Preparation method of composite ceramic coating slurry for diaphragm and ceramic coating slurry
By modifying the non-covalent interaction between the ceramic powder and the binder and optimizing the particle grading of the ceramic raw materials, the problem of low stability of the composite ceramic coating slurry is solved, and high bonding and low thermal conductivity are achieved. Ceramic slurry preparation improves the thermal stability and wettability of the diaphragm, simplifies the preparation process and reduces costs.
Patent Information
- Application Number
- CN202410701352.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-11-22
AI Technical Summary
The existing composite ceramic coating slurry has low stability and complex preparation process. The organic solvents used are high cost and are not environmentally friendly. The ceramic raw materials have high thermal conductivity but poor thermal insulation performance, which leads to the membrane being easily shrinking and deforming at high temperatures. Increase the risk of battery short circuit.
Ceramic powder is prepared by aluminum and silicon sources, ceramic powder is modified by silanization reagent, and non-covalent interaction with the binder to form a composite ceramic coating slurry with high bonding and low thermal conductivity. Use kaolin, alumina powder and white corundum powder as ceramic raw materials to optimize particle grading and mixing to improve wetting and thermal stability.
Improve the adhesion and density of ceramic slurry, enhance the thermal stability and wettability of the diaphragm, reduce the risk of high-temperature shrinkage and deformation, reduce the possibility of battery short circuit, and simplify the preparation process and reduce the cost. Environmentally friendly mineral raw materials.
Smart Images

Figure CN119009361A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of preparation of composite ceramic coating slurries, and in particular to a preparation method of composite ceramic coating slurries for battery separators and ceramic coating slurries. Background Art
[0002] In lithium-ion batteries, the separator acts as an electronic insulator between the positive and negative electrodes, while also ensuring the free movement of ions. However, simple PP or PE separators have poor high-temperature thermal stability and are prone to shrinkage and deformation at high temperatures, leading to internal battery short circuits and explosions. Therefore, a ceramic coating is applied to the separator to improve its thermal stability. The ceramic coating prevents short circuits at high temperatures, while also providing excellent water absorption, which improves the separator's wettability and fluid absorption and retention capabilities.
[0003] Existing ceramic slurry preparation processes are complex, and most additives are organic solvents, resulting in high costs and environmental concerns. Furthermore, the ceramic raw materials themselves have high thermal conductivity and poor thermal insulation properties. Diaphragms coated with ordinary ceramic binder slurries will noticeably shrink and deform at temperatures as low as 150°C. By replacing these common ceramic raw materials with a ceramic raw material that offers low thermal conductivity, excellent thermal stability, and a simpler preparation method, the thermal stability of the diaphragm can be improved. Summary of the Invention
[0004] The main purpose of the present invention is to provide a preparation method of a composite ceramic coating slurry for a battery separator and a ceramic coating slurry, so as to solve the problem of low stability of the composite ceramic coating slurry in the prior art.
[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for preparing a composite ceramic coating slurry for a battery separator is provided, comprising: preparing a ceramic powder by using an aluminum source and a silicon source; adding the ceramic powder to a silanization agent and stirring to obtain a ceramic powder slurry; washing, centrifuging and drying the ceramic powder slurry to obtain a modified ceramic powder; adding a binder and the modified ceramic powder to a solvent, stirring and filtering to obtain a composite ceramic coating slurry.
[0006] Furthermore, the ceramic powder is prepared by using the aluminum source and the silicon source, including: mixing kaolin, aluminum oxide powder, and white corundum powder and stirring to obtain the ceramic powder.
[0007] Furthermore, in the step of mixing kaolin, alumina powder and white corundum powder and then stirring, the alumina powder is obtained by mixing at least a first alumina powder and a second alumina powder, and the particle diameter of the first alumina powder is larger than the particle diameter of the second alumina powder.
[0008] Furthermore, in the step of mixing kaolin, alumina powder and white corundum powder and then stirring them, the mass fraction of the first alumina powder in the ceramic powder is 26%-28%, the mass fraction of the second alumina powder in the ceramic powder is 20%-22%, the mass fraction of the second alumina powder in the ceramic powder is 49%-51%, and the mass fraction of kaolin in the ceramic powder is 1%-2%.
[0009] Furthermore, the silanization agent is prepared from 3-aminopropyl-trimethoxysilane and ethanol solution, and the weight percentage of 3-aminopropyl-trimethoxysilane in the silanization agent is 70%-80%.
[0010] Furthermore, in the step of adding the ceramic powder to the silanization agent and stirring to obtain a ceramic powder slurry, the stirring method is to use a high-speed stirrer with a stirring speed of 1500 r / min and stir at room temperature for 2.5 hours.
[0011] Furthermore, adding a binder and modified ceramic powder to a solvent, stirring and filtering to obtain a composite ceramic coating slurry includes: adding a thickener, a binder and modified ceramic powder to a solvent, stirring and filtering to obtain a composite ceramic coating slurry.
[0012] Furthermore, the thickener is sodium carboxymethyl cellulose, and / or the binder is polymethacrylic acid, and / or the solvent is deionized water.
[0013] Furthermore, in the step of adding a binder and modified ceramic powder to a solvent, stirring and filtering to obtain a composite ceramic coating slurry, the stirring method is to use a magnetic stirrer, the stirring temperature is 60° C., and the stirring time is 2.5 h.
[0014] According to one aspect of the present invention, a ceramic coating slurry is provided. The ceramic coating slurry is prepared using the above-mentioned method for preparing the composite ceramic coating slurry for battery separators.
[0015] The technical solution of the present invention is applied, by adding ceramic powder to a silanization agent, stirring to obtain a ceramic powder slurry, and then making a modified ceramic powder, and adding a binder and modified ceramic powder to a solvent, stirring and filtering to obtain a composite ceramic coating slurry. Due to the use of silanization-modified ceramic powder, the obtained ceramic powder can produce non-covalent interactions with the binder, thereby improving its adhesion, so that the ceramic slurry has high adhesion, strong density, better coating effect and better stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The accompanying drawings, which constitute part of this application, are intended to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are intended to explain the present invention and do not constitute an undue limitation of the present invention. In the accompanying drawings:
[0017] Figure 1 A schematic flow chart of an embodiment of a method for preparing a composite ceramic coating slurry for a battery separator according to the present invention is shown;
[0018] Figure 2 shows an XRD pattern of an example of calcined kaolin according to the present invention;
[0019] Figure 3 A contact angle diagram of an embodiment of a ceramic slurry according to the present invention is shown. DETAILED DESCRIPTION
[0020] It should be noted that, in the absence of conflict, the embodiments and features of the embodiments in this application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0021] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, they indicate the presence of features, steps, operations, devices, components and / or combinations thereof.
[0022] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way are interchangeable where appropriate, so that the embodiments of the present application described herein can, for example, be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0023] Now, exemplary embodiments according to the present application will be described in more detail with reference to the accompanying drawings. However, these exemplary embodiments can be implemented in a variety of different forms and should not be interpreted as being limited to the embodiments described herein. It should be understood that these embodiments are provided to make the disclosure of this application thorough and complete, and to fully convey the concepts of these exemplary embodiments to those of ordinary skill in the art. In the accompanying drawings, for the sake of clarity, the thickness of layers and regions may be exaggerated, and the same reference numerals are used to represent the same devices, and thus their descriptions will be omitted.
[0024] Combine Figures 1 to 3 As shown, according to a specific embodiment of the present application, a method for preparing a composite ceramic coating slurry for a battery separator is provided, comprising: preparing a ceramic powder from an aluminum source and a silicon source; adding the ceramic powder to a silanization agent, and stirring to obtain a ceramic powder slurry; washing, centrifuging and drying the ceramic powder slurry to obtain a modified ceramic powder; adding a binder and the modified ceramic powder to a solvent, stirring and filtering to obtain a composite ceramic coating slurry.
[0025] The technical solution of the present invention is applied, by adding ceramic powder to a silanization agent, stirring to obtain a ceramic powder slurry, and then making a modified ceramic powder, and adding a binder and modified ceramic powder to a solvent, stirring and filtering to obtain a composite ceramic coating slurry. Due to the use of silanization-modified ceramic powder, the obtained ceramic powder can produce non-covalent interactions with the binder, thereby improving its adhesion, so that the ceramic slurry has high adhesion, strong density, better coating effect and better stability.
[0026] Ceramic powder is prepared from aluminum source and silicon source, including: 1. Selection and pretreatment of raw materials; Aluminum source: Commonly used aluminum sources include alumina (Al2O3), aluminates, aluminum powder, etc. Silicon source: Commonly used silicon sources include silicon dioxide (SiO2), silicates, silicon powder, etc. During the preparation process, the raw materials must first be properly pretreated, such as drying, grinding, screening, etc., to obtain a particle size and purity suitable for the synthesis reaction. 2. Mix evenly; Mix the pretreated aluminum source and silicon source evenly in a certain molar ratio. This step is usually carried out in a ball mill to ensure that the two powders are fully mixed. Sometimes it may be necessary to add appropriate organic solvents or surfactants to improve the mixing effect.
[0027] Silanization is the process of chemically treating or modifying the surface of a target substance using a silanizing agent (a class of chemicals containing silicon). The silanization process primarily involves the silanizing agent reacting with hydroxyl groups (-OH) or other reactive groups on the surface of the substance, forming a stable chemical bond.
[0028] Due to the use of silanized modified ceramic powder, the obtained ceramic powder can produce non-covalent interaction with the binder, thereby improving its adhesion, making the ceramic slurry highly adhesive, dense, and having a better coating effect.
[0029] The composite ceramic slurry has been modified to have better adhesion, which allows it to better combine with the diaphragm, thereby improving the wettability and thermal stability of the diaphragm, making it less likely to shrink and deform at high temperatures, and reducing the risk of internal short circuit in the battery.
[0030] Furthermore, the ceramic powder is prepared by using the aluminum source and the silicon source, including: mixing kaolin, aluminum oxide powder, and white corundum powder and stirring to obtain the ceramic powder.
[0031] Figure 2 The XRD pattern of an embodiment of calcined kaolin according to the present invention is shown. Kaolin is an important clay mineral, the main component of which is aluminum hydroxide silicate. It belongs to a type of mica structure with a layered structure and is a high-quality white or nearly white clay. Kaolin not only has good hiding power, oil absorption and good acid and alkali resistance, but also has high insulation and heat resistance. Alumina powder is a fine powder composed of aluminum oxide particles, which has the characteristics of high hardness, high melting point, good electrical insulation, thermal stability and corrosion resistance. White corundum powder is smelted from high-quality aluminum oxide raw materials by electric fusion.
[0032] White corundum and calcined kaolin are selected as ceramic raw materials. White corundum is primarily composed of α-Al2O3, while kaolin is a non-polluting, environmentally friendly mineral raw material whose main components after calcination are Al2O3 and SiO2. The combination of these two materials results in a ceramic slurry with lower thermal conductivity. The two-dimensional layered kaolin has excellent adsorption properties, which increases the water absorption of the ceramic slurry and improves the wettability of the separator.
[0033] By adopting the technical solution of the present application, a ceramic raw material with low thermal conductivity, good thermal stability and simple preparation method is provided to replace ordinary ceramic raw materials, thereby improving the thermal stability of the diaphragm.
[0034] Furthermore, in the step of mixing kaolin, alumina powder and white corundum powder and then stirring, the alumina powder is obtained by mixing at least a first alumina powder and a second alumina powder, and the particle diameter of the first alumina powder is larger than the particle diameter of the second alumina powder.
[0035] Selecting raw materials with different particle gradations makes the ceramic particles in the slurry more densely packed, and small particles can be filled between the gaps of large particles, making the slurry denser.
[0036] Furthermore, in the step of mixing kaolin, alumina powder and white corundum powder and then stirring them, the mass fraction of the first alumina powder in the ceramic powder is 26%-28%, the mass fraction of the second alumina powder in the ceramic powder is 20%-22%, the mass fraction of the second alumina powder in the ceramic powder is 49%-51%, and the mass fraction of kaolin in the ceramic powder is 1%-2%.
[0037] The technical solution of this application uses white corundum and green mineral kaolin as ceramic raw materials. The two-dimensional layered structure of calcined kaolin gives it good adsorption properties. It also has a certain degree of adhesiveness. The internal SiO2 and silane coupling agent are more tightly bonded, improving its silanization performance. The ceramic powder is modified using a silane solvent to improve its adhesion to the binder, resulting in a ceramic slurry with low thermal conductivity, high adhesion, high density, and good wettability. The high adhesion slurry allows it to bond more tightly to the diaphragm, thereby improving the thermal stability of the diaphragm and reducing the risk of high-temperature shrinkage and deformation of the diaphragm and battery short circuit.
[0038] In an optional embodiment, the preparation method is as follows:
[0039] Step S1, mixing ceramic powders: Al2O3 micropowders (450 mesh, 380 mesh), white corundum micropowder, and calcined kaolin of different particle sizes were weighed in a mass ratio of 27.02%: 21.04%: 50.08%: 1.86%, respectively, and placed in a stirring cup. Dry stirring was performed for 30 minutes to ensure uniform mixing of the powders.
[0040] Step S2, silanization of ceramic particles: Prepare in advance a 1 mol / L 75 wt% ethanol aqueous solution of 3-aminopropyl-trimethoxysilane, add the powder from step 1 to the solution, and use a high-speed stirrer at 1500 rpm at room temperature for 2.5 hours to obtain a uniformly dispersed ceramic powder;
[0041] Step S3: The slurry obtained in step 2 is rinsed with deionized water, centrifuged, and the supernatant is discarded until the aqueous solution is neutral. The solid matter is placed in an oven and dried at 80° C. for 8 hours to obtain a modified ceramic powder;
[0042] Step S4, ceramic slurry preparation: Place the modified ceramic powder obtained in step 3 in a stirring cup, add 50 wt% of deionized water by mass fraction of the ceramic powder, and similarly add 0.4 wt% of thickener sodium carboxymethyl cellulose (CMC-Na) and 5 wt% of binder polymethacrylic acid. Use a magnetic stirrer, heat to 60°C, and stir for 2 hours; stir and disperse the evenly dispersed ceramic slurry through a 200-mesh sieve to obtain a evenly dispersed ceramic slurry.
[0043] Furthermore, the silanization agent is prepared from 3-aminopropyl-trimethoxysilane and ethanol solution, and the weight percentage of 3-aminopropyl-trimethoxysilane in the silanization agent is 70%-80%.
[0044] Furthermore, in the step of adding the ceramic powder to the silanization agent and stirring to obtain a ceramic powder slurry, the stirring method is to use a high-speed stirrer with a stirring speed of 1500 r / min and stir at room temperature for 2.5 hours.
[0045] Furthermore, adding a binder and modified ceramic powder to a solvent, stirring and filtering to obtain a composite ceramic coating slurry includes: adding a thickener, a binder and modified ceramic powder to a solvent, stirring and filtering to obtain a composite ceramic coating slurry.
[0046] In an optional embodiment, the particle size of the ceramic raw powder, the type of binder, the different types of aluminum-silicon raw materials, and the stirring and dispersing time can be selected according to the actual project conditions.
[0047] Furthermore, the thickener is sodium carboxymethyl cellulose, and / or the binder is polymethacrylic acid, and / or the solvent is deionized water.
[0048] Sodium carboxymethyl cellulose is a water-soluble polymer that effectively increases the viscosity of a mixture, thereby improving the stability and anti-precipitation ability of the product. Sodium carboxymethyl cellulose has good solubility in water and is compatible with a variety of ingredients, facilitating the formation of a uniform mixture.
[0049] Polymethacrylic acid, as a binder, can improve the mechanical strength and durability of the material, making the product stronger and more durable.
[0050] Deionized water does not contain ions that may interfere with product performance, helping to improve product purity and stability.
[0051] Furthermore, in the step of adding a binder and modified ceramic powder to a solvent, stirring and filtering to obtain a composite ceramic coating slurry, the stirring method is to use a magnetic stirrer, the stirring temperature is 60° C., and the stirring time is 2.5 h.
[0052] According to one aspect of the present invention, a ceramic coating slurry is provided. The ceramic coating slurry is prepared using the above-mentioned method for preparing the composite ceramic coating slurry for battery separators.
[0053] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0054] 1. Provide a low-cost Al2O3 / SiO2 composite ceramic slurry for battery coating diaphragm;
[0055] 2. Provide a silanized ceramic powder so that it can produce non-covalent interaction with the binder, thereby improving the adhesion of the slurry and obtaining a highly adhesive ceramic slurry.
[0056] 3. The use of high temperature resistant binder improves the thermal stability of the slurry, thereby improving the heat resistance of the diaphragm.
[0057] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used herein to describe the spatial positional relationship of a device or feature to other devices or features as shown in the figures. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figures. For example, if the device in the drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.
[0058] In addition to the above, it should be noted that references to "one embodiment," "another embodiment," "an embodiment," and the like in this specification refer to specific features, structures, or characteristics described in conjunction with that embodiment as included in at least one embodiment generally described in this application. The appearance of the same expression in multiple places in the specification does not necessarily refer to the same embodiment. Furthermore, when a specific feature, structure, or characteristic is described in conjunction with any embodiment, it is intended that such feature, structure, or characteristic, when implemented in conjunction with other embodiments, also falls within the scope of the present invention.
[0059] In the above embodiments, the description of each embodiment has its own focus. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0060] The foregoing description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art will readily appreciate that various modifications and variations of the present invention are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.
Claims
1. A method for preparing a composite ceramic coating slurry for a battery separator, It is characterized in that include: Ceramic powder is prepared by using aluminum source and silicon source; Adding the ceramic powder into a silanization agent and stirring to obtain a ceramic powder slurry; The ceramic powder slurry is washed, centrifuged and dried to obtain modified ceramic powder; Add the binder and the modified ceramic powder into the solvent, stir and filter to obtain the composite ceramic coating slurry.
2. The method for preparing the composite ceramic coating slurry for battery separator according to claim 1, It is characterized in that The ceramic powder prepared by using aluminum source and silicon source includes: The ceramic powder is obtained by mixing kaolin, alumina micropowder and white corundum micropowder and stirring.
3. The method for preparing the composite ceramic coating slurry for battery separator according to claim 2, It is characterized in that In the step of mixing kaolin, alumina powder and white corundum powder and then stirring, the alumina powder is obtained by mixing at least a first alumina powder and a second alumina powder, and the particle diameter of the first alumina powder is larger than the particle diameter of the second alumina powder.
4. The method for preparing the composite ceramic coating slurry for battery separator according to claim 3, It is characterized in that In the step of mixing kaolin, alumina powder and white corundum powder and then stirring, the mass fraction of the first alumina powder in the ceramic powder is 26%-28%, the mass fraction of the second alumina powder in the ceramic powder is 20%-22%, the mass fraction of the second alumina powder in the ceramic powder is 49%-51%, and the mass fraction of the kaolin in the ceramic powder is 1%-2%.
5. The method for preparing the composite ceramic coating slurry for battery separator according to claim 1, It is characterized in that The silanization agent is prepared from 3-aminopropyl-trimethoxysilane and ethanol solution, and the weight percentage of the 3-aminopropyl-trimethoxysilane in the silanization agent is 70%-80%.
6. The method for preparing the composite ceramic coating slurry for battery separator according to claim 1, It is characterized in that In the step of adding the ceramic powder to the silanization agent and stirring to obtain a ceramic powder slurry, the stirring method is to use a high-speed stirrer with a stirring speed of 1500 r / min and stir at room temperature for 2.5 hours.
7. The method for preparing the composite ceramic coating slurry for battery separator according to claim 1, It is characterized in that Adding a binder and the modified ceramic powder to a solvent, stirring and filtering to obtain a composite ceramic coating slurry comprising: The thickener, the binder and the modified ceramic powder are added to the solvent, stirred and filtered to obtain the composite ceramic coating slurry.
8. The method for preparing the composite ceramic coating slurry for battery separator according to claim 7, It is characterized in that The thickener is sodium carboxymethyl cellulose, and / or the binder is polymethacrylic acid, and / or the solvent is deionized water.
9. The method for preparing the composite ceramic coating slurry for battery separator according to claim 1, It is characterized in that In the step of adding the binder and the modified ceramic powder to the solvent, stirring and filtering to obtain the composite ceramic coating slurry, the stirring method is to use a magnetic stirrer, the stirring temperature is 60° C., and the stirring time is 2.5 hours.
10. A ceramic coating slurry, It is characterized in that The ceramic coating slurry is prepared by the preparation method of the composite ceramic coating slurry for battery separator according to any one of claims 1 to 9.