Additive of aqueous zinc ion battery, electrolyte and aqueous zinc ion battery
By using organic salts of phospho-oxygen functional groups in aqueous zinc ion batteries to construct the interface protective layer of organic inorganic composite solid electrolyte, the passivation, corrosion and dendritic growth of zinc negative electrodes are solved, and the cycle stability and Coulomb efficiency of the battery are improved. Large-scale energy storage application.
Patent Information
- Application Number
- CN202410900408.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-22
AI Technical Summary
The aqueous zinc ion battery has problems such as passivation, corrosion, hydrogen evolution and dendrite growth during the deposition/stripping process of zinc negative electrode, resulting in low Coulomb efficiency, low capacity and limited cycle life, which limits its application.
Using organic salts containing phosphorus and oxygen functional groups as electrolyte additives, the interface protective layer of organic inorganic composite solid electrolyte is constructed on the surface of zinc negative electrode to form zinc-oxygen bonds to regulate the conduction of zinc ions, inhibit dendrites' growth and corrosion, and improve circulation stability. sex.
It achieves long cycle life under large current density and deposition capacity, reduces corrosion and passivation of zinc negative electrodes, improves the Coulomb efficiency and safety of zinc ion batteries, and is suitable for large-scale energy storage applications.
Smart Images

Figure CN119009159A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery electrolytes, and in particular relates to an additive for an aqueous zinc ion battery, an electrolyte and an aqueous zinc ion battery. Background Art
[0002] The development and application of new high-energy-density energy storage systems is a hot topic of common concern in today's scientific and industrial communities. Today, the commercialization of lithium-ion batteries has brought great convenience to people's lives, but there is a shortcoming: they usually use organic systems as electrolytes, which have safety hazards such as flammability and explosion. At the same time, the reserves of lithium ore resources are small, resulting in relatively high costs for lithium-ion batteries, making it difficult to apply them in large-scale energy storage fields. Therefore, it is urgent to develop new battery technologies that are intrinsically safe and low-cost. Among them, aqueous zinc-ion batteries use metallic zinc as the negative electrode and have a high theoretical capacity (820mAh·g -1 and 5855mAh·cm -3 ), low electrochemical potential (-0.762V relative to the standard hydrogen electrode), simple preparation process, rich content, low cost, safety and environmental protection, etc., have attracted widespread attention. However, the metal zinc anode inevitably has problems such as passivation, corrosion, hydrogen evolution and dendrite growth during the deposition / stripping process, resulting in low Coulombic efficiency, low capacity and limited cycle life of zinc-ion batteries, which restricts its practical application.
[0003] In response to these problems with zinc negative electrodes, researchers have proposed many strategies to inhibit zinc dendrite growth and side reactions and thus improve the cycle performance of zinc ion batteries, such as surface coating modification, negative electrode structure optimization, and electrolyte modification. The first two require the construction of an artificial coating on the zinc metal surface and secondary design and processing of the zinc metal negative electrode, which leads to a high overall production cost. In addition, these non-in-situ modification strategies will make the coating or three-dimensional structure introduced on the negative electrode surface very easy to deform and collapse during repeated electroplating-stripping processes, thereby losing the protective effect. The modification strategy of introducing multifunctional additives into the electrolyte is not only inexpensive, easy to operate, and suitable for large-scale energy storage applications, but also can form a solid electrolyte interface in situ on the zinc negative electrode surface during the charge and discharge process, which can effectively inhibit the dendrite growth, hydrogen evolution and corrosion of the zinc metal negative electrode during the cycle, greatly improving the Coulomb efficiency and cycle stability of aqueous zinc ion batteries.
[0004] At present, it has been reported that by introducing various additives into the electrolyte, it has the advantages of high ionic conductivity and good compatibility with the electrode-electrolyte interface. However, these electrolyte systems usually cannot ensure that the zinc negative electrode has a long cycle life, which seriously hinders the development and application of aqueous zinc-ion batteries. In addition, the functions of the additives currently introduced into the electrolyte are relatively simple. For example, while playing a role in slowing down the dehydrogenation reaction, it will sacrifice the kinetics of the zinc deposition process and reduce the ionic conductivity of the electrolyte; while directional regulation of (002) crystal surface zinc deposition, it is easy to reduce the pH value of the electrolyte, causing serious hydrogen evolution side reactions in the electrolyte.
[0005] Therefore, there is an urgent need to develop a zinc ion battery aqueous electrolyte that is cheap, low in concentration, has high ionic conductivity and good cycle performance. Summary of the invention
[0006] In order to solve the problem of poor cycle performance of aqueous zinc ion batteries in the prior art due to passivation, corrosion, hydrogen evolution and dendrite growth, the present invention provides an additive for aqueous zinc ion batteries.
[0007] The additive of the aqueous zinc ion battery comprises an organic salt containing a phosphorus oxygen functional group, and the negative electrode material of the aqueous zinc ion battery is zinc.
[0008] Furthermore, the additives of the aqueous zinc ion battery also include zinc salts.
[0009] Further, the organic salt containing a phosphorus oxygen functional group is selected from one or more of [[(phosphorylmethyl)imino]bis[(2,1-ethylenediaminebis(methylene)]]tetraphosphonic acid, [[(phosphorylmethyl)imino]bis[(2,1-ethylenediaminebis(methylene)]]tetraphosphonic acid heptathodium and [[(phosphorylmethyl)imino]bis[(2,1-ethylenediaminebis(methylene)]]tetraphosphonic acid tetrasodium;
[0010] The zinc salt is selected from one or more of zinc sulfate, zinc methanesulfonate, zinc trifluoromethanesulfonate, zinc imide trifluoromethanesulfonate, zinc chloride, zinc hexafluorosilicate, zinc perchlorate and zinc nitrate.
[0011] The negative electrode material of the aqueous zinc ion battery is zinc sheet, zinc powder or zinc mesh.
[0012] The invention also provides an electrolyte containing the additive for an aqueous zinc ion battery.
[0013] The electrolyte containing the additive for aqueous zinc ion batteries comprises the additive for aqueous zinc ion batteries as described in any one of the above items.
[0014] Furthermore, the concentration of the organic salt containing phosphorus oxygen functional groups is 0.001 to 1 mmol / L;
[0015] The concentration of the zinc salt is 0.5-3 mol / L.
[0016] The invention also provides a method for preparing an electrolyte containing the additive for an aqueous zinc ion battery.
[0017] The preparation method of the electrolyte containing the additive of the aqueous zinc ion battery comprises the following steps:
[0018] The organic salt containing phosphorus oxygen functional groups is added to deionized water, stirred at 25-50° C. for 2-5 hours, and then ultrasonicated, and then the zinc salt is added, stirred at 25-60° C. to obtain the electrolyte containing the additive for aqueous zinc ion batteries.
[0019] Furthermore, ultrasound 1 hour long;
[0020] Stirring time: 4 hours;
[0021] The deionized water is ultrapure water with a resistivity of 18 MΩ*cm.
[0022] The invention also provides an aqueous zinc ion battery.
[0023] The aqueous zinc ion battery comprises a zinc negative electrode and an electrolyte containing the additive for aqueous zinc ion battery as described above.
[0024] Furthermore, the positive electrode material of the aqueous zinc ion battery is manganese dioxide, vanadium pentoxide, zinc iodide, sodium vanadate, ammonium vanadate, bimetallic sulfide or nitrogen-oxygen-containing organic matter;
[0025] The separator is selected from glass fiber separator, cellulose separator, filter paper or PP separator.
[0026] Furthermore, the aqueous zinc ion battery is a zinc ion soft pack battery, comprising an aluminum plastic film, a negative electrode current collector, a zinc negative electrode, a positive electrode, a positive electrode current collector, a separator and an electrolyte containing an additive for an aqueous zinc ion battery as described in any one of the above items, wherein the negative electrode current collector includes but is not limited to titanium foil, carbon fiber cloth, graphite paper, tinned copper foil, the zinc negative electrode is selected from zinc sheet, zinc powder, foamed zinc or zinc mesh, the separator includes a glass fiber separator, a cellulose separator or a hydrophilic polypropylene separator, and the amount of the electrolyte is 50 to 200 μL / cm 2 , the positive electrode of the zinc ion battery includes at least one of manganese dioxide, vanadium pentoxide, and iodine, and the positive electrode current collector includes at least one of a titanium mesh, a carbon fiber cloth, and a tinned copper mesh;
[0027] The aqueous zinc ion battery is an assembled button battery, comprising a positive electrode shell, a gasket, a zinc sheet / positive electrode sheet, a diaphragm, a zinc sheet, a gasket, a spring, a negative electrode shell and an electrolyte containing an additive for aqueous zinc ion batteries as described in any one of the above items.
[0028] Compared with the prior art, the advantages of the present invention are mainly reflected in the following aspects:
[0029] 1) The electrolyte containing organic additives with phosphorus and oxygen functional groups provided in the present application can form an in-situ organic-inorganic composite solid electrolyte interface protection layer on the surface of the zinc negative electrode based on chemical bonding, while ensuring the advantages of high ionic conductivity, low cost and environmental protection of pure aqueous electrolytes.
[0030] 2) The inner layer of the organic-inorganic composite solid electrolyte interface protection layer is a zinc-oxygen bond formed by the phosphorus-oxygen functional groups of organic molecules and the zinc negative electrode, which can limit the two-dimensional diffusion of zinc ions and regulate the conduction of zinc ions, effectively solving the problem of easy growth of dendrites on the zinc negative electrode during charging and discharging. The outer organic structure can repel the active water in the electrolyte, solving the problem of easy corrosion and passivation of the zinc negative electrode in the aqueous electrolyte.
[0031] 3) It was applied in rechargeable aqueous zinc-ion batteries, achieving long cycle life at high current density and deposition capacity, indicating that the electrolyte configured with organic matter containing phosphorus and oxygen functional groups as additives has broad application prospects in low-cost, high-safety and large-scale zinc-ion batteries. The electrolyte was also applied in zinc-ion soft-pack full batteries. The assembled zinc-ion soft-pack full batteries had a discharge capacity of more than 75mAh and a cycle life of about 1130 cycles at a high current density of 200mA.
[0032] 4) The materials involved in this application have the advantages of abundant sources, low prices, simple preparation and processing technology, and wide application range. They have great application prospects and research value in aqueous zinc ion energy storage devices and other battery systems, which is conducive to the further development of large-scale energy storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is the technical route for aqueous zinc-ion batteries;
[0034] Figure 2 The infrared spectrum of the electrolyte provided in Example 1;
[0035] Figure 3 The electron microscope scanning image provided for Example 1;
[0036] Figure 4 Cyclic performance diagram provided for Example 3;
[0037] Figure 5 The cycle-capacity diagram of the zinc-iodine button cell provided in Example 3;
[0038] Figure 6 The cycle-capacity diagram of the zinc-iodine soft-pack full battery provided in Example 3;
[0039] Figure 7 This is a Tafel test effect diagram provided in Example 3. DETAILED DESCRIPTION
[0040] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation modes of the present invention are described in detail below with reference to the accompanying drawings, but they should not be construed as limiting the applicable scope of the present invention.
[0041] The present invention aims at the above-mentioned problems faced by zinc ion batteries, and designs an organic salt containing phosphorus oxygen functional groups as an aqueous electrolyte additive. It can construct a layer of organic-inorganic composite solid electrolyte interface protective layer rich in phosphorus oxygen functional groups on the surface of the zinc negative electrode in situ. The solid electrolyte interface protective layer has a double-layer structure, the inner layer is an inorganic substance rich in phosphorus oxygen functional groups, which is riveted together with zinc metal by forming zinc-oxygen bonds, and the outer layer is an organic molecule. The anchored zinc-oxygen bond can orderly regulate the conduction of zinc ions, regulate the directional deposition of zinc to inhibit dendrite growth, hydrogen evolution, and the occurrence of corrosion side reactions, and improve the cycle life of aqueous zinc ion batteries under high current density and large deposition capacity. Secondly, the solid electrolyte interface protective layer effectively isolates the direct contact between the zinc metal negative electrode and the active water molecules in the electrolyte, and solves the problem of easy corrosion of the zinc negative electrode interface. Thirdly, the preparation method of the electrolyte system has the characteristics of simple preparation process, mild preparation conditions, low raw material cost, etc., which is convenient for large-scale production.
[0042] The invention provides an additive for an aqueous zinc ion battery, comprising an organic salt containing a phosphorus oxygen functional group. The negative electrode material of the aqueous zinc ion battery is zinc.
[0043] Optionally, the organic salt containing a phosphorus oxygen functional group is selected from one or more of [[(phosphorylmethyl)imino]bis[(2,1-ethylenediaminebis(methylene)]]tetraphosphonic acid, [[(phosphorylmethyl)imino]bis[(2,1-ethylenediaminebis(methylene)]]tetraphosphonic acid heptathodium and [[(phosphorylmethyl)imino]bis[(2,1-ethylenediaminebis(methylene)]]tetraphosphonic acid tetrasodium.
[0044] Organic salts containing phosphorus and oxygen functional groups can realize the in-situ construction of an organic-inorganic composite solid electrolyte interface protection layer on the surface of the zinc negative electrode, regulate the conduction of zinc ions, reduce interfacial hydrogen evolution and corrosion side reactions, and improve the cycle life of aqueous zinc ion batteries under high current density and large deposition capacity.
[0045] Optionally, the negative electrode material of the aqueous zinc ion battery is zinc sheet, zinc powder or zinc mesh.
[0046] Furthermore, the additives of the aqueous zinc ion battery also include zinc salts.
[0047] Optionally, the zinc salt is selected from one or more of zinc sulfate, zinc methanesulfonate, zinc trifluoromethanesulfonate, zinc imide trifluoromethanesulfonate, zinc chloride, zinc hexafluorosilicate, zinc perchlorate and zinc nitrate.
[0048] Zinc salts have high solubility in aqueous electrolytes and do not react with phosphorus-containing additives, which reduces the cost and viscosity of the electrolyte while ensuring high ionic conductivity.
[0049] The present invention also provides an electrolyte containing an additive for an aqueous zinc ion battery, comprising the additive for an aqueous zinc ion battery described in any one of the above.
[0050] Optionally, the concentration of the organic salt containing phosphorus oxygen functional groups is 0.001-1 mmol / L.
[0051] Optionally, the concentration of the zinc salt is 0.5 to 3 mol / L.
[0052] The present invention also provides a method for preparing an electrolyte containing an additive for an aqueous zinc ion battery, comprising the following steps:
[0053] An organic salt containing a phosphorus oxygen functional group is added to deionized water, stirred at 25-50° C. for 2-5 hours, and then ultrasonicated, and then a zinc salt is added, stirred at 25-60° C. to obtain an electrolyte containing an additive for an aqueous zinc ion battery.
[0054] Optionally, the sonication duration is 1 hour.
[0055] Optionally, stirring is continued for 4 hours.
[0056] Optionally, the deionized water is ultrapure water with a resistivity of 18 MΩ*cm.
[0057] The duration of ultrasound and stirring is not limited to the duration mentioned above. The duration of ultrasound and stirring can be determined according to circumstances in order to obtain a uniform and stably dispersed electrolyte containing the additive for aqueous zinc ion batteries.
[0058] See also Figure 1 Based on the above-provided electrolyte containing an aqueous zinc ion battery additive and a preparation method thereof, the present invention provides an aqueous zinc ion battery including a zinc negative electrode.
[0059] Optionally, the positive electrode material of the aqueous zinc ion battery is manganese dioxide, vanadium pentoxide, zinc iodide, sodium vanadate, ammonium vanadate, bimetallic sulfide or nitrogen-oxygen-containing organic matter.
[0060] Optionally, the diaphragm of the aqueous zinc ion battery is selected from a glass fiber diaphragm, a cellulose diaphragm, a filter paper or a pp diaphragm. The diaphragm is used to separate the anode and cathode materials, and can remain stable during the battery charge and discharge process, and has electronic insulation and high ion conductivity.
[0061] In one embodiment, a zinc ion soft pack battery is provided, comprising an aluminum-plastic film, a negative electrode current collector, a zinc negative electrode, a positive electrode, a positive electrode current collector, a separator, and an electrolyte containing any one of the above additives for aqueous zinc ion batteries.
[0062] Optionally, the negative electrode current collector includes but is not limited to titanium foil, carbon fiber cloth, graphite paper, and tinned copper foil.
[0063] Optionally, the zinc negative electrode is selected from zinc sheet, zinc powder, zinc foam or zinc mesh.
[0064] Optionally, the separator includes a glass fiber separator, a cellulose separator or a hydrophilic polypropylene separator.
[0065] Optionally, the amount of the electrolyte is 50 to 200 μL / cm 2 .
[0066] Optionally, the positive electrode of the zinc ion battery includes at least one of manganese dioxide, vanadium pentoxide, and iodine.
[0067] Optionally, the positive electrode current collector includes at least one of a titanium mesh, a carbon fiber cloth, and a tin-plated copper mesh.
[0068] In one embodiment, an assembled button battery is provided, comprising a positive electrode shell, a gasket, a zinc sheet / positive electrode sheet, a separator, an electrolyte, a zinc sheet, a gasket, a spring, a negative electrode shell, and any one of the above electrolytes containing an additive for aqueous zinc ion batteries.
[0069] Example 1
[0070] The preparation of an electrolyte containing an organic substance containing phosphorus and oxygen functional groups as an additive comprises the following steps:
[0071] In 10 ml of deionized water, add 0.1 to 0.4 mmol·L -1 [[(Phosphorylmethyl)imino]bis[(2,1-ethylenenitrobis(methylene)]]tetraphosphonate heptasodium (DTP, organic compound containing phosphorus and oxygen functional groups) was stirred at 40°C for 5 hours, then ultrasonicated for 1 hour, and then 2 mol·L -1 Zinc sulfate, the stirrer continues stirring at 30°C for 4 hours to obtain a uniform aqueous electrolyte containing organic matter with phosphorus and oxygen functional groups as additives.
[0072] The aqueous electrolyte containing the organic matter containing phosphorus oxygen functional group as additive and 2 mol L -1 The infrared peak of zinc sulfate is Figure 2 As shown in the figure, after adding the additive, the -1The OH bonds attributable to water were weakened and slightly shifted, indicating that the addition of additives weakened the effect of the hydrogen bond network.
[0073] Testing of zinc deposition behavior:
[0074] Then the electrolyte prepared in Example 1 was transferred to a 25 mL three-electrode reaction cell. Zinc sheets cut to a size of 1 cm*1 cm were used as the working electrode and the counter electrode, and AgCl was used as the reference electrode to form a three-electrode system. The three-electrode system was measured at 1 mA cm using an electrochemical workstation. -2 The zinc sheets were electro-deposited at a current density of . The deposited zinc sheets were washed with deionized water and their deposition morphology was characterized by scanning electrochemical microscopy. Figure 3 As shown, at 1 mA·cm -2 The deposition current density was 1 mAh·cm -2 After adding zinc, the zinc deposited on the surface of the experimental group was flat and dense, while the zinc deposited on the control group was leaf-shaped dendrites. This shows that the problem of easy dendrite growth of zinc negative electrode has been significantly improved.
[0075] Example 2
[0076] The preparation of an electrolyte containing an organic substance containing phosphorus and oxygen functional groups as an additive comprises the following steps:
[0077] The difference from Example 1 is that in step (1), only one organic additive containing phosphorus and oxygen functional groups is selected, while in Example 2, 0.01 mmol·L -1 [[(Phosphorylmethyl)imino]bis[(2,1-ethylenenitrobis(methylene)]]tetraphosphonate heptasodium (DTP) and 0.1mmol·L -1 [[(Phosphorylmethyl)imino]bis[(2,1-ethylenenitrobis(methylene)]]tetraphosphonic acid was stirred at 40°C for 5 hours, then ultrasonicated for 1 hour, and then 2 mol·L -1 Zinc sulfate, the stirrer continues stirring at 30°C for 4 hours to obtain a uniform aqueous electrolyte containing organic matter with phosphorus and oxygen functional groups as additives.
[0078] Example 3
[0079] Application of an electrolyte composed of an organic substance containing phosphorus and oxygen functional groups as an additive in a secondary aqueous zinc ion battery and its performance test:
[0080] (1) Assembled batteries: The first type of battery is a zinc-zinc symmetrical battery, in which both the anode and cathode are made of zinc sheets. The second type of battery is a zinc-zinc iodide full battery, in which the anode is made of zinc sheets and the cathode is made of highly stable zinc iodide. Both types of battery separators are made of glass fiber, and the electrolyte is made of the zinc ion concentration of 2 mol·L prepared by the present invention in Example 1. -1The electrolyte containing [[(phosphorylmethyl)imino]bis[(2,1-ethylenenitrobis(methylene)]]tetraphosphonate heptasodium is assembled into a CR2032 button battery. The structure of the assembled button battery is: positive electrode shell, gasket, zinc sheet / positive electrode sheet, electrolyte, diaphragm, electrolyte, zinc sheet, gasket, shrapnel and negative electrode shell.
[0081] (2) Assembling soft-pack batteries: The materials required for assembling zinc-ion soft-pack batteries include aluminum-plastic film, negative electrode current collector, zinc negative electrode, prepared positive electrode, positive electrode current collector, separator and the electrolyte. First, stack the negative electrode current collector-zinc negative electrode-separator-positive electrode sheet-positive electrode current collector flatly, then put them into an aluminum-plastic film bag and inject an appropriate amount of electrolyte, and finally use a sealing machine to complete the battery packaging.
[0082] (3) Electrochemical test: The assembled button cell was subjected to charge and discharge tests on a Sunway battery test system at room temperature. The test conditions for the zinc-zinc symmetrical cell were a current density of 5 mA cm -2 , the deposition capacity is 2 mAh·cm -2 , its cycle performance diagram is as follows Figure 4 The test conditions of the zinc-iodine button battery are as follows: the charge and discharge voltage range is 0.3 to 1.8 V, and the -1 The charge and discharge test was carried out at a current density of , and the cycle-capacity diagram is shown in Figure 5 As shown in the figure, it can stably cycle more than 1600 times under this condition. The test conditions of the zinc-iodine soft-pack full battery are: the charge and discharge voltage range is 0.3~1.8V, and the charge and discharge voltage is 12.5mA·cm -2 The charge and discharge test was carried out at a current density of , and the cycle-capacity diagram is shown in Figure 6 As shown, it can stably cycle more than 800 times under this condition.
[0083] (4) The zinc-zinc symmetrical button cells of Example 3 were subjected to Tafel test using an electrochemical workstation. Figure 7 As shown in the figure, the corrosion current of the experimental group increased from 10.2 mA cm -2 Reduced to 7.12 mA cm -2 This shows that the electrolyte in the experimental group can effectively inhibit the occurrence of corrosion side reactions.
Claims
1. An additive for aqueous zinc ion batteries, characterized in that Including organic salts containing phosphorus and oxygen functional groups, the negative electrode material of the aqueous zinc ion battery is zinc.
2. The additive for aqueous zinc ion batteries according to claim 1, characterized in that Also included are zinc salts.
3. The additive for aqueous zinc ion batteries according to claim 2, characterized in that: The organic salt containing a phosphorus oxygen functional group is selected from one or more of [[(phosphorylmethyl)imino]bis[(2,1-ethylenediaminebis(methylene)]]tetraphosphonic acid, [[(phosphorylmethyl)imino]bis[(2,1-ethylenediaminebis(methylene)]]tetraphosphonic acid heptasodium and [[(phosphorylmethyl)imino]bis[(2,1-ethylenediaminebis(methylene)]]tetraphosphonic acid tetrasodium; The zinc salt is selected from one or more of zinc sulfate, zinc methanesulfonate, zinc trifluoromethanesulfonate, zinc bis(trifluoromethanesulfonate imide), zinc chloride, zinc hexafluorosilicate, zinc perchlorate and zinc nitrate; The negative electrode material of the aqueous zinc ion battery is zinc sheet, zinc powder or zinc mesh.
4. An electrolyte containing an additive for an aqueous zinc ion battery, characterized in that: The invention comprises the additive for aqueous zinc ion battery as claimed in any one of claims 1 to 3.
5. The electrolyte containing the additive for aqueous zinc ion battery according to claim 4, characterized in that: The concentration of the organic salt containing phosphorus oxygen functional groups is 0.001 to 1 mmol / L; The concentration of the zinc salt is 0.5-3 mol / L.
6. A method for preparing an electrolyte containing an additive for an aqueous zinc ion battery as claimed in claim 4, characterized in that: The following steps are involved: The organic salt containing phosphorus oxygen functional groups is added to deionized water, stirred at 25-50° C. for 2-5 hours, and then ultrasonicated, and then the zinc salt is added, stirred at 25-60° C. to obtain the electrolyte containing the additive for aqueous zinc ion batteries.
7. The method for preparing an electrolyte containing an additive for an aqueous zinc ion battery according to claim 6, wherein: Ultrasound 1 hour duration; Stirring time: 4 hours; The deionized water is ultrapure water with a resistivity of 18 MΩ*cm.
8. An aqueous zinc ion battery, characterized in that: An electrolyte comprising a zinc negative electrode and an additive for an aqueous zinc ion battery as described in any one of claims 4 to 5.
9. The aqueous zinc ion battery according to claim 8, characterized in that The positive electrode material of the aqueous zinc ion battery is manganese dioxide, vanadium pentoxide, zinc iodide, sodium vanadate, ammonium vanadate, bimetallic sulfide or nitrogen-oxygen-containing organic matter; The separator is selected from glass fiber separator, cellulose separator, filter paper or PP separator.
10. The aqueous zinc ion battery according to claim 9, characterized in that: The aqueous zinc ion battery is a zinc ion soft pack battery, comprising an aluminum plastic film, a negative electrode current collector, a zinc negative electrode, a positive electrode, a positive electrode current collector, a separator and an electrolyte containing an additive for an aqueous zinc ion battery as claimed in any one of claims 4 to 5, wherein the negative electrode current collector comprises but is not limited to titanium foil, carbon fiber cloth, graphite paper, tinned copper foil, the zinc negative electrode is selected from zinc sheet, zinc powder, foamed zinc or zinc mesh, the separator comprises a glass fiber separator, a cellulose separator or a hydrophilic polypropylene separator, and the amount of the electrolyte is 50 to 200 μL / cm 2 , the positive electrode of the zinc ion battery includes at least one of manganese dioxide, vanadium pentoxide, and iodine, and the positive electrode current collector includes at least one of a titanium mesh, a carbon fiber cloth, and a tinned copper mesh; The aqueous zinc ion battery is an assembled button battery, comprising a positive electrode shell, a gasket, a zinc sheet / positive electrode sheet, a diaphragm, a zinc sheet, a gasket, a spring, a negative electrode shell and an electrolyte containing an additive for aqueous zinc ion batteries as described in any one of claims 4-5.
Citation Information
Cited By
Interlayer-surface dual-modified layered manganese dioxide positive electrode active material, preparation thereof and application of interlayer-surface dual-modified layered manganese dioxide positive electrode active material in aqueous zinc secondary battery
CN120081423A
Interlayer-Surface Dual-Modified Layered Manganese Dioxide Cathode Active Material, Its Preparation and Application in Aqueous Zinc Secondary Batteries
CN120081423B
Preparation method of modified zinc negative electrode, modified zinc negative electrode and aqueous zinc ion battery