Polishing pad and method for manufacturing polishing product
By adjusting the dynamic viscoelastic characteristics of the end point detection window of the abrasive pad and the abrasive layer, the problem of surface defects during the abrasive process is solved, and the surface quality of the abrasive object and the accuracy of the abrasive end point detection are improved.
Patent Information
- Application Number
- CN202380028544.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-22
AI Technical Summary
During the chemical mechanical grinding process, the difference in the dynamic viscoelastic characteristics of the end point detection window of the existing abrasive pad and the abrasive layer leads to surface defects, affecting the accuracy of the grinding end point detection and the surface quality of the abrasive object.
By adjusting the dynamic viscoelastic characteristics of the end point detection window and the grinding layer, the difference in energy storage modulus ratio and loss factor in the stretching mode, frequency 1.6Hz, 30-55°C and immersion state is within a specific range, ensuring that the two The dynamic viscoelastic properties of the user are close, thereby inhibiting the occurrence of surface defects.
With the end point detection window, it is realized that the grinding object that is not prone to defects and has excellent surface quality is obtained, and the accuracy and surface quality of the grinding end point detection are improved.
Smart Images

Figure CN119013122A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polishing pad and a method for producing a polished product using the polishing pad. Background Art
[0002] In the semiconductor manufacturing process, chemical mechanical polishing (CMP) is used in the flattening of the insulating film after film formation and the formation of metal wiring. As one of the important technologies required for chemical mechanical polishing, there is a polishing endpoint detection to detect whether the polishing process is completed. For example, over-polishing or under-polishing relative to the target polishing endpoint directly leads to defective products. Therefore, in chemical mechanical polishing, it is necessary to strictly manage the polishing amount through polishing endpoint detection.
[0003] Chemical mechanical polishing is a complex process. The polishing speed (polishing rate) varies due to the operating state of the polishing device, the quality of consumables (slurry, polishing pad, dresser, etc.), and the deviation of the state over time during the polishing process. In addition, the accuracy of the residual film thickness and the uniformity within the surface required in the semiconductor manufacturing process have become increasingly stringent in recent years. Due to this situation, it has become more difficult to detect the polishing endpoint with sufficient accuracy.
[0004] As the main methods for detecting the grinding endpoint, there are known optical endpoint detection methods, torque endpoint detection methods, eddy current endpoint detection methods, etc. In the optical endpoint detection method, light is irradiated to the chip through a transparent window component set on the grinding pad, and the endpoint detection is performed by monitoring the reflected light.
[0005] As a polishing pad using such an optical endpoint detection method, for example, Patent Document 1 discloses a polishing pad for the purpose of providing a polishing pad capable of suppressing slurry from being retained in the grooves of a window component and improving the detection accuracy of a polishing rate, wherein, in a polishing pad having a pad main body and a transparent window component integrally formed with a portion of the pad main body, a material having a higher abrasiveness than the material of the pad main body is used for the surface of the window component.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2002-001647 Summary of the invention
[0009] Problems to be solved by the invention
[0010] However, if the characteristics of the grinding layer and the end point detection window are different as in Patent Document 1, for example, the end point detection window is ground faster than the grinding layer and becomes concave, and slurry and grinding debris are easily accumulated there, sometimes resulting in defects (surface defects). In addition, if the end point detection window is ground slower than the grinding layer, as the grinding proceeds, the end point detection window becomes a convex portion, resulting in defects, which may reduce the surface quality of the object being ground.
[0011] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a polishing pad having an end point detection window, which can produce an object to be polished that is less likely to have defects and has excellent surface quality, and a method for manufacturing a polished product using the same.
[0012] Means for solving problems
[0013] The inventors of the present application have conducted intensive studies to solve the above-mentioned problems and have found that the above-mentioned problems can be solved by setting a predetermined relationship between the viscoelasticity of the endpoint detection window and the polishing layer, thereby completing the present invention.
[0014] That is, the present invention is as follows.
[0015] [1]
[0016] A polishing pad having a polishing layer and an endpoint detection window provided at an opening of the polishing layer.
[0017] In the dynamic viscoelasticity measurement conducted in a tensile mode at a frequency of 1.6 Hz, 30 to 55° C., and in a water-immersed state, the ratio of the storage modulus E'w40 of the endpoint detection window at 40° C. to the storage modulus E'p40 of the polishing layer at 40° C. (E'p40 / E'w40) is 0.70 to 3.00.
[0018] [2]
[0019] The polishing pad as described in [1], wherein in the dynamic viscoelasticity measurement, the ratio of the storage modulus E'w50 of the endpoint detection window at 50°C to the storage modulus E'p50 of the polishing layer at 50°C (E'p50 / E'w50) is 0.70 to 5.00.
[0020] 〔3〕
[0021] A polishing pad as described in [1] or [2], wherein in the aforementioned dynamic viscoelasticity measurement, the difference between the loss factor tanδw30 of the aforementioned endpoint detection window at 30°C and the loss factor tanδp30 of the aforementioned polishing layer at 30°C (|tanδw30-tanδp30|) is 0.05 to 0.30.
[0022] [4]
[0023] A polishing pad as described in any one of [1] to [3], wherein in the aforementioned dynamic viscoelasticity measurement, the difference between the loss factor tanδw40 of the aforementioned endpoint detection window at 40°C and the loss factor tanδp40 of the aforementioned polishing layer at 40°C (|tanδw40-tanδp40|) is 0.05 to 0.40.
[0024] 〔5〕
[0025] A polishing pad as described in any one of [1] to [4], wherein in the aforementioned dynamic viscoelasticity measurement, the difference between the loss factor tanδw50 of the aforementioned endpoint detection window at 50°C and the loss factor tanδp50 of the aforementioned polishing layer at 50°C (|tanδw50-tanδp50|) is 0.05 to 0.50.
[0026] [6]
[0027] The polishing pad as described in any one of [1] to [5], wherein the endpoint detection window comprises a polyurethane resin WI,
[0028] The polyurethane resin WI includes a structural unit derived from an aliphatic isocyanate.
[0029] 〔7〕
[0030] The polishing pad as described in any one of [1] to [6], wherein the polishing layer comprises a polyurethane resin P,
[0031] The polyurethane resin P contains a structural unit derived from an aromatic isocyanate.
[0032] 〔8〕
[0033] The polishing pad according to any one of [1] to [7], wherein the polishing layer includes hollow fine particles dispersed in the polishing layer.
[0034] 〔9〕
[0035] A method for producing a polished product, comprising:
[0036] a polishing step of polishing an object to be polished using the polishing pad described in any one of [1] to [8] in the presence of a polishing slurry to obtain a polished object; and
[0037] In the end point detection step, an optical end point detection method is used to detect the end point during the polishing process.
[0038] Effects of the Invention
[0039] According to the present invention, it is possible to provide a polishing pad having an endpoint detection window, which can produce an object to be polished that is less likely to have defects and has excellent surface quality, and a method for producing a polished product using the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] [ Figure 1 ] is a schematic three-dimensional diagram of the polishing pad of this embodiment.
[0041] [ Figure 2 ] is a schematic cross-sectional view of the endpoint detection window portion of the polishing pad of the present embodiment.
[0042] [ Figure 3 ] is a schematic cross-sectional view of another embodiment of the endpoint detection window portion of the polishing pad of the present embodiment.
[0043] [ Figure 4 ] is a schematic diagram showing a film thickness control system mounted on CMP. DETAILED DESCRIPTION
[0044] Hereinafter, an embodiment of the present invention (hereinafter referred to as "the present embodiment") will be described in detail with reference to the accompanying drawings as needed, but the present invention is not limited thereto and can be variously modified without departing from the main purpose thereof. It should be noted that in the accompanying drawings, the same element is marked with the same figure mark and repeated descriptions are omitted. In addition, the positional relationship such as up and down, left and right is based on the positional relationship shown in the accompanying drawings unless otherwise specified. Moreover, the dimensional ratio of the accompanying drawings is not limited to the ratio shown in the drawings.
[0045] 1. Abrasive pad
[0046] The polishing pad of this embodiment has a polishing layer and an endpoint detection window arranged at an opening of the polishing layer. In a dynamic viscoelasticity measurement performed under the conditions of a tensile mode, a frequency of 1.6 Hz, 30 to 55°C, and an immersed state, the ratio of the storage modulus E'w40 of the aforementioned endpoint detection window at 40°C to the storage modulus E'p40 of the aforementioned polishing layer at 40°C (E'p40 / E'w40) is 0.70 to 3.00.
[0047] Thus, during grinding, the dynamic viscoelastic properties of the grinding layer and the endpoint detection window are closer, so even if the endpoint detection window as a different component is embedded in the grinding layer, the generation of defects (surface defects) on the surface of the object to be ground can be further suppressed. Therefore, an object to be ground with excellent surface quality can be obtained.
[0048] Figure 1 A schematic three-dimensional diagram of the polishing pad according to this embodiment is shown. Figure 1As shown, the polishing pad 10 of this embodiment includes a polishing layer 11 which is a polyurethane sheet, and an endpoint detection window 12 , and may include a cushion layer 13 on the side opposite to the polishing surface 11 a as required.
[0049] Figures 2-3 Show Figure 1 A cross-sectional view of the periphery of the endpoint detection window 12 in FIG. Figures 2-3 As shown, an adhesive layer 14 may be provided between the grinding layer 11 and the buffer layer 13. In addition, a bonding layer 14 may be provided on the surface of the buffer layer 13 for bonding with the grinding layer 11. Figure 4 The worktable 22 is bonded with the adhesive layer 15. The polishing surface 11a of the polishing pad of this embodiment has Figure 2 In addition to the flat case shown, it can also be Figure 3 The figure shows a concavo-convex shape formed with grooves 16. The grooves 16 may be formed singly or in combination of a plurality of grooves in various shapes such as concentric circles, lattice, or radial shapes.
[0050] 1.1. End point detection window
[0051] The end point detection window is a transparent component provided at the opening of the polyurethane sheet, and in the optical end point detection, it becomes a transmission path of light from the film thickness detection sensor. In the present embodiment, the end point detection window is circular, but it can also be square, rectangular, polygonal, elliptical or other shapes as required.
[0052] In this embodiment, by adjusting the wear degree of the endpoint detection window and the polishing layer during polishing, etc., the ratio of the endpoint detection window to the storage modulus E' of the polyurethane sheet is specified from the viewpoint of suppressing defects (surface defects) on the non-polished object caused by excessive polishing of one of the endpoint detection window or the polishing layer.
[0053] Dynamic viscoelasticity
[0054] The storage modulus E' of the endpoint detection window and the polishing layer in this embodiment can be obtained by dynamic viscoelasticity measurement under the conditions of tensile mode, frequency 1.6 Hz, 30-55°C, and immersion in water. It should be noted that, unless otherwise specified in this embodiment, the dynamic viscoelasticity measurement is performed under immersion in water.
[0055] In the polishing process in which the slurry contacts the polishing pad, the polishing surface is in a water-immersed state. Therefore, in the present embodiment, at 40°C, which is equivalent to the temperature during polishing, the ratio of the dynamic viscoelasticity of the endpoint detection window and the polishing layer in the water-immersed state is specified. More specifically, in the dynamic viscoelasticity measurement performed under the conditions of a tensile mode, a frequency of 1.6 Hz, 30 to 55°C, and a water-immersed state, the ratio (E'p40 / E'w40) of the storage modulus E'w40 of the endpoint detection window at 40°C and the storage modulus E'p40 of the polishing layer at 40°C is specified.
[0056] The ratio (E'p40 / E'w40) is 0.70 to 3.00, preferably 0.80 to 2.50, and more preferably 0.90 to 2.00. By making the ratio (E'p40 / E'w40) within the above range, the characteristics of the end point detection window and the grinding layer during grinding are similar, so the surface quality of the obtained object to be ground is further improved. As a result, the contact state with the object to be ground (workpiece) during grinding is further optimized, and the continuous pressing of grinding chips is suppressed, thereby suppressing the generation of scratches.
[0057] In the dynamic viscoelasticity measurement in the above-mentioned immersed state, the ratio of the storage modulus E'w50 of the end point detection window at 50°C to the storage modulus E'p50 of the polishing layer at 50°C (E'p50 / E'w50) is preferably 0.70 to 5.00, more preferably 0.80 to 4.00, and further preferably 0.90 to 3.00. By making the ratio (E'p50 / E'w50) within the above-mentioned range, the characteristics of the end point detection window and the polishing layer during polishing are similar, so there is a tendency for the surface quality of the obtained object to be polished to be further improved.
[0058] In the dynamic viscoelasticity measurement in the above-mentioned immersed state, the difference between the loss factor tanδw30 of the endpoint detection window at 30°C and the loss factor tanδp30 of the polishing layer at 30°C (|tanδw30-tanδp30|) is preferably 0 to 0.30, more preferably 0.05 to 0.30, and further preferably 0.05 to 0.20.
[0059] In the dynamic viscoelasticity measurement in the above-mentioned immersed state, the difference between the loss factor tanδw40 of the endpoint detection window at 40°C and the loss factor tanδp40 of the polishing layer at 40°C (|tanδw40-tanδp40|) is preferably 0 to 0.40, more preferably 0.05 to 0.40, and further preferably 0.05 to 0.30.
[0060] In the dynamic viscoelasticity measurement in the above-mentioned immersed state, the difference between the loss factor tanδw50 of the endpoint detection window at 50°C and the loss factor tanδp50 of the polishing layer at 50°C (|tanδw50-tanδp50|) is preferably 0 to 0.50, more preferably 0.05 to 0.50, and further preferably 0.05 to 0.40.
[0061] By making the difference (|tanδw30-tanδp30|), the difference (|tanδw40-tanδp40|), and the difference (|tanδw50-tanδp50|) respectively within the above-mentioned ranges, the characteristics of the endpoint detection window and the polishing layer during polishing are similar, so there is a tendency for the surface quality of the polished object to be further improved.
[0062] The storage modulus E'w40 of the endpoint detection window at 40°C in the water-immersed state is preferably 6.0 to 50×10 7 Pa, more preferably 8.0 to 40×10 7 Pa is more preferably 10 to 30×10 7 Pa.
[0063] The storage modulus E'w50 of the endpoint detection window at 50°C in the water-immersed state is preferably 2.0 to 40×10 7 Pa, more preferably 3.0 to 30×10 7 Pa is more preferably 4.0 to 20×10 7 Pa.
[0064] The tan δw40 of the endpoint detection window at 40° C. in the immersed state is preferably 0.1 to 0.7, more preferably 0.1 to 0.6, and even more preferably 0.1 to 0.5.
[0065] The tan δw50 of the endpoint detection window at 50° C. in the immersed state is preferably 0.1 to 0.6, more preferably 0.1 to 0.5, and even more preferably 0.1 to 0.4.
[0066] By setting E'w40, E'w50, tan δw40, and tan δw50 to be within the above ranges, the endpoint detection window during polishing and the characteristics of the polishing layer are made similar, so that the surface quality of the obtained object to be polished tends to be further improved.
[0067] The measurement conditions for the dynamic viscoelasticity measurement are not particularly limited, and the measurement can be performed under the conditions described in the Examples.
[0068] 1.1.3. Constituent materials
[0069] The material constituting the endpoint detection window is not particularly limited as long as it is a transparent component that can function as a window, and for example, polyurethane resin WI, polyvinyl chloride resin, polyvinylidene fluoride resin, polyether sulfone resin, polystyrene resin, polyethylene resin, polytetrafluoroethylene resin, etc. can be cited. Among them, polyurethane resin WI is preferred. By using such a resin, it is easier to adjust the above-mentioned dynamic viscoelastic properties and transparency, and the surface quality can be further improved.
[0070] The polyurethane resin WI can be synthesized from polyisocyanate and polyol, and includes a structural unit derived from polyisocyanate and a structural unit derived from polyol.
[0071] 1.1.3.1. Structural units derived from polyisocyanates
[0072] The structural unit from polyisocyanate is not particularly limited, for example, a structural unit from alicyclic isocyanate, a structural unit from aliphatic isocyanate, and a structural unit from aromatic isocyanate can be cited. Among them, the polyurethane resin WI preferably includes a structural unit from alicyclic isocyanate and / or aliphatic isocyanate, and more preferably includes a structural unit from aliphatic isocyanate. Thus, it is easy to adjust the dynamic viscoelastic properties within the above range, and in addition to further improving transparency, there is also a trend of further improving surface quality.
[0073] The alicyclic isocyanate is not particularly limited, and examples thereof include 4,4′-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), cyclohexylene-1,2-diisocyanate, cyclohexylene-1,4-diisocyanate, and isophorone diisocyanate.
[0074] The aliphatic isocyanate is not particularly limited, and examples thereof include hexamethylene diisocyanate (HDI), pentamethylene diisocyanate (PDI), tetramethylene diisocyanate, propylene-1,2-diisocyanate, butylene-1,2-diisocyanate, trimethylene diisocyanate, and trimethylhexamethylene diisocyanate.
[0075] The aromatic isocyanate is not particularly limited, and examples thereof include phenylene diisocyanate, 2,6-toluene diisocyanate (2,6-TDI), 2,4-toluene diisocyanate (2,4-TDI), xylylene diisocyanate, naphthalene diisocyanate, and diphenylmethane-4,4′-diisocyanate (MDI).
[0076] 1.1.3.2. Structural units from polyols
[0077] The structural unit derived from the polyol is not particularly limited, and examples thereof include low-molecular-weight polyols having a molecular weight of less than 300 and high-molecular-weight polyols having a molecular weight of 300 or more.
[0078] The low molecular weight polyol is not particularly limited, and examples thereof include low molecular weight polyols having two hydroxyl groups, such as ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, 1,2-butanediol, 1,3-butanediol, 2,3-butanediol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 2,5-hexanediol, dipropylene glycol, 2,2,4-trimethyl-1,3-pentanediol, tricyclodecane dimethanol, 1,4-cyclohexanedimethanol, and low molecular weight polyols having three or more hydroxyl groups, such as glycerol, hexanetriol, trimethylolpropane, isocyanuric acid, and erythritol. The low molecular weight polyol may be used alone or in combination of two or more.
[0079] Among them, low molecular weight polyols having three or more hydroxyl groups are preferred, and glycerol is more preferred. By using such low molecular weight polyols, the dynamic viscoelasticity characteristics can be easily adjusted within the above range, the wear amount can be adjusted, and in addition to further improving transparency, there is a trend that the surface quality is further improved.
[0080] The content of the structural unit derived from the low molecular weight polyol having 3 or more hydroxyl groups is preferably 7.5 to 30 parts by mass, more preferably 10 to 25 parts by mass, and further preferably 12.5 to 20 parts by mass relative to 100 parts by mass of the structural unit derived from the polyisocyanate. By making the content of the structural unit derived from the low molecular weight polyol having 3 or more hydroxyl groups within the above range, it is easy to adjust the dynamic viscoelastic properties within the above range, and in addition to further improving transparency, there is also a tendency for further improving surface quality.
[0081] In addition, the polymer polyol is not particularly limited, and examples thereof include polyether polyol, polyester polyol, polycarbonate polyol, polyether polycarbonate polyol, polyurethane polyol, epoxy polyol, vegetable oil polyol, polyolefin polyol, acrylic polyol, and vinyl monomer modified polyol. The polymer polyol may be used alone or in combination of two or more.
[0082] The number average molecular weight of the high molecular weight polyol is preferably 300 to 3000, and more preferably 500 to 2500. By using such a high molecular weight polyol, the dynamic viscoelasticity characteristics tend to be easily adjusted to the above range.
[0083] Among them, polyether polyol is preferred, and poly(oxytetramethylene) glycol is more preferred. By using such a high molecular weight polyol, it is easy to adjust the dynamic viscoelasticity characteristics to the above range. In addition, in addition to further improving transparency, there is also a trend that the yellowing resistance of the window is further improved.
[0084] The content of the structural unit derived from the polyether polyol is preferably 60 to 130 parts by mass, preferably 65 to 120 parts by mass, and more preferably 70 to 110 parts by mass relative to 100 parts of the structural unit derived from the polyisocyanate. By making the content of the structural unit derived from the polyether polyol within the above range, it is easy to adjust the dynamic viscoelastic properties within the above range, and in addition to further improving the transparency, there is also a tendency for the yellowing resistance of the window to be further improved.
[0085] In addition, as the polyol, it is preferred to use a low molecular weight polyol and a high molecular weight polyol in combination, and it is more preferred to use a low molecular weight polyol having three or more hydroxyl groups and a polyether polyol in combination. Thus, it is easy to adjust the dynamic viscoelasticity characteristics to the above range, and in addition to further improving transparency, there is also a tendency for the yellowing resistance of the window to be further improved.
[0086] From the above viewpoints, the content of the polyether polyol is preferably 2.0 to 15.0 parts, more preferably 3.0 to 12.5 parts, and even more preferably 4.0 to 9.0 parts, based on 1 part of the low-molecular polyol having three or more hydroxyl groups.
[0087] 1.2. Grinding layer
[0088] The polishing layer of this embodiment has an opening for embedding the end point detection window. The position of the opening is not particularly limited, but it is preferably set at a position in the radial direction corresponding to the film thickness detection sensor 23 set on the workbench 22. In addition, the number of openings is not particularly limited, but it is preferably provided with a plurality of openings at the same radial position so that when the polishing pad 10 attached to the workbench 22 rotates one circle, the window passes over the film thickness detection sensor 23 multiple times.
[0089] The form of the polishing layer is not particularly limited, and examples thereof include a resin foamed molded product, a non-foamed molded product, and a resin-impregnated substrate in which a fiber substrate is impregnated with a resin.
[0090] Here, the resin foamed molded body refers to a foamed body composed of a predetermined resin without a fiber base material. The foamed shape is not particularly limited, and examples thereof include spherical cells, substantially spherical cells, teardrop-shaped cells, or continuous cells formed by partially connecting cells.
[0091] In addition, the non-foamed molded body of resin refers to a non-foamed body that does not have a fiber substrate and is composed of a specified resin. Non-foamed body refers to a material that does not have bubbles as described above. In the first embodiment, a material formed by adhering a curable composition to a substrate such as a film and solidifying it is also included in the non-foamed molded body of resin. More specifically, the resin cured product formed by gravure coating, small-diameter gravure coating, reverse roll coating, transfer roll coating, kiss coating, die coating, screen printing, spray coating, etc. is also included in the non-foamed molded body of resin.
[0092] The resin-impregnated substrate refers to a substrate obtained by impregnating a fiber substrate with a resin. The fiber substrate is not particularly limited, and examples thereof include woven fabrics, nonwoven fabrics, and knitted fabrics.
[0093] Dynamic viscoelasticity
[0094] The storage elastic modulus E'p40 of the polishing layer at 40°C in the water-immersed state is preferably 10 to 40×10 7 Pa, more preferably 15 to 35×10 7 Pa is more preferably 20 to 30 × 10 7 Pa.
[0095] The storage elastic modulus E'p50 of the polishing layer at 50°C in the water-immersed state is preferably 50 to 35×10 7 Pa, more preferably 10 to 30×10 7 Pa is more preferably 15 to 25×10 7 Pa.
[0096] The tan δp40 of the polishing layer in a water-immersed state at 40° C. is preferably 0.01 to 0.25, more preferably 0.03 to 0.20, and even more preferably 0.05 to 0.15.
[0097] The tan δp50 of the polishing layer in a water-immersed state at 50° C. is preferably 0.01 to 0.25, more preferably 0.03 to 0.20, and even more preferably 0.05 to 0.15.
[0098] By making E' p40 , E' p50 , tanδ p40 , and tanδ p50 When each is within the above range, the characteristics of the endpoint detection window and the polishing layer during polishing are similar, so there is a tendency that the surface quality of the obtained object to be polished is further improved.
[0099] 1.2.2. Polyurethane sheet
[0100] Hereinafter, as an example of the grinding layer, a polyurethane sheet is exemplified. As the polyurethane resin P constituting the polyurethane sheet, there is no particular restriction, for example, polyester polyurethane resin, polyether polyurethane resin, and polycarbonate polyurethane resin can be cited. These can be used alone or in combination of two or more.
[0101] As such polyurethane resin P, it can be synthesized by polyisocyanate and polyol, and the reactant of urethane prepolymer and curing agent is particularly preferred. Here, urethane prepolymer can be synthesized by polyisocyanate and polyol. Hereinafter, polyisocyanate, polyol, and curing agent constituting polyurethane resin P are described.
[0102] 1.2.2.1. Structural units from polyisocyanates
[0103] The structural unit derived from the polyisocyanate is not particularly limited, and examples thereof include structural units derived from alicyclic isocyanates, structural units derived from aliphatic isocyanates, and structural units derived from aromatic isocyanates. Among them, aromatic isocyanates are preferred, and 2,4-toluene diisocyanate (2,4-TDI) is more preferred.
[0104] Examples of the alicyclic isocyanate, the aliphatic isocyanate, and the aromatic isocyanate include the same ones as those exemplified in the above-mentioned endpoint detection window.
[0105] 1.2.2.2. Structural units from polyols
[0106] The structural unit derived from the polyol is not particularly limited, and examples thereof include low molecular weight polyols having a molecular weight of less than 300 and high molecular weight polyols having a molecular weight of 300 or more. Among them, it is preferred to use at least a low molecular weight polyol, and it is preferred to use a low molecular weight polyol and a high molecular weight polyol in combination.
[0107] As low molecular weight polyol and high molecular weight polyol, the same substances as those exemplified in the above-mentioned endpoint detection window can be exemplified. Among them, as low molecular weight polyol, preferably a low molecular weight polyol having two hydroxyl groups, more preferably diethylene glycol. In addition, as high molecular weight polyol, preferably a polyether polyol, more preferably poly (oxytetramethylene) glycol.
[0108] 1.2.2.3. Curing agent
[0109] The curing agent is not particularly limited, and examples thereof include polyamines and polyols. The curing agent may be used alone or in combination of two or more.
[0110] The polyamine is not particularly limited, and examples thereof include aliphatic polyamines such as ethylenediamine, propylenediamine, and hexamethylenediamine; alicyclic polyamines such as isophoronediamine and dicyclohexylmethane-4,4'-diamine; and aromatic polyamines such as 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA), 4-methyl-2,6-bis(methylthio)-1,3-phenylenediamine, 2-methyl-4,6-bis(methylthio)-1,3-phenylenediamine and 2,2-bis(3-amino-4-hydroxyphenyl)propane.
[0111] Among them, aromatic polyamines are preferred, and 3'-dichloro-4,4'-diaminodiphenylmethane (MOCA) is more preferably used.
[0112] Examples of the polyol include the same polyols as those exemplified in the above-mentioned endpoint detection window, among which polymer polyols are preferred, polyether polyols are more preferred, and polypropylene glycol is still more preferred.
[0113] 1.2.2.4. Hollow particles
[0114] The polishing layer preferably includes hollow particles dispersed in the polishing layer. Specifically, the polyurethane sheet is preferably a foamed polyurethane sheet including a polyurethane resin P and hollow particles dispersed in the polyurethane resin P. Such a polyurethane sheet has independent bubbles from the hollow particles, and tends to easily adjust the dynamic viscoelastic properties to the above range.
[0115] Hollow particles can use commercially available hollow particles, and hollow particles synthesized by conventional methods can also be used. As the material of the shell of hollow particles, there is no particular restriction, for example, polyvinyl alcohol, polyvinyl pyrrolidone, poly (methyl) acrylic acid, polyacrylamide, polyethylene glycol, polyhydroxy ether acrylate, maleic acid copolymer, polyethylene oxide, polyurethane, acrylonitrile-vinylidene chloride copolymer, acrylonitrile-methyl methacrylate copolymer, vinyl chloride-ethylene copolymer etc. can be cited.
[0116] The shape of the hollow fine particles is not particularly limited, and may be, for example, spherical or substantially spherical. In addition, when the hollow fine particles are expandable balloons, the hollow fine particles may be used in an unexpanded state or in an expanded state.
[0117] The average particle size of the hollow fine particles contained in the polyurethane sheet is preferably 5 to 200 μm, more preferably 5 to 80 μm, further preferably 5 to 50 μm, and particularly preferably 5 to 35 μm. By making the average particle size within the above range, there is a tendency to easily adjust the dynamic viscoelastic properties to the above range. It should be noted that the average particle size can be measured by a laser diffraction particle size distribution measuring device (e.g., Mastersizer-2000 manufactured by Spectris (Strain)).
[0118] 1.3. Others
[0119] The polishing pad of this embodiment may have a buffer layer on the side of the polishing layer opposite to the polishing surface, or may have an adhesive layer between the polishing layer and the buffer layer, on the surface of the buffer layer on the non-polishing layer side (the surface attached to the grinder). In this case, the buffer layer and the adhesive layer have openings at the same location as the location of the endpoint detection window of the polishing layer.
[0120] 2. Manufacturing method of polishing pad
[0121] The manufacturing method of the polishing pad of the present embodiment is not particularly limited, and for example, comprises the following steps: a step of filling a resin composition constituting a polishing layer in a mold having a window component serving as an endpoint detection window fixed thereto and curing the resin composition to obtain a resin block in which the window component is embedded; and a step of slicing the obtained resin block to obtain a polyurethane sheet having an endpoint detection window at an opening. If necessary, the polishing surface of the obtained polyurethane sheet may also be trimmed in the manufacturing method.
[0122] The temperature during slicing is preferably 70 to 100° C. The temperature during trimming is preferably 20 to 30° C.
[0123] 3. Method for manufacturing polished product
[0124] The method for producing a polished product of this embodiment includes: a polishing step of polishing an object to be polished using the polishing pad in the presence of a polishing slurry to obtain a polished product; and an endpoint detection step of performing endpoint detection during the polishing using an optical endpoint detection method.
[0125] 3.1. Grinding process
[0126] The lapping process may be a single lapping (rough lapping), a double lapping (fine lapping), a single polishing (rough polishing), a double polishing (fine polishing), or a combination of these lapping processes. It should be noted that, herein, the so-called "lapping" refers to lapping at a relatively high rate using coarse abrasive grains, and the so-called "polishing" refers to lapping at a relatively low rate using fine abrasive grains to improve the surface quality.
[0127] Among them, the polishing pad of this embodiment is preferably used for chemical mechanical polishing (CMP). Hereinafter, the manufacturing method of the polishing material of this embodiment will be described by taking chemical mechanical polishing as an example, but the manufacturing method of the polishing material of this embodiment is not limited to the following.
[0128] The object to be polished is not particularly limited, and examples thereof include materials such as semiconductor devices and electronic components, and in particular, thin substrates (object to be polished) such as Si substrates (silicon wafers), SiC (silicon carbide) substrates, GaAs (gallium arsenide) substrates, glass, hard disks, and LCD (liquid crystal display) substrates. In particular, semiconductor devices having metal wiring such as W (tungsten) and Cu (copper) can be cited.
[0129] As a grinding method, a known method in the past can be used, which is not particularly limited. For example, first, the object to be ground held by the holding platform configured in a manner opposed to the grinding pad is pressed to the grinding surface side, and slurry is supplied from the outside while the grinding pad and / or the holding platform are rotated. The grinding pad and the holding platform can rotate in the same direction with different rotation speeds, or they can rotate in different directions. In addition, the object to be ground can also be ground while moving (rotating) in the inner side of the frame during grinding.
[0130] The slurry may contain chemical components such as water, oxidizing agents represented by hydrogen peroxide, additives, abrasives (abrasive particles; for example, SiC, SiO2, Al2O3, CeO2), etc., depending on the object to be polished, polishing conditions, etc.
[0131] 3.2. End point detection process
[0132] The method for producing a polished product of the present embodiment includes an endpoint detection step of performing endpoint detection by an optical endpoint detection method in the polishing step. As the endpoint detection method using the optical endpoint detection method, specifically, a conventionally known method can be used.
[0133] Figure 4 A schematic diagram of an endpoint detection method of an optical endpoint detection method is shown. In the schematic diagram, a chemical mechanical polishing process is shown in which a slurry 24 is made to flow on a polishing pad 10 attached to a workbench 22 while a wafer W held by a top ring 21 is pressed, thereby grinding the concave-convex film on the surface of the wafer W to make it flat. In the polishing device 20, in order to perform endpoint detection of a predetermined film thickness while flattening and terminate the process with high precision, a film thickness detection sensor 23 that monitors the film thickness is mounted on the workbench 22. The film thickness detection sensor 23, for example, irradiates light to the polished surface of the wafer W, and can detect the polishing endpoint by measuring and analyzing the spectral intensity characteristics of the reflected light.
[0134] More specifically, the film thickness detection sensor 23 causes light to be incident on the surface of the chip W through the endpoint detection window 12, and detects the strength of the reflection intensity caused by the phase difference between the light reflected by the film on the chip W (chip surface) and the light reflected at the interface between the film on the chip W and the chip substrate, thereby detecting the change in film thickness.
[0135] Example
[0136] The present invention will be described in more detail below using Examples and Comparative Examples. The present invention is not limited to the following Examples. It should be noted that "parts" refer to parts by mass.
[0137] [Manufacturing Example 1: End point detection window 1]
[0138] 100 parts of 4,4′-methylenebis(cyclohexyl isocyanate), 90.6 parts of poly(oxytetramethylene) glycol (PTMG) having a number average molecular weight of 1000, and 16.7 parts of glycerol were reacted to obtain a transparent member serving as the end point detection window 4 .
[0139] [Manufacturing Example 2: End point detection window 2]
[0140] 100 parts of 4,4′-methylenebis(cyclohexyl isocyanate), 103.6 parts of poly(oxytetramethylene) glycol (PTMG) having a number average molecular weight of 1000, and 15.9 parts of glycerol were reacted to obtain a transparent member serving as the end point detection window 2 .
[0141] [Manufacturing Example 3: End point detection window 3]
[0142] 100 parts of 4,4′-methylenebis(cyclohexyl isocyanate), 78.6 parts of poly(oxytetramethylene) glycol (PTMG) having a number average molecular weight of 650, 4.5 parts of glycerol, and 10.5 parts of ethylene glycol were reacted to obtain a transparent member serving as the end point detection window 3 .
[0143] [Example 1]
[0144] 2.9 parts of unexpanded hollow fine particles (average particle size: 8.5 μm) whose shell part is composed of acrylonitrile-vinylidene chloride copolymer and which are not expanded are added to 100 parts of a urethane prepolymer having an NCO equivalent of 420 obtained by reacting 2,4-toluene diisocyanate (2,4-TDI), poly(oxytetramethylene) glycol (PTMG) having a number average molecular weight of 650, poly(oxytetramethylene) glycol (PTMG) having a number average molecular weight of 1000, and diethylene glycol (DEG) to obtain a urethane prepolymer mixed liquid. The obtained urethane prepolymer mixed liquid is placed in a first liquid tank and kept at 60°C. In addition, 28.0 parts of 3,3'-dichloro-4,4'-diaminodiphenylmethane (methylenebis(o-chloroaniline)) (MOCA) as a curing agent is placed in a second liquid tank separately from the first liquid tank, heated and melted at 120°C and mixed, and further degassed under reduced pressure to obtain a curing agent melt.
[0145] Next, the liquids in the first liquid tank and the second liquid tank are injected from the respective injection ports of a mixer having two injection ports, and stirred and mixed to obtain a mixed liquid.
[0146] Then, the obtained mixed solution was cast into a mold pre-set with the endpoint detection window 1 obtained as described above, and primary curing was performed at 80° C. for 30 minutes. The formed block-shaped molded product was taken out of the mold and secondary cured in an oven at 120° C. for 4 hours to obtain a polyurethane resin block. The obtained polyurethane resin block was naturally cooled to 25° C.
[0147] Then, after heating in an oven at 120° C. for 5 hours, the sheet was sliced, and the surface obtained by slicing was ground (polished) as needed to obtain a foamed polyurethane sheet. A double-sided tape was pasted on the back of the obtained polyurethane sheet, a buffer layer was pasted, and a double-sided tape was pasted on the surface of the buffer layer to obtain a polishing pad.
[0148] [Example 2]
[0149] A polishing pad of Example 2 was obtained by the same operation as in Example 1 except that the endpoint detection window 2 produced in the above-mentioned Production Example 2 was used instead of the endpoint detection window 1 .
[0150] [Comparative Example 1]
[0151] A polishing pad of Comparative Example 1 was obtained by the same operation as in Example 1 except that the endpoint detection window 3 produced in the above-mentioned Production Example 3 was used instead of the endpoint detection window 1 .
[0152] [Dynamic viscoelasticity measurement]
[0153] Based on the following conditions, the dynamic viscoelasticity of the polyurethane sheet was measured. First, the polyurethane sheet was immersed in water at a temperature of 23°C for 3 days. The obtained polyurethane sheet was used as a sample to perform a dynamic viscoelasticity measurement in water (immersed in water). It should be noted that the sample size of the endpoint detection window is set to 5 cm long × 0.5 cm wide × 0.13 cm thick, and the sample size of the grinding layer is set to 5 cm long × 0.5 cm wide × 0.13 cm thick.
[0154] (Measurement conditions)
[0155] Measuring device: RSA G2 (manufactured by TA Instruments)
[0156] Test length: 1cm
[0157] Sample pretreatment: Keep in water at 23°C for 3 days
[0158] Test mode: tensile
[0159] Frequency: 1.6Hz
[0160] Temperature range: 30~55℃
[0161] Heating rate: 0.3℃ / min
[0162] Strain range: 0.10%
[0163] Initial load: 300g
[0164] Measurement interval: 200 points / ℃
[0165] 〔Surface quality confirmation test〕
[0166] A polishing pad was set at a predetermined position of a polishing device via a double-sided tape having an acrylic adhesive, and a Cu film substrate was polished under the following conditions.
[0167] (Grinding conditions)
[0168] Grinding machine: F-REX300X (manufactured by Ebara Manufacturing Co., Ltd.)
[0169] Disk: A188 (manufactured by 3M)
[0170] Speed: (platform) 85rpm, (top ring) 86rpm
[0171] Grinding pressure: 3.5psi
[0172] Abrasive temperature: 20°C
[0173] Abrasive spray volume: 200ml / min
[0174] Abrasive: CSL-9044C (manufactured by FUJIMI CORPORATION) (Use a mixture of CSL-9044C stock solution and pure water at a weight ratio of 1:9)
[0175] Object to be polished: Cu film substrate
[0176] Grinding time: 60 seconds
[0177] Pad activation operation: 35N 10 minutes
[0178] Conditioning: Ex-situ, 35N, 4 scans
[0179] For the 10th to 50th pieces of the polished material after the above-mentioned grinding process, the high-sensitivity measurement mode of the surface inspection device (Surfscan SP2XP manufactured by KLA-Tencor) was used to detect and evaluate defects (surface defects) with a size of 155 nm or more. Based on the confirmation results of the defects (surface defects), the surface quality was evaluated.
[0180] [Table 1]
[0181]
[0182] It should be noted that the "ratio p / w" in the table represents the ratio of the storage modulus E'w of the endpoint detection window to the storage modulus E'p of the polishing layer at the same temperature, or the ratio of tanδw of the endpoint detection window to tanδp of the polishing layer. For example, according to Table 1, the ratio (E'p40 / E'w40) of Example 1 is 0.95, the ratio (E'p40 / E'w40) of Example 2 is 1.62, and the ratio (E'p40 / E'w40) of Comparative Example 1 is 4.90.
[0183] In addition, the "difference |pw|" in the table represents the difference between the storage modulus E'w of the endpoint detection window and the storage modulus E'p of the polishing layer at the same temperature, or the difference between tanδw of the endpoint detection window and tanδp of the polishing layer. For example, according to Table 1, the difference (|tanδw30-tanδp30|) of Example 1 is 0.07, the difference (|tanδw30-tanδp30|) of Example 2 is 0.12, and the difference (|tanδw30-tanδp30|) of Comparative Example 1 is 0.34.
[0184] Industrial Applicability
[0185] The polishing pad of the present invention has industrial applicability as a pad suitable for polishing semiconductor wafers and the like.
[0186] Description of Reference Numerals
[0187] 10...polishing pad, 11...polishing layer, 11a...polishing surface, 12...end point detection window, 13...buffer layer, 14, 15...adhesive layer, 16...groove, 20...polishing device, 21...top ring, 22...work table, 23...film thickness detection sensor, 24...slurry, W...wafer
Claims
1. A polishing pad comprising a polishing layer and an endpoint detection window provided at an opening of the polishing layer, In the dynamic viscoelasticity measurement conducted in a tensile mode at a frequency of 1.6 Hz, 30 to 55° C., and in a water-immersed state, the ratio of the storage modulus E'w40 of the endpoint detection window at 40° C. to the storage modulus E'p40 of the polishing layer at 40° C. (E'p40 / E'w40) is 0.70 to 3.
00.
2. The polishing pad according to claim 1, wherein In the dynamic viscoelasticity measurement, a ratio of a storage elastic modulus E'w50 of the endpoint detection window at 50° C. to a storage elastic modulus E'p50 of the polishing layer at 50° C. (E'p50 / E'w50) is 0.70 to 5.
00.
3. The polishing pad according to claim 1, wherein In the dynamic viscoelasticity measurement, the difference between the loss factor tanδw30 of the endpoint detection window at 30°C and the loss factor tanδp30 of the polishing layer at 30°C (|tanδw30-tanδp30|) is 0.05 to 0.
30.
4. The polishing pad according to claim 1, wherein In the dynamic viscoelasticity measurement, the difference between the loss factor tanδw40 of the endpoint detection window at 40°C and the loss factor tanδp40 of the polishing layer at 40°C (|tanδw40-tanδp40|) is 0.05 to 0.
40.
5. The polishing pad according to claim 1, wherein In the dynamic viscoelasticity measurement, the difference between the loss factor tanδw50 of the endpoint detection window at 50°C and the loss factor tanδp50 of the polishing layer at 50°C (|tanδw50-tanδp50|) is 0.05 to 0.
50.
6. The polishing pad according to claim 1, wherein The endpoint detection window comprises polyurethane resin WI, The polyurethane resin WI comprises structural units derived from aliphatic isocyanate.
7. The polishing pad according to claim 1, wherein The grinding layer comprises a polyurethane resin P, The polyurethane resin P includes a structural unit derived from an aromatic isocyanate.
8. The polishing pad according to claim 1, wherein The polishing layer includes hollow fine particles dispersed in the polishing layer.
9. A method for producing a ground product, comprising: a polishing step of polishing an object to be polished using the polishing pad according to any one of claims 1 to 8 in the presence of a polishing slurry to obtain a polished object; and In the end point detection step, an optical end point detection method is used to detect the end point during the polishing process.