Die-casting pouring method for solving shrinkage of middle air hole of multi-cylinder body product
By controlling the cylinder filling sequence and cross-splitting flow through the bilateral pouring runner, the problem of air hole shrinkage in the thick plate between the middle wall of the multi-cylinder cylinder is solved, and the compactness and mechanical properties of the cylinder are significantly improved.
Patent Information
- Application Number
- CN202411137496.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
It is difficult for traditional die-casting technology to set up effective exhaust channels at the thick wall plates in the middle of multi-cylinder cylinders, resulting in frequent defects in air holes and shrinkage holes, affecting the density and mechanical properties of the cylinder.
The double-sided pouring runner is adopted. By controlling the discharge flow and flow rate of the cross-sort, the cylinder block is filled in order in order in multiple cylinders. The metal liquid is preferred to intersect at the thick wall plate to ensure that the gas is discharged in time and reduce pores and pores. Generation of shrink holes.
It effectively avoids the gas sealing problem caused by filling hysteresis of wall thick plates, significantly reduces the probability of air holes and shrinkage holes in the middle after casting, and improves the density and mechanical properties of the cylinder.
Smart Images

Figure CN119016704A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of die casting, and in particular to a die casting pouring method for solving the problem of shrinkage holes in the middle of a multi-cylinder cylinder body product. Background Art
[0002] The engine block, as the cornerstone of the power core, has a manufacturing quality that is directly related to the performance of the engine and even the entire vehicle. The density and mechanical strength of the cylinder block are not only the cornerstones of the efficient operation of the engine, but also the key indicators for measuring the life and reliability of the engine. However, the complex internal structure of the cylinder block, the significant difference in wall thickness, and the dense heat dissipation rib design together constitute an insurmountable challenge in the casting process, which can easily induce various casting defects and seriously restrict the improvement of engine performance.
[0003] Taking the cylinder block of a four-cylinder engine as an example, the traditional casting process often adopts a single-side feeding method, such as the attachment of patent announcement number CN208811031U "A double-side feeding casting system for engine cylinder block" Figure 1 Although the disclosed single-sided pouring system can achieve initial molding, product defects frequently occur and it is difficult to meet the stringent requirements of modern engines for cylinder quality. To this end, industry experts explored the bilateral synchronous pouring technology, which is the attached patent of the public patent. Figure 2 The solution shown is intended to overcome the limitation of unilateral pouring and improve casting quality through balanced material distribution.
[0004] However, even with bilateral synchronous pouring, it is still difficult to overcome the problem of casting the thick wall plate located in the center of the cylinder body. The thick wall plate not only bears the heavy task of separating multiple cylinders, but also due to its structural characteristics - large thickness, central position, and holes in different directions - the traditional process cannot set an effective exhaust channel at the thick wall plate. In addition, the wall plate is deep, and even under bilateral pouring conditions, there are still common defects such as pores and shrinkage holes after casting, which seriously affects the density and mechanical properties of the cylinder body, becoming a bottleneck restricting the development of cylinder body die-casting technology, and a problem that the current industry urgently needs to solve. Summary of the invention
[0005] The present invention aims to provide a die-casting pouring method for solving the problem of pores and shrinkage holes in the middle of a multi-cylinder cylinder body product, so as to solve the problem that pores and shrinkage holes are easily generated in the thick wall plate in the middle of the multi-cylinder cylinder body.
[0006] In order to achieve the above object, the present invention adopts the following technical scheme:
[0007] A die-casting pouring method for solving the problem of shrinkage of the middle pores of a multi-cylinder body product requires the use of a double-sided pouring runner, which includes a main runner symmetrically connected to a feed port, and a plurality of cross runners arranged along the extension direction of the main runner, and all the cross runners are connected to the main runner;
[0008] Control the discharge flow rate of the runner on the same side to change in sequence along the multi-cylinder arrangement direction, so that the cylinder cavity is filled in sequence according to the multi-cylinder arrangement order;
[0009] When pouring the same pair of runners, priority is given to ensuring that the molten metal meets at the wall thick plate, and then meets at the bottom area where the wall thick plates are connected.
[0010] The principle and advantage of this scheme are as follows: the inventor studied the existing double-sided pouring method and found that due to the fast flow speed of the molten metal in the main runner, the molten metal in the main runner will quickly fill the cylinder cavity to improve production efficiency, but the molten metal on the left and right sides of each cylinder will quickly converge to the middle under the fast filling, especially quickly converge to the bottom area of the thick wall plate and block the exhaust path of the gas in the cavity where the thick wall plate is located, especially for the case where the thick wall plate is not only thick but also deep, the gas that cannot be discharged will eventually gather in the area of the thick wall plate where the molten metal is filled later, causing pores and shrinkage holes in the thick wall plate.
[0011] This solution controls the flow rate and flow rate of the cross runner so that when the cylinder body is cast, it is filled sequentially along the multi-cylinder arrangement order of the cylinder body, thereby avoiding the situation where the synchronous filling of all cylinders hinders the discharge of gas. The sequential filling form of this solution allows the gas in the cavity to move to the side of the cylinder filled last and be discharged, ensuring that more gas can be discharged, reducing the probability of gas staying in the cavity and causing pores and shrinkage holes; and controlling the thick wall plate to be poured first can ensure that the gas in the thick wall plate is discharged first, effectively avoiding the gas sealing problem caused by delayed filling of the thick wall plate, significantly promoting the timely discharge of gas, and thereby greatly reducing the probability of pores and shrinkage holes in the thick wall plate in the middle position after the casting is formed.
[0012] Preferably, as an improvement, the cross-sectional area of the runner closest to the feed port is the largest, so that when the cylinder body cavity is filled, the cylinder closest to the feed port is filled first.
[0013] Preferably, as an improvement, the main runner is wavy in shape, and each fork of the main runner is connected to a cross runner. The discharge direction of the main runner at the fork is toward the cross runner, so that the molten metal on the main runner at the fork will preferentially enter the cross runner, thereby ensuring that the cross runner closer to the feed port has a larger flow rate, and when the flow rate and cross-section are large, the discharge pressures of the inner gates of each cross runner tend to be consistent.
[0014] Preferably, as an improvement, the main runner is stepped along the discharge extension direction, and each step starts from a fork position. The steps are arranged so that the length and width of the cross-sectional width of the step gradually decrease as it is farther away from the feed port. This solution arranges steps at the fork so that each step forms an obstruction to the molten metal, thereby allowing more molten metal to flow preferentially to the cross runner connected to the fork, thereby ensuring that the casting cavities are filled sequentially.
[0015] Preferably, as an improvement, the wavy main runner includes a primary main runner, a secondary main runner ... N-level main runners, and except for the primary main runner, the remaining main runners all have corners to reduce vortex air entrainment.
[0016] Preferably, as an improvement, the discharge angle of the inner gate of the cross runner is consistent with the inclination angle of the cavity wall of the cylinder body, and the inner gate is an outward expansion structure. The outward expansion structure of the inner gate makes the distance between adjacent cross runner discharge ports smaller as it is closer to the cylinder body.
[0017] Beneficial effect: This solution allows the molten metal to diffuse from the inner gate to the outward direction when the cross runner is discharged, and the diffusion direction makes the discharge of two adjacent cross runners tend to approach each other, so that the thick wall plate located between adjacent cross runners can be filled first, effectively avoiding the gas sealing problem caused by delayed filling of the thick wall plate, significantly promoting the timely discharge of gas, and thus greatly reducing the generation of pores and shrinkage holes after casting.
[0018] Preferably, as an improvement, the runner is V-shaped with an angle greater than 90°, and a shrinkage compensation area is provided on the side of the inner gate of the runner. The shrinkage compensation area has a gradual wedge-shaped structure, and the shrinkage compensation area transitions from the V-shaped corner of the runner to the discharge end close to the inner gate, and the side of the shrinkage compensation area close to the discharge end of the inner gate is also transitionally connected to the inner gate.
[0019] Beneficial effect: In this scheme, the cross-section of the feeding area is designed to be a gradual wedge-shaped structure, so that the feeding area can preheat the molten metal of the ingate, avoiding the situation where the molten metal is cooled due to the excessive length of the ingate of the V-shaped structure in the cross runner, which helps to maintain the heat flow temperature at the discharge end of the ingate and prevents excessive cooling. At the same time, the flat and narrow structure of the feeding area and the ingate helps to increase pressure for feeding, effectively inhibit the formation of shrinkage defects, and improve the quality and mechanical properties of castings.
[0020] Preferably, as an improvement, the number of cross runners located on the same side is one less than the number of cylinders of the formed cylinder body, so that the cylinder farthest from the feed port has no corresponding cross runner, thereby ensuring that the cylinder cavity farthest from the feed port is filled with molten metal in the end, thereby avoiding the situation where when a negative pressure suction exhaust duct is set at the edge of the cylinder body, the negative pressure will draw away the molten metal closest to the cylinder cavity and block the exhaust duct, which helps to further reduce the probability of pores and shrinkage holes and improve the quality of the cylinder body after casting.
[0021] Preferably, as an improvement, the double-sided pouring runner adopted for pouring is arranged vertically so that all the cross runners on the same side are arranged at different heights, and the feed port is located at the bottom, so that the entire molding process is fed from the bottom, which facilitates the gas in the cavity to be gradually driven away from the top, and the gas accidentally drawn into the molten metal can also gradually escape from the molten metal due to the different densities of the molten metal and the gas, further reducing the probability of pores and shrinkage holes.
[0022] Preferably, as an improvement, when the molten metal is poured, the exhaust duct provided on the die-casting mold simultaneously performs negative pressure suction, so that the gas is driven away by the inflowing molten metal on the one hand, and is also sucked away under negative pressure on the other hand, which helps to increase the filling speed and speed up the discharge of gas, and is also beneficial for the negative pressure to help the gas to be discharged from the molten metal after the gas is drawn in, thereby effectively reducing the probability of pores and shrinkage holes. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of a three-dimensional structure of an embodiment of the present invention.
[0024] Figure 2 for Figure 1 Schematic diagram of the three-dimensional structure after adjusting the viewing angle.
[0025] Figure 3 for Figure 2 Top view of the .
[0026] Figure 4 for Figure 3 AA section view in.
[0027] Figure 5 for Figure 2 Front view of.
[0028] Figure 6 for Figure 1 A schematic diagram of the three-dimensional structure in which the cylinder block is not shown and only the runner and exhaust channel are shown.
[0029] Figure 7 for Figure 6 Schematic diagram of the three-dimensional structure after adjusting the viewing angle (the direction of the arrow in the figure indicates the direction of negative pressure suction).
[0030] Figure 8 for Figure 6 Only the three-dimensional structure diagram of the double-sided pouring runner is shown.
[0031] Fig. 9 for Figure 8 Schematic diagram of the three-dimensional structure after adjusting the viewing angle.
[0032] Fig.10 for Fig. 9 Top view.
[0033] Fig.11 for Fig. 9 Right view of .
[0034] Fig.12 for Fig. 9 Front view of.
[0035] Figure 13-Figure 20 It is a schematic diagram of the simulation of the flow of molten metal during the die casting pouring process of the present embodiment (also called a mold flow analysis diagram).
[0036] Fig.13 It is a schematic diagram of the molten metal when it is diverted at the fork of the primary main runner (it can be clearly seen in the figure that when the fork is diverted, the discharge of the primary main runner preferentially flows to the cross flow channel connected to the fork position).
[0037] Fig.14 It is a schematic diagram of three symmetrical pairs of cross runners when all the materials are discharged (it is clearly seen in the figure that when the discharge between two adjacent cross runners is diffused, the discharge is close to each other so as to preferentially fill the thick wall plate).
[0038] Fig.15 Schematic diagram of the thick wall plate filled with molten metal flowing into the runner (it is clearly seen in the figure that the thick wall plate is filled first, and the amount filled is also the largest in the area where the lowest cylinder is located).
[0039] Fig.16 This is a schematic diagram showing that the area where the lowest cylinder is located is basically filled, while the remaining cylinders are not filled (it is obvious from the figure that the filling area of the four cylinders from bottom to top becomes smaller as the cylinders go up, which shows that the cavity filling follows the order from bottom to top).
[0040] Fig.17 It is a schematic diagram of the remaining two cylinders that are not filled (in the figure, after the area of the cylinder at the bottom (closest to the feed port) is filled, the molten metal squeezes out to the slag bag area, and at this time the area of the cylinder at the top (farthest from the feed port) has not yet been filled).
[0041] Fig.18 This is a schematic diagram of all cylinders being basically filled (in the figure, after all cylinders are basically filled, the slag bag / exhaust channel are not yet filled, which is convenient for continuing to fill the material to allow the molten metal to shrink).
[0042] Fig.19Schematic diagram of the process of molten metal entering the slag bag area connected to the end of the cylinder.
[0043] Fig. 20 This is a schematic diagram showing that the exhaust channel is also filled with molten metal, and the pouring is now completed.
[0044] Figure 21-Figure 25 As a comparative example, the mold flow analysis diagram of the runner of the present embodiment is a preliminary optimization based on the existing technical solution. The difference between the runner of the present embodiment and the main runner is a conventional straight runner, the number of cross runners is the same as the conventional number, and the cross runner does not have a necking, a discharge flaring, a shrinkage-feeding area, etc. Figure 21 to Figure 24 Screenshots taken at different time points / positions for the same solution and the same mold flow analysis.
[0045] Fig.21 This is a screenshot of the mold flow analysis shortly after the comparative example was poured (it is clearly seen from the figure that the molten metal in the main runner moves quickly. When the runner closest to the gate is not yet filled, the molten metal has moved to the end of the main runner).
[0046] Fig. 22 For Fig.21 Screenshot of mold flow analysis after continued pouring (the figure clearly shows that the flow rate is: the flow rate of the runner farthest from the feed port > the flow rate of the middle runner > the flow rate of the runner closest to the feed port).
[0047] Fig.23 For Fig. 22 The top view of the mold flow after continued pouring (the figure shows that the end cylinder fills the fastest).
[0048] Fig.24 For Fig.23 The top view screenshot of the mold flow after continued pouring (it is clearly seen from the figure that the filling speeds in different cylinder areas are different, and the flow rates in the cylinder during filling are also different. It is expected that the mechanical properties of different areas of the cylinder body after molding will be greatly different).
[0049] Fig.25 For Fig.24 The top view screenshot of the mold flow after continued pouring (it is clearly seen from the figure that when pouring is nearing the end, the flow velocities in different areas between the cylinders are still different, and the flow rate is still greater the farther away from the gate). DETAILED DESCRIPTION
[0050] The following is further described in detail through specific implementation methods:
[0051] The figure marks in the drawings of the specification include: feed port 1, main runner 2, primary main runner 21, secondary main runner 22, tertiary main runner 23, cross runner 3, connecting section 31, inner gate section 32, inner gate 321, shrinkage compensation area 322, exhaust channel 4, slag bag area 41, cylinder body 10, and wall thickness plate 101.
[0052] The embodiment is basically as shown in the attached Figures 1 to 20 shown.
[0053] The embodiment provides a double-sided pouring runner, including a feed port 1 and a main runner 2 symmetrically arranged about the feed port 1, the feed port 1 is located at the lowermost end, the feed port 1 is located on the central axis of the cylinder body 10, the main runner 2 is symmetrical about the central axis, the main runner 2 extends from bottom to top, and a plurality of cross runners 3 are arranged along the height direction of the main runner 2, all the cross runners 3 are connected to the main runner 2, and along the height direction, the cross runner 3 has a larger cross-sectional area as it goes downward, and the specific detailed designs of the main runner 2 and the cross runner 3 are as follows:
[0054] 1. Design of main runner 2: The main runner 2 is designed to be in a wave shape, with a fork formed at the connection of each wave. The fork is connected to the runner 3. The runner 3 is located in the discharge direction of the main runner 2 on each waveform. The feed port 1 of the runner 3 is in the same direction as the discharge direction of the main runner 2 of each waveform. The feed direction of the next adjacent waveform is different from the discharge direction of the previous waveform and forms a V-shape with the opening away from the runner 3, so as to ensure that the molten metal output from each waveform enters the connected runner 3 first, and ensure that the runner 3 closer to the feed port 1 has a larger flow rate.
[0055] Secondly, in order to ensure the flow rate in each waveform, the discharge center line of the previous waveform is directly opposite to the feed center of the next waveform to ensure that a certain amount of molten metal can enter the next waveform when it hits the corner of the next waveform and the cross runner 3.
[0056] In order to increase the tendency of the molten metal to flow to the runner 3 and ensure the sequential filling of the cavity, the main runner 2 is set in a stepped shape along the discharge direction, each step starts from a fork, that is, each step corresponds to a waveform, and the length and width of the step cross section away from the feed port 1 gradually decrease. In this embodiment, the number of runners 3 is three pairs, the cylinder body 10 to be processed has four cylinders (including 5 thick wall plates 101 in the middle), and the wavy main runner 2 is divided into a primary main runner 21, a secondary main runner 22 and a tertiary main runner 23. Except for the primary main runner 21, the other two main runners 2 have a corner design to reduce vortex air entrainment, thereby reducing the formation of pores / shrinkage cavities.
[0057] 2. Design of the runner 3: The runner 3 itself is in a V-shape with an angle greater than 90°. The runner 3 includes a connecting section 31 parallel to the main runner 2 and an inner gate section 32 inclined toward the end face of the cylinder cavity 10. The connecting section 31 is transitionally connected with the inner gate section 32, and the inner gate section 32 and the connecting section 31 are in a V-shape greater than 90°. The connection between the runner 3 and the main runner 2 adopts a necking structure, and the discharge end, that is, the inner gate section 32, gradually expands outward, and the expansion direction points to the direction of the inner gate section 32 of the adjacent runner 3, so that the discharge of each inner gate 321 tends to diffuse and converge toward the side runner 3, ensuring that the molding area of the thick-walled plate 101 can have the adjacent runner 3 injected with molten metal at the same time, thereby ensuring the priority of pouring in the thick-walled plate 101 area, greatly reducing or even avoiding the probability of air holes / shrinkage holes in the thick-walled plate 101.
[0058] In order to further optimize the runner structure, a gradual wedge-shaped compensation area 322 is provided on the outer side of the inner gate section 32 toward the cylinder body 10 to prevent the molten metal from cooling down too quickly in the inner gate section 32. At the same time, the compensation area 322 makes the overall cross-sectional area of the inner gate section 32 change from large to small, and then suddenly shrinks at the discharge end, thereby facilitating pressurization compensation.
[0059] The inclination angle of the ingate segment 32 matches the inclination angle of the cavity wall, and the end ingate 321 of the ingate segment 32 is inclined toward the middle of the cavity end surface.
[0060] The number of runners 3 is one pair less than the number of cylinders in the cylinder body 10, ensuring that the cylinder cavity farthest from the feed port 1 is filled last to avoid blockage of the exhaust channel 4.
[0061] In order to ensure that the cylinder cavity portion closest to the feed port 1 is filled and that the thick wall plate 101 in the middle of the end is filled first, in this embodiment, the line connecting the inner gates 321 of a pair of cross runners 3 with the largest cross-sectional area covers the thick wall plate 101 at the edge of the cylinder body 10, ensuring that the area of the thick wall plate 101 at the edge is filled first to reduce gas retention.
[0062] The middle pair of runners 3 are located between adjacent thick-walled plates 101 , and the pair of runners 3 with the smallest cross-sectional area is close to the penultimate thick-walled plate 101 .
[0063] This embodiment also provides a die-casting pouring method to solve the problem of shrinkage holes in the middle of multi-cylinder cylinder products, which requires the use of the above-mentioned double-sided pouring runner. When pouring castables into the cavity of the cylinder body 10, the multiple cylinders of the cylinder body 10 are arranged in the height direction, and the discharge flow of the horizontal runner 3 on the same side is controlled to change from bottom to top in sequence to ensure that the cylinder body 10 cavity is filled in sequence from bottom to top. When the cylinder body 10 is die-cast, the exhaust channel 4 is connected to multiple slag bag areas 41. The slag bag area 41 is set at the bottom or end of the molded cylinder body 10 away from the pouring channel. In this embodiment, the exhaust channel 4 is Figure 1There are exhaust ducts 4 around the back of the cylinder body, and there are also exhaust ducts 4 around the top of the cylinder body where the cylinder body is finally formed. The exhaust ducts 4 are connected to the slag bag area 41. In addition, there are exhaust ducts 4 at the bottom of the cylinder body, and the exhaust ducts 4 are also connected to multiple slag bag areas 41. Before the cavity is completely filled, the molten metal entering from the primary main runner 21 with the largest cross-sectional area not only diffuses upward but also diffuses downward, thereby ensuring that the temperature difference between the upper and lower parts of the cavity is small under sequential filling, avoiding the problem of local temperature cooling too fast and affecting the casting quality; and avoiding the problem that the cavity area filled first at the lower part of the cylinder body is over-pressurized, which is not conducive to improving the life of the die-casting mold.
[0064] In order to increase the exhaust speed and exhaust volume of the gas in the cavity, the exhaust channel 4 adopts negative pressure suction during the pouring process of the die casting.
[0065] At the same time, when pouring the same pair of cross runners 3, due to the wave design and step design of the main runner 2 and the outward expansion structure design of the cross runner 3, after the metal is hot poured into the same pair of cross runners 3, the molten metal first converges at the thick wall plate 101, and then converges at the bottom area connected to the thick wall plate 101, thereby ensuring that the thick wall plate 101 area is filled before the bottom area, ensuring that the gas in the thick wall plate 101 can be discharged in time, greatly reducing or even avoiding the generation of pores or shrinkage cavities in the thick wall plate 101, ensuring the lethality and mechanical properties of the cylinder body 10, and breaking the bottleneck that the performance of the cylinder body 10 cannot be improved after die-casting.
[0066] To verify this design, the mold flow analysis of this embodiment and the comparative example was compared. Figures 13 to 20 This is a screenshot of the mold flow analysis of the embodiment. Figure 21 to Figure 25 This is a screenshot of the mold flow analysis of the comparative example. The information shown in the specific figure has been explained in the figure description and will not be repeated here.
[0067] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A die-casting pouring method for solving the problem of shrinkage of the middle pores in a multi-cylinder body product, which requires the use of a double-sided pouring runner, which includes a main runner symmetrically connected to a feed port, and a plurality of cross runners arranged along the extension direction of the main runner, and all the cross runners are connected to the main runner; characterized in that: Control the discharge flow rate of the runner on the same side to change in sequence along the multi-cylinder arrangement direction, so that the cylinder cavity is filled in sequence according to the multi-cylinder arrangement order; When pouring the same pair of runners, priority is given to ensuring that the molten metal meets at the wall thick plate, and then meets at the bottom area where the wall thick plates are connected.
2. A die-casting pouring method for solving the problem of middle pore shrinkage in multi-cylinder products according to claim 1, characterized in that: The cross-sectional area of the runner closest to the feed port is the largest, so that when the cylinder cavity is filled, the cylinder closest to the feed port is filled first.
3. A die-casting pouring method for solving the problem of middle pore shrinkage in multi-cylinder products according to claim 2, characterized in that: The main runner is wavy in shape, and each fork of the main runner is connected to a cross runner, and the discharge direction of the main runner at the fork is toward the cross runner.
4. A die-casting pouring method for solving the problem of middle pore shrinkage in multi-cylinder products according to claim 3, characterized in that: The main runner is stepped along the direction of material discharge, each step starts from a fork position, and the steps are arranged so that the length and width of the cross-sectional width of the step farther away from the feed port gradually decrease.
5. The die-casting pouring method for solving the problem of middle pore shrinkage in multi-cylinder products according to claim 3, characterized in that: The wavy main runner includes a primary main runner, a secondary main runner ... N-level main runners, and except for the primary main runner, the remaining main runners all have corners.
6. The die-casting pouring method for solving the problem of middle pore shrinkage in multi-cylinder products according to claim 3, characterized in that: The discharge angle of the ingates of the runner is consistent with the inclination angle of the cavity wall of the cylinder body, and the ingates are outwardly expanded. The outward expansion structure of the ingates makes the distance between adjacent ingates of the runner smaller the closer to the cylinder body.
7. A die-casting pouring method for solving the problem of middle pore shrinkage in multi-cylinder products according to claim 6, characterized in that: The runner is V-shaped with an angle greater than 90°, and a shrinkage compensation area is provided on the side of the inner gate of the runner. The shrinkage compensation area has a gradual wedge-shaped structure. The shrinkage compensation area transitions from the V-shaped corner of the runner to the discharge end close to the inner gate, and the side of the shrinkage compensation area close to the discharge end of the inner gate is also transitionally connected to the inner gate.
8. The die-casting pouring method for solving the problem of middle pore shrinkage in multi-cylinder products according to claim 1, characterized in that: The number of runners located on the same side is one less than the number of cylinders of the molded cylinder body.
9. The die-casting pouring method for solving the problem of middle pore shrinkage in multi-cylinder products according to claim 1, characterized in that: The double-sided pouring runner is placed vertically so that all the horizontal runners on the same side are arranged at different heights, and the feed port is located at the bottom.
10. A die-casting pouring method for solving the problem of middle pore shrinkage in multi-cylinder products according to any one of claims 1 to 9, characterized in that: When the molten metal is poured in, the exhaust duct provided on the die-casting mold simultaneously performs negative pressure suction.
Citation Information
Patent Citations
Oblique pouring system and vacuum die-casting process
CN116900272A
Pouring passage system of automobile die-casting parts
CN202377511U
Die -casting cylinder body waters based on prevent device that splits
CN205967351U
Double-side pouring type pouring system for engine cylinder body
CN208811031U
The invention discloses a pouring system for vacuum die casting of a special-shaped optical fiber module
CN208895146U
Cited By
Die-casting die for aluminum alloy connecting support of new energy automobile
CN119973076A
A die-casting mold for an aluminum alloy connecting bracket for new energy vehicles
CN119973076B