of ≤10%, comprising:
[0060] S1. Under a temperature of 25±3°C, the solvent used in the negative electrode batching process is N-methylpyrrolidone (NMP), and the binder is polyvinylidene fluoride (PVDF). NMP and PVDF are mixed and stirred in proportion to form a glue solution;
[0061] S2. Add the conductive agent and hard carbon to the glue solution in turn, mix them evenly, adjust the viscosity, and prepare a slurry with a solid content of 50wt%. Apply the slurry on the current collector, roll and cut it to obtain a negative electrode sheet, and then wind, assemble, inject and seal the negative electrode sheet and the positive electrode sheet to obtain a sodium ion battery.
[0062] Specifically, the conductive agent is conductive carbon black SP and carbon nanotubes (CNT), and the mass ratio thereof is 1:1; the mass ratio of hard carbon, PVDF, and conductive agent is 96:2:2.
[0063] Specifically, the active material of the positive electrode sheet is layered oxide sodium nickel iron manganese oxide, and the electrolyte is sodium hexafluorophosphate.
[0064] In the above embodiments, the chemical reagents used are all commercial reagents, and the test methods and sodium battery assembly processes used are all prior art, which will not be described in detail in this patent. For details, please refer to patents CN115172644B and CN115084792B.
[0065] The present invention is not limited to the above-mentioned embodiments, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A production process for sodium ion batteries, It is characterized in that include: The solvent used in the negative electrode batching process is N-methylpyrrolidone, and the binder is polyvinylidene fluoride. N-methylpyrrolidone and polyvinylidene fluoride are mixed and stirred according to a certain proportion to form a glue solution; The conductive agent and the negative electrode active material are sequentially added to the glue solution, mixed evenly, and the viscosity is adjusted to obtain a slurry, which is then coated on a current collector, rolled and cut to obtain a negative electrode sheet, and the negative electrode sheet and the positive electrode sheet are wound, assembled, injected with electrolyte, and sealed to obtain a sodium ion battery.
2. A production process for a sodium ion battery according to claim 1, It is characterized in that The interval time between the slurry being introduced into the feeding system and the coating being completed is controlled within 60 minutes, and the interval time between the slitting and winding is controlled within 1 to 2 hours.
3. A production process for a sodium ion battery according to claim 1, It is characterized in that The negative electrode active material is hard carbon.
4. A production process for a sodium ion battery according to claim 1, It is characterized in that The conductive agent is one or more of conductive carbon black, carbon nanotubes and graphene.
5. A production process for a sodium ion battery according to claim 1, It is characterized in that The solid content of the slurry is 50-54 wt %.
6. A production process for a sodium ion battery according to claim 1, It is characterized in that The mass ratio of the negative electrode active material, the binder and the conductive agent is 96-98:1-2:1-2.
7. A production process for a sodium ion battery according to claim 1, It is characterized in that In both the steps of preparing the glue solution and mixing, stirring is performed twice, the first stirring rate is 800-900 r / min, and the second stirring rate is 1500-1600 r / min.