Deep eutectic solvent / polymer blend membrane material for SO2 separation

Through the combination of deep eutectic solvent and polymer matrix blended membrane materials, the solid waste and pollution problems of traditional flue gas desulfurization methods are solved, and high selectivity and low cost SO2 separation is achieved, meeting the requirements of green chemical industry and improving The properties of the membrane material.

CN119015894APending Publication Date: 2024-11-26NANJING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310586626.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The traditional flue gas desulfurization method has irreversible industrial solid waste and wastewater production, as well as volatile organic substance pollution during the absorption of organic solvents, which violates the concept of green chemical engineering, and it is difficult for polymer films to achieve high permeability and high selectivity at the same time.

Method used

The SO2 separation membrane was prepared by blending a deep eutectic solvent with a polymer matrix, and a homogeneous membrane and a thin-layer composite membrane were prepared by solution casting. The imidazole halogen salt and polyol were combined as hydrogen bond acceptors and donors to prepare deep eutectic membranes. A blended film material of solvent and polymer matrix for selective separation of SO2 at different concentrations and compositions.

Benefits of technology

It has achieved low cost, stable structure, large penetration flux and good selectivity, reduced investment and operation costs for industrial applications, and has broad industrial application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BSA0000296985580000041
    Figure BSA0000296985580000041
Patent Text Reader

Abstract

The invention discloses a deep eutectic solvent / polymer blended membrane material for high-selectivity separation of SO2. The membrane material is prepared by blending a deep eutectic solvent containing imidazole halide salt and a polymer matrix. Specifically, the deep eutectic solvent is composed of an imidazole halide salt as a hydrogen bond acceptor and a polyol as a hydrogen bond donor. A polymer which is high in stability and good in compatibility with a used deep eutectic solvent is adopted as a matrix, and the separation membrane material is prepared through a solution casting method. The deep eutectic solvent / polymer membrane material is simple to prepare and low in cost, has high SO2 permeation rate and high SO2 selectivity (SO2 / CO2 and SO2 / N2), can be used for selective separation of SO2 in flue gases with various concentrations and compositions, and has the potential of large-scale application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a membrane material for selectively separating SO2 mixed gas, belonging to the technical field of gas separation and purification in green chemical industry, and specifically to the preparation of a deep eutectic solvent / polymer blend membrane material and its use for highly selective separation of SO2 in flue gases of different concentrations and compositions. Background Art

[0002] Sulfur dioxide (SO2) mainly comes from industrial waste gas, which can cause acid rain and haze. Traditional flue gas desulfurization methods mainly include limestone slurry absorption, ammonia washing and organic solvent absorption. However, the inherent shortcomings of these technologies cannot be ignored. For example, the absorption of SO2 by limestone slurry or ammonia will irreversibly produce a large amount of industrial solid waste and wastewater; during the organic solvent absorption process, volatile organic compounds (VOCs) are easily volatilized into the airflow to cause pollution, which violates the concept of green chemical industry. In view of the above shortcomings, it is a challenge to develop new desulfurization media or technologies with good reversibility, high efficiency and environmental friendliness, but it is also extremely necessary.

[0003] Membrane separation has outstanding advantages in energy efficiency, equipment cost and process flexibility, and is one of the most widely studied and fastest growing separation technologies. Polymers have become the most commonly used gas separation membrane materials due to their low cost and processability. However, it is difficult for polymer membranes to achieve high permeability and high selectivity at the same time. In addition to synthesizing new membrane materials, the method of modifying commonly used polymers is currently widely used to break through the mutual constraints between permeability and selectivity.

[0004] Deep Eutectic Solvents (DESs) are a new type of green solvent, usually formed by a simple mixture of hydrogen bond donors and hydrogen bond acceptors through hydrogen bond interactions. They have the advantages of a wide range of raw material sources, simple synthesis, no need for subsequent purification, low cost, and high gas capture capacity. At present, there are many studies on the absorption of SO2 by DESs, among which DESs containing 1-alkyl-3-methylimidazolium halide ionic liquids have the best effect (CN110448996A; CN111821813A; CN109529555A). However, most of the above-mentioned deep eutectic solvents are aimed at the SO2 absorption and capture process. However, considering that the dosage of industrial absorbents is generally high and heating desorption is required, the direct use of such deep eutectic solvents as industrial absorbents will result in higher investment costs and operating costs.

[0005] The present invention reports a deep eutectic solvent / polymer blend membrane material for SO2 separation. This type of membrane material combines the advantages of the high SO2 separation performance of the deep eutectic solvent and the membrane separation technology. It has the advantages of low cost, stable structure, excellent performance, and long-lasting operation. It can be used for the selective separation of SO2 in various flue gases and has great industrial application potential. Summary of the invention

[0006] The purpose of the present invention is to disclose a SO2 separation membrane material prepared from a deep eutectic solvent and a polymer matrix, which can be used for highly selective separation of SO2 in various concentrations and compositions. The deep eutectic solvent uses imidazole halide as a hydrogen bond acceptor and polyols as a hydrogen bond donor, which are mixed at a certain temperature in a specific ratio. The prepared deep eutectic solvent and a polymer matrix with good compatibility are used to prepare a separation membrane material by a solution casting method. The SO2 separation membrane of the present invention has the advantages of simple preparation, low cost, good stability, large permeation flux, good selectivity, etc.

[0007] The hydrogen bond acceptor and the hydrogen bond donor in the deep eutectic solvent are mixed in a specific ratio at a certain temperature, wherein the molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is 1:0.2 to 1:5, and the temperature is room temperature to 80°C.

[0008] The polymer matrix is ​​characterized in that the polymer is selected from one of polyvinylidene fluoride, polyether sulfone, polyether block polyamide, and poly(vinylidene fluoride-co-hexafluoropropylene).

[0009] The separation membrane is prepared by blending the deep eutectic solvent based on ionic liquid with a polymer matrix, and is characterized in that the mass ratio of the deep eutectic solvent to the polymer matrix is ​​1:0.5 to 1:20.

[0010] The deep eutectic solvent is blended with a polymer matrix to prepare a SO2 separation membrane, which is characterized in that the preparation method is a solution casting method, such as spin coating, blade coating and dip coating, and the prepared membrane morphology includes homogeneous membranes and thin layer composite membranes, and the application methods include but are not limited to flat membranes, hollow fiber membranes and rolled membranes.

[0011] The selective separation of the mixed gas containing SO2 is characterized in that the pressure of the feed gas is 0.1-5MPa, the volume concentration of SO2 is 0-20%, and the separation temperature is room temperature to 100°C.

[0012] The deep eutectic solvent is made of imidazolium halide as a hydrogen bond donor, characterized in that the imidazolium halide includes 1-octyl-3-methylimidazolium chloride, 1-hexyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium chloride, 1-octyl-3-methylimidazolium bromide, 1-hexyl-3-methylimidazolium bromide, 1-butyl-3-methylimidazolium bromide, 1-ethyl-3-methylimidazolium bromide and binary or multinary mixtures thereof.

[0013] The deep eutectic solvent is composed of a polyol as a hydrogen bond donor, characterized in that the polyol includes ethylene glycol, diethylene glycol, tetraethylene glycol, polyethylene glycol 200, polyethylene glycol 400, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, glycerol and tetraethylene glycol and their binary or multi-component mixtures.

[0014] The solution casting method is characterized in that 1 to 20 wt.% of a polymer is first dissolved in a solvent, and the resulting mixture is continuously stirred at 50 to 120°C until a clear and uniform solution is obtained. Next, a predetermined amount of DES is added to the above solution, and the mixture is continuously stirred at 50 to 120°C for 4 hours to obtain a casting solution. After cooling to room temperature, the casting solution is cast on an ultra-flat glass culture dish. Finally, most of the solvent is evaporated at room temperature to 80°C, and then the solvent is completely evaporated under vacuum conditions at 50 to 120°C to obtain the desired SO2 separation membrane.

[0015] The solvent is characterized in that the selected solvent must be able to dissolve the polymer and the deep eutectic solvent at the same time, specifically including deionized water, anhydrous ethanol, acetone, tetrahydrofuran, ethyl acetate, acetic acid, N,N-dimethylformamide, N,N-dimethylacetamide and their binary or multi-component mixtures. DETAILED DESCRIPTION

[0016] The technical solution of the present invention is further described below through specific embodiments.

[0017] Case Study 1 Preparation of SO2 Membrane Separation Active Component-Deep Eutectic Solvent System

[0018] The SO2 membrane separation active component-deep eutectic solvent system was prepared by the following methods, as follows:

[0019] 1) 1-Hexyl-3-methylimidazolium chloride and ethylene glycol are heated and stirred at 60° C. in a molar ratio of 1:1 until the mixed system becomes a clear and transparent liquid, and then cooled to room temperature to obtain a deep eutectic solvent, which is recorded as [Hmim]Cl-EG 1-1.

[0020] 2) 1-Hexyl-3-methylimidazolium chloride and butanediol are heated and stirred at 60° C. in a molar ratio of 1:2 until the mixed system becomes a clear and transparent liquid, and then cooled to room temperature to obtain a deep eutectic solvent, which is recorded as [Hmim]Cl-DEG 1-2.

[0021] 3) 1-ethyl-3-methylimidazolium bromide and ethylene glycol are heated and stirred at 60° C. in a molar ratio of 1:1 until the mixed system becomes a clear and transparent liquid, and then cooled to room temperature to obtain a deep eutectic solvent, which is recorded as [Emim]Br-EG 1-1.

[0022] 4) 1-Butyl-3-methylimidazolium bromide and diethylene glycol are heated and stirred at 60° C. in a molar ratio of 1:2 until the mixed system becomes a clear and transparent liquid, and then cooled to room temperature to obtain a deep eutectic solvent, which is recorded as [Bmim]Br-DEG 1-2.

[0023] Example 2 Preparation of polymer membrane for selective separation of SO2

[0024] The polymer membranes for selectively separating SO2 were prepared by the following solution casting method, as follows:

[0025] 1) Polyvinylidene fluoride (5wt.%, PVDF for short) powder is first dissolved in acetone solvent, and the resulting mixture is continuously stirred at 50°C until a clear and uniform solution is obtained. Then, DES (50wt.%) is added to the above solution, and the mixture is continuously stirred at 50°C for 4 hours to obtain a casting solution. After cooling to room temperature, the casting solution is cast on an ultra-flat glass culture dish. Finally, most of the solvent is evaporated at room temperature, and then the solvent is completely evaporated under vacuum conditions at 50°C to obtain the desired self-supporting homogeneous membrane, which is recorded as PVDF / DES 50%, where 50% is the mass percentage of DES to PVDF.

[0026] 2) Polyether block polyamide MH1657 (5wt.%, abbreviated as Pebax) particles are first dissolved in an ethanol / water (70 / 30wt.%) mixed solvent, and the resulting mixture is continuously stirred at 60°C until a clear and uniform solution is obtained. Then, DES (80wt.%) is added to the above solution, and the mixture is continuously stirred at 60°C for 4 hours to obtain a casting solution. After cooling to room temperature, the casting solution is cast on an ultra-flat glass culture dish. Finally, most of the solvent is evaporated at 40°C and a water content of 20%, and then the solvent is completely evaporated at 50°C under vacuum conditions to obtain the desired self-supporting homogeneous membrane, recorded as Pebax / DES 80%, where 80% is the mass percentage of DES in Pebax.

[0027] 3) Polyethersulfone powder (5wt.%, abbreviated as PES) particles are first dissolved in N, N-dimethylformamide solvent, and the resulting mixture is continuously stirred at 80°C until a clear and uniform solution is obtained. Then, DES (50wt.%) is added to the above solution, and the mixture is continuously stirred at 80°C for 4 hours to obtain a casting solution. After cooling to room temperature, the casting solution is cast on an ultra-flat glass culture dish. Finally, most of the solvent is evaporated at 60°C, and then the solvent is completely evaporated under vacuum conditions at 100°C to obtain the desired self-supporting homogeneous membrane, which is recorded as PES / DES 50%, where 50% is the mass percentage of DES to PES.

[0028] Implementation Case 3 According to the SO2 separation membrane prepared in Implementation Case 2, the corresponding separation data was obtained under certain test conditions. The specific results are shown in the following table:

[0029]

[0030] The above are only preferred embodiments of the present invention. The protection scope of the present invention is not limited to the above implementation cases. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should be regarded as the protection scope of the present invention.

Claims

1. A deep eutectic solvent / polymer membrane material for SO2 selective separation, characterized in that The membrane material is prepared by blending a class of deep eutectic solvents based on imidazolium halide salts with a polymer matrix, and can be used to separate SO2 in flue gases of various concentrations and compositions with high selectivity (SO2 / CO2 and SO2 / N2) and high stability.

2. A deep eutectic solvent / polymer membrane material for SO2 selective separation according to claim 1, characterized in that The deep eutectic solvent is synthesized by using imidazolium halide ionic liquid as hydrogen bond acceptor and polyol as hydrogen bond donor according to the molar ratio of hydrogen bond acceptor to hydrogen bond donor of 1:0.2 to 1:5 and the temperature of room temperature to 80°C.

3. A deep eutectic solvent / polymer membrane material for SO2 selective separation according to claim 1, characterized in that The polymer is one of polyvinylidene fluoride, polyether sulfone, polyether block polyamide and poly(vinylidene fluoride-co-hexafluoropropylene).

4. A deep eutectic solvent / polymer membrane material for SO2 selective separation according to claim 1, characterized in that The mass ratio of the deep eutectic solvent to the polymer matrix is ​​1:0.5 to 1:

20.

5. A deep eutectic solvent / polymer membrane material for SO2 selective separation according to claim 1, characterized in that The preparation method is solution casting, such as spin coating, blade coating and dip coating. The prepared membrane morphology includes homogeneous membrane and thin layer composite membrane. The application methods include but are not limited to flat membrane, hollow fiber membrane and rolled membrane.

6. A deep eutectic solvent / polymer membrane material for SO2 selective separation according to claim 1, characterized in that The pressure of the feed mixed gas containing SO2 is 0.1-5 MPa, the volume concentration of SO2 is 0-20%, and the separation temperature is room temperature to 100°C.

7. A deep eutectic solvent / polymer membrane material for SO2 selective separation according to claim 2, characterized in that Imidazolium halide ionic liquids include 1-octyl-3-methylimidazolium chloride, 1-hexyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium chloride, 1-octyl-3-methylimidazolium bromide, 1-hexyl-3-methylimidazolium bromide, 1-butyl-3-methylimidazolium bromide, 1-ethyl-3-methylimidazolium bromide and binary or multinary mixtures thereof.

8. A deep eutectic solvent / polymer membrane material for SO2 selective separation according to claim 2, characterized in that The polyols include ethylene glycol, diethylene glycol, tetraethylene glycol, polyethylene glycol 200, polyethylene glycol 400, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, glycerol, tetraethylene glycol and binary or polyvalent mixtures thereof.

9. A deep eutectic solvent / polymer membrane material for SO2 selective separation according to claim 5, characterized in that The solution casting method is to first dissolve 1 to 20 wt.% of the polymer in a solvent, and continuously stir the resulting mixture at 50 to 120°C until a clear and uniform solution is obtained. Next, a predetermined amount of DES is added to the above solution, and the mixture is continuously stirred at 50 to 120°C for 4 hours to obtain a casting solution. After cooling to room temperature, the casting solution is cast on an ultra-flat glass culture dish. Finally, most of the solvent is evaporated at room temperature to 80°C, and then the solvent is completely evaporated under vacuum conditions at 50 to 120°C to obtain the desired SO2 separation membrane.

10. A deep eutectic solvent / polymer membrane material for SO2 selective separation according to claim 9, characterized in that The selected solvent needs to be able to dissolve the polymer and the deep eutectic solvent at the same time, specifically including deionized water, anhydrous ethanol, acetone, tetrahydrofuran, ethyl acetate, acetic acid, N,N-dimethylformamide, N,N-dimethylacetamide and binary or multi-component mixtures thereof.