Ethylene-alpha-olefin copolymer and preparation method thereof

By using metallocene olefin polymerization catalyst and cocatalyst for copolymerization reaction in the presence of hydrogen, ethylene-α-olefin copolymers that meet specific parameters are prepared, which solves the difficulty of ethylene-α-olefin copolymers in the prior art to have high melting in both the prior art The problems of body flow rate, excellent tensile strength, and elongation at break have achieved higher mechanical properties and wide application prospects.

CN119019589APending Publication Date: 2024-11-26BEOYI (SHANDONG) NEW MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411369881.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing ethylene-α-olefin copolymers are difficult to have excellent tensile strength and elongation of break while meeting the high melt flow rate.

Method used

By copolymerizing reaction using metallocene olefin polymerization catalyst and cocatalyst in the presence of hydrogen, ethylene-α-olefin copolymers that meet specific formula parameters are prepared, including optimized melt index, melt flow activation energy, melt tension, and intrinsic viscosity. , copolymers of chain length and characteristic relaxation time.

Benefits of technology

On the basis of high melt flow rate, the ethylene-α-olefin copolymer has significantly improved the tensile strength and elongation of break, and has simple process and easy control of conditions, and has broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides an ethylene-alpha-olefin copolymer, which has a melt index of 0.1-100g / 10min and melt flow activation energy greater than or equal to 50kJ / mol, and MT, [eta], A and tau meet the following formula: 2.1 * MFR-0. 59 lt; mTlt; 18 * MFR-0. 59 is adopted; 1.03 * MFR <-0.094 lt >; [eta] lt; 1.52 * MFR < 0.156 > is adopted; log A is greater than or equal to-0.0815 * log (MFR) + 4.06; tau is greater than or equal to 8.15 * MFR-0.746; wherein MFR is melt index, MT is 190 DEG C melt tension, [eta] is intrinsic viscosity, A is chain length, and tau is characteristic relaxation time. Compared with the prior art, the ethylene-alpha-olefin copolymer provided by the invention meets specific index parameter limit requirements, and not only has high melt flow rate, but also has excellent tensile strength and elongation at break.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and more specifically to an ethylene-alpha-olefin copolymer and a preparation method thereof. Background Art

[0002] As a thermoplastic elastomer, ethylene-α-olefin copolymer has the dual characteristics of plastic and rubber. On the one hand, the narrow molecular weight distribution and short chain branches give it excellent physical and mechanical properties, such as high elasticity, high strength, high elongation and good low-temperature performance; on the other hand, its molecular chain is saturated and contains relatively few tertiary carbon atoms, so it has excellent resistance to heat, oxygen, aging and UV rays.

[0003] For example, CN100404564C discloses an ethylene copolymer comprising repeating units derived from ethylene and repeating units derived from α-olefins having 3 to 20 carbon atoms, wherein the melt flow rate is 1 to 100 g / 10 min, the melt flow activation energy is 60 kJ / mol or higher, the melt tension (MT) at 190°C, the intrinsic viscosity ([η]) and the chain length A satisfy a certain formula, wherein the chain length A is the chain length of the component with the highest molecular weight in the log-normal distribution curve at the peak of the log-normal distribution curve, the chain length distribution curve is determined by gel permeation chromatography, and the chain length distribution curve is divided into at least two log-normal distribution curves to obtain the log-normal distribution curve.

[0004] However, although the ethylene copolymer disclosed in the above technical solution has a high melt flow rate, it is difficult to meet the strength requirements, and thus the tensile strength and elongation at break need to be further improved. Summary of the invention

[0005] In view of this, an object of the present invention is to provide an ethylene-α-olefin copolymer and a preparation method thereof. The ethylene-α-olefin copolymer provided by the present invention has excellent tensile strength and elongation at break.

[0006] The present invention provides an ethylene-α-olefin copolymer having a melt index of 0.1 to 100 g / 10 min, a melt flow activation energy of 50 kJ / mol or more, and MT, [η], A and τ satisfying formulas (1) to (4):

[0007] 2.1×MFR -0.59 <MT<18×MFR -0.59 (1);

[0008] 1.03×MFR -0.094 <[η]<1.52×MFR -0.156 (2);

[0009] logA≥-0.0815×log(MFR)+4.06 (3);

[0010] τ≥8.15×MFR -0.746 (4);

[0011] Wherein, MFR is melt index, MT is melt tension at 190°C, [η] is intrinsic viscosity, A is chain length, and τ is characteristic relaxation time.

[0012] Preferably, the ethylene-α-olefin copolymer is an ethylene-α-olefin copolymer comprising repeating units derived from ethylene and repeating units derived from α-olefins having 3 to 20 carbon atoms; wherein the repeating units derived from ethylene account for 70 mol% to 99.9 mol%, and the repeating units derived from α-olefins having 3 to 20 carbon atoms account for 0.1 mol% to 30 mol%.

[0013] Preferably, the MFR is 1-30 g / 10 min, and the melt flow activation energy is 60 kJ / mol-100 kJ / mol.

[0014] Preferably, the MT, [η], A and τ satisfy the formula:

[0015] 2.3×MFR -0.59 <MT<13×MFR -0.59 ;

[0016] 1.06×MFR -0.094 <[η]<1.47×MFR -0.156 ;

[0017] logA≥-0.0815×log(MFR)+4.07;

[0018] τ≥8.25×MFR -0.746 .

[0019] Preferably, the SR and intrinsic viscosity of the ethylene-α-olefin copolymer satisfy formulas (5) to (6):

[0020] If [η] < 1.20,

[0021] -0.91×[η]+2.265<SR<2.1 (5);

[0022] If [η] ≥ 1.20,

[0023] 1.15<SR<2.1 (6);

[0024] Wherein, SR is the expansion ratio.

[0025] The present invention also provides a method for preparing the ethylene-α-olefin copolymer described in the above technical solution, comprising the following steps:

[0026] Ethylene and α-olefin are copolymerized in the presence of hydrogen using a metallocene olefin polymerization catalyst and a co-catalyst, and then filtered, washed and devolatilized in sequence to obtain an ethylene-α-olefin copolymer.

[0027] Preferably, the metallocene olefin polymerization catalyst is selected from dimethylsilyl bridge group-tetramethylcyclopentadienyl-tert-butylamino-titanium dichloride and / or dimethylsilyl bridge group-tetramethylcyclopentadienyl-tert-butylamino-dimethyltitanium.

[0028] Preferably, the co-catalyst is selected from one or more of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride, ethylaluminum dichloride, methylaluminoxane, modified methylaluminoxane, perfluorophenylboron, triphenylcarbon tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, and N,N-di(hexadecyl)anilinium tetrakis(pentafluorophenyl)borate.

[0029] Preferably, the copolymerization reaction is carried out at a temperature of 65° C. to 250° C., a pressure of 1 MPa to 15 MPa, and a time of 6 h to 10 h.

[0030] Preferably, the devolatilization method is oven vacuum heating; the temperature of the oven vacuum heating is 50°C to 100°C, the pressure is ≤-0.08MPa, and the time is ≥5h.

[0031] The present invention provides an ethylene-α-olefin copolymer having a melt index of 0.1 to 100 g / 10 min, a melt flow activation energy of 50 kJ / mol or more, and MT, [η], A and τ satisfying formulas (1) to (4):

[0032] 2.1×MFR -0.59 <MT<18×MFR -0.59 (1);

[0033] 1.03×MFR -0.094 <[η]<1.52×MFR -0.156 (2);

[0034] logA≥-0.0815×log(MFR)+4.06 (3);

[0035] τ≥8.15×MFR -0.746 (4);

[0036] Wherein, MFR is melt index, MT is melt tension at 190°C, [η] is intrinsic viscosity, A is chain length, and τ is characteristic relaxation time.

[0037] Compared with the prior art, the ethylene-α-olefin copolymer provided by the present invention meets the requirements of specific index parameters, and has not only a high melt flow rate, but also excellent tensile strength and elongation at break.

[0038] In addition, the preparation method provided by the present invention has simple process, easily controllable conditions and broad application prospects. DETAILED DESCRIPTION

[0039] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] The present invention provides an ethylene-α-olefin copolymer having a melt index of 0.1 to 100 g / 10 min, a melt flow activation energy of 50 kJ / mol or more, and MT, [η], A and τ satisfying formulas (1) to (4):

[0041] 2.1×MFR -0.59 <MT<18×MFR -0.59 (1);

[0042] 1.03×MFR -0.094 <[η]<1.52×MFR -0.156 (2);

[0043] logA≥-0.0815×log(MFR)+4.06 (3);

[0044] τ≥8.15×MFR -0.746 (4);

[0045] Wherein, MFR is melt index, MT is melt tension at 190°C, [η] is intrinsic viscosity, A is chain length, and τ is characteristic relaxation time.

[0046] The present invention provides an ethylene-α-olefin copolymer, specifically an ethylene-α-olefin copolymer having better mechanical properties than those of the prior art, wherein the α-olefin is preferably one or more α-olefins having 3 to 20 carbon atoms.

[0047] In the present invention, the ethylene-α-olefin copolymer is preferably an ethylene-α-olefin copolymer comprising repeating units derived from ethylene and repeating units derived from α-olefins having 3 to 20 carbon atoms; wherein the repeating units derived from ethylene are preferably 70 mol% to 99.9 mol%, and the repeating units derived from α-olefins having 3 to 20 carbon atoms are preferably 0.1 mol% to 30 mol%.

[0048] The ethylene-α-olefin copolymer provided by the present invention may also contain repeating units derived from other monomers other than ethylene and α-olefins having 3 to 20 carbon atoms; examples of other monomers include conjugated dienes (e.g., butadiene, isoprene), non-conjugated dienes (e.g., 1,4-pentadiene), acrylic acid, acrylic acid esters (e.g., methyl acrylate, ethyl acrylate), methacrylic acid, methacrylic acid esters (e.g., methyl methacrylate, ethyl methacrylate), vinyl acetate, and the like.

[0049] The ethylene-α-olefin copolymer provided by the present invention is preferably a copolymer of ethylene and an α-olefin of 5 to 10 carbon atoms, or a copolymer of ethylene, 1-butene and an α-olefin of 5 to 10 carbon atoms, more preferably a copolymer of ethylene and an α-olefin of 6 to 10 carbon atoms, or a copolymer of ethylene, 1-butene and an α-olefin of 6 to 10 carbon atoms; examples of ethylene-α-olefin copolymers include ethylene-1-hexene copolymers, ethylene-4-methyl-1-pentene copolymers and ethylene-1-octene copolymers, and preferably ethylene-1-hexene copolymers. In addition, it can also be a terpolymer of ethylene, an α-olefin of 6 to 10 carbon atoms and 1-butene, including an ethylene-1-butene 1-hexene terpolymer, an ethylene-1-butene-4-methyl-1-pentene terpolymer and an ethylene-1-butene-1-octene terpolymer, more preferably an ethylene-1-butene-1-hexene terpolymer.

[0050] In the present invention, the ethylene-α-olefin copolymer has a melt index (MFR, unit: g / 10min) of 0.1 to 100 g / 10min, preferably 1 to 30 g / 10min, more preferably 1.2 to 15 g / 10min, and even more preferably 2.1 to 10.3 g / 10min. In the present invention, the MFR is measured at 190°C and 21.18N (2.16kg) load according to the method defined in JIS K7210-1995.

[0051] Furthermore, the ethylene-α-olefin copolymer has a melt flow activation energy (Ea) greater than or equal to 50 kJ / mol, preferably 60 kJ / mol to 100 kJ / mol, and more preferably 63 kJ / mol to 90 kJ / mol.

[0052] Moreover, MT, [η], A and τ satisfy formulas (1) to (4):

[0053] 2.1×MFR -0.59 <MT<18×MFR -0.59 (1);

[0054] 1.03×MFR -0.094 <[η]<1.52×MFR -0.156 (2);

[0055] logA≥-0.0815×log(MFR)+4.06 (3);

[0056] τ≥8.15×MFR -0.746 (4);

[0057] Wherein, MT is the melt tension at 190°C, [η] is the intrinsic viscosity, A is the chain length, and τ is the characteristic relaxation time.

[0058] In the present invention, the 190°C melt tension (MT, unit: cN) of the ethylene-α-olefin copolymer satisfies formula (1):

[0059] 2.1×MFR -0.59 <MT<18×MFR -0.59 (1).

[0060] The ethylene-α-olefin copolymer provided by the present invention may be a polymer having a similar tightly wound long chain branching structure, and it is considered that due to the above structure, and the melt tension and MFR of the ethylene-α-olefin copolymer of the present invention satisfy the above formula (1), the melt tension of the ethylene-α-olefin copolymer of the present invention is higher than that of a conventional ethylene-α-olefin copolymer having the same MFR as the ethylene-α-olefin copolymer of the present invention.

[0061] The ethylene-α-olefin copolymer provided by the present invention satisfies the relationship of the above formula (1), so the extrusion molding processability of the copolymer of the present invention is excellent; when the relationship 2.1×MFR in formula (1) is not satisfied -0.59 When MT < MT (such as when the melt tension is too low), the extrusion molding processability will deteriorate. When the relationship MT < 18 × MFR is not satisfied in formula (1) -0.59 When the melt tension is too high (such as when the melt tension is too high), taking over the process at high speed may become difficult.

[0062] In the present invention, the MT of the ethylene-α-olefin copolymer preferably satisfies:

[0063] 2.3×MFR -0.59 <MT<13×MFR-0.59 ;

[0064] More preferably, the following conditions are met:

[0065] 2.8×MFR -0.59 <MT<8×MFR -0.59 .

[0066] In the present invention, the melt tension (MT, unit: cN) in the above formula (1) is measured as follows: using a melt tension tester, a molten resin is extruded by a piston at an extrusion speed of 5.5 mm / min at 190°C through a hole with a diameter of φ2.09 mm and a length of 8 mm, and a roller with a diameter of 50 mm is used to wind the above-mentioned strand, while increasing the rotation speed at a rate of 40 r / min per minute. The tension value displayed when the strand is about to break is considered to be the melt tension in formula (1).

[0067] In the present invention, the intrinsic viscosity ([η], unit: dl / g) of the ethylene-α-olefin copolymer satisfies formula (2):

[0068] 1.03×MFR -0.094 <[η]<1.52×MFR -0.156 (2).

[0069] The ethylene-α-olefin copolymer provided by the present invention may be a polymer having a similar tightly wound long chain branched structure, and it is considered that due to the above structure, and the intrinsic viscosity and MFR of the ethylene-α-olefin copolymer of the present invention satisfy the above formula (2), the intrinsic viscosity of the ethylene-α-olefin copolymer of the present invention is higher than that of a conventional ethylene-α-olefin copolymer having the same MFR as the ethylene-α-olefin copolymer of the present invention.

[0070] The ethylene-α-olefin copolymer provided by the present invention satisfies the relationship of the above formula (2), so the copolymer of the present invention has low extrusion torque and excellent extrusion molding processability; when the relationship 1.03×MFR in formula (2) is not satisfied -0.094 When the intrinsic viscosity [η] is too low, the impact strength will decrease. When the relationship [η] < 1.52 × MFR is not satisfied in formula (2), -0.156 When the intrinsic viscosity [η] is too high, the extrusion torque becomes high and the extrusion moldability becomes poor.

[0071] In the present invention, [η] of the ethylene-α-olefin copolymer preferably satisfies:

[0072] 1.06×MFR -0.094 <[η]<1.47×MFR -0.156 ;

[0073] More preferably, the following conditions are met:

[0074] 1.09×MFR -0.094 <[η]<1.42×MFR -0.156 .

[0075] In the present invention, the intrinsic viscosity ([η], unit: dl / g) in the above formula (2) is measured as follows: 100 mg of an ethylene-α-olefin copolymer is dissolved in 100 ml of tetralin containing 5 wt% of butylated hydroxytoluene (i.e., BHT, as a thermal degradation inhibitor) at 135°C to prepare a sample solution, and the relative viscosity (ηrel) at 135°C is calculated from the dripping time of the above sample solution and a blank solution using an Ubbelohde viscometer, and then the intrinsic viscosity is calculated; the blank solution is tetralin containing 5 wt% of BHT (as a thermal degradation inhibitor).

[0076] [η] = 23.3 × log (ηrel);

[0077] The melt flow rate (MFR, unit: g / 10min) in formula (2) is the same as the melt flow rate (MFR) used in formula (1), and will not be repeated here.

[0078] In the present invention, the chain length A of the ethylene-α-olefin copolymer satisfies the following formula (3):

[0079] logA≥-0.0815×log(MFR)+4.06 (3).

[0080] In the present invention, chain length A is the chain length at the peak of the logarithmic normal distribution curve of the component with the highest molecular weight in the logarithmic normal distribution curve. The chain length distribution curve is determined by gel permeation chromatography, and the chain length distribution curve is divided into at least two logarithmic normal distribution curves to obtain the logarithmic normal distribution curve.

[0081] The ethylene-α-olefin copolymer provided by the present invention satisfies the relationship of the above formula (3), and the copolymer of the present invention has a low extrusion torque and excellent extrusion molding processability; from the perspective of improving the extrusion molding processability and appearance of extruded products (such as films), the chain length A (logA) is usually 4.3 or less.

[0082] In the present invention, A of the ethylene-α-olefin copolymer preferably satisfies:

[0083] logA≥-0.0815×log(MFR)+4.07;

[0084] More preferably, the following conditions are met:

[0085] logA≥-0.0815×log(MFR)+4.08.

[0086] The present invention obtains a chain length distribution curve by gel permeation chromatography under the following conditions.

[0087] (1) Apparatus: Waters 150C manufactured by Waters;

[0088] (2) Separation column: TOSOH TSKgel GMH-HT;

[0089] (3) Measurement temperature: 145°C;

[0090] (4) Carrier: o-dichlorobenzene;

[0091] (5) Flow rate: 1.0 ml / min;

[0092] (6) Injection volume: 500 μL.

[0093] The division of the chain length distribution curve is performed as follows:

[0094] First, the chain length distribution curve is measured by gel permeation chromatography, in which the Y axis is the weight ratio dW / d (logAw), and the X axis is the logarithm of the chain length Aw logAw. The number of plotted data should be greater than 300 in order to obtain a continuous distribution curve. Next, four logarithmic normal distribution curves (XY curves) are added to the above X axis in an arbitrary proportion to make a comprehensive curve, wherein the logarithmic normal distribution curve has a standard deviation of 0.30 and an arbitrary average value (usually corresponding to the chain length A at the peak). The average value and the ratio are then determined to minimize the sum of the variances of the differences, which is the difference between the y value of the actually measured chain length distribution curve (yobs) and the y value of the comprehensive curve (ycal), and the two y values ​​are plotted for the same x value. It is preferred that the total variance is as small as possible and the percentage relative to each peak is 0, usually not exceeding 0.5% of the total variance of yobs.

[0095] When the mean value and ratio providing the minimum total variance are obtained, logA is calculated from the chain length A at the peak of the lognormal distribution curve of the component with the highest molecular weight in the lognormal distribution curve obtained by dividing into four lognormal distribution curves. The ratio of the lognormal distribution curve of the component with the highest molecular weight is usually not less than 10% of the comprehensive curve.

[0096] In the present invention, the characteristic relaxation time (τ, unit: second) of the ethylene-α-olefin copolymer at 190° C. satisfies formula (4):

[0097] τ≥8.15×MFR -0.746 (4).

[0098] The ethylene-α-olefin copolymer provided by the present invention may be a polymer having a similar tightly wound long chain branched structure, and it is believed that due to the above structure, and the characteristic relaxation time and MFR of the ethylene-α-olefin copolymer of the present invention satisfy the above formula (4), the characteristic relaxation time of the ethylene-α-olefin copolymer of the present invention is higher than that of a conventional ethylene-α-olefin copolymer having the same MFR as the ethylene-α-olefin copolymer of the present invention.

[0099] The ethylene-α-olefin copolymer provided by the present invention satisfies the relationship of the above formula (4), so the copolymer of the present invention has low extrusion torque, excellent extrusion molding processability, and excellent appearance of extruded products (such as films, etc.). From the perspective of reducing the extrusion torque to improve the extrusion molding processability and appearance of the extruded products (such as films), the above characteristic relaxation time τ is preferably 20 seconds or shorter.

[0100] In the present invention, τ of the ethylene-α-olefin copolymer preferably satisfies:

[0101] τ≥8.25×MFR -0.746 ;

[0102] More preferably, the following conditions are met:

[0103] τ≥8.45×MFR -0.746 .

[0104] In the present invention, the characteristic relaxation time τ at 190°C in the above formula (4) is a value calculated by approximating the master curve using the following CROSS equation; the temperature is measured under the following conditions using a Rheometrics Mechanical Spectrometer RMS-800 manufactured by Rheometrics as a viscoelasticity measuring device based on the temperature-time equivalence (superposition) principle, and the dynamic viscoelastic data at each temperature are converted to obtain a master curve, which shows the correlation between the dynamic viscosity (η, unit: Pa·s) and the shear rate (ω, unit: rad / s) at 190°C.

[0105] Test conditions for dynamic viscoelastic data at each temperature T(K):

[0106] (1) Geometry: parallel plates, diameter: 25 mm, plate spacing: 1.5-2 mm;

[0107] (2) Strain: 5%;

[0108] (3) Shear rate: 0.1~100 rad / s;

[0109] (4) Temperature: 190°C, 170°C, 150°C, 130°C;

[0110] An appropriate amount (e.g., 1000 ppm or more) of an antioxidant such as Irganox 1076 or the like is added to the sample in advance, and the measurements are all performed in nitrogen.

[0111] An appropriate amount (e.g. 1000 ppm or more) of an antioxidant such as Irganox 1076 may also be pre-compounded with the sample and the measurements are all carried out in nitrogen.

[0112] CROSS approximate equation:

[0113] η=η0 / [1+(τ×ω)n];

[0114] Similar to the characteristic relaxation time τ, η0 and n are constants obtained by measuring the dynamic viscoelastic data of the ethylene-α-olefin copolymer.

[0115] Rhios V.4.4.4 manufactured by Rheometrics was used as calculation software for obtaining the master curve and the CROSS approximate formula.

[0116] In a preferred embodiment of the present invention, the ethylene-α-olefin copolymer may be a polymer having a similar tightly wound long-chain branched structure, and it is believed that the melt flow activation energy of the ethylene-α-olefin copolymer of the present invention is higher than that of conventional ethylene-α-olefin copolymers, so that the above-mentioned polymer has excellent extrusion molding processability.

[0117] From the viewpoint of improving the melt tension at a relatively low temperature and obtaining sufficient molding processability, the melt flow activation energy (Ea, unit: kJ / mol) of the ethylene-α-olefin copolymer provided by the present invention is preferably greater than or equal to 50 kJ / mol, more preferably greater than or equal to 63 kJ / mol, and even more preferably greater than or equal to 66 kJ / mol. In order not to reduce the melt viscosity and good molding processability of the ethylene-α-olefin copolymer too much at high temperature, and to prevent the appearance of the extruded article (such as film) from deteriorating, Ea is preferably less than or equal to 100 kJ / mol, and more preferably less than or equal to 90 kJ / mol.

[0118] In the present invention, the above melt flow activation energy (Ea) is a value calculated by converting the dynamic viscoelastic data at each temperature T (K) according to the Arrhenius type equation of the following conversion factor (aT), and is used as a moldability index. The temperature T (K) measurement conditions are the same as those for calculating the characteristic relaxation time (τ), and Rheometrics Mechanical Spectrometer RMS-800 manufactured by Rheometrics is used as a viscoelasticity measurement device based on the temperature-time equivalence principle.

[0119] Arrhenius type equation for the conversion factor (aT):

[0120] log(aT)=Ea / R((1 / T)-(1 / T0));

[0121] Where R is the gas constant and T0 is the standard temperature (463K).

[0122] Rhios V.4.4.4 manufactured by Rheometrics was used as calculation software, and the Ea value when the correlation factor r2 obtained by linear approximation in the Arrhenius curve log(aT)-(1 / T) was 0.99 or more was taken as the flow activation energy of the ethylene-α-olefin copolymer of the present invention.

[0123] On this basis, the ethylene-α-olefin copolymer provided by the present invention has a polymer structure similar to the tightly entangled long-chain branches as described above, and its expansion ratio (SR) and intrinsic viscosity ([η], unit: dL / g) satisfy the following formulas (5) to (6):

[0124] If [η] < 1.20,

[0125] -0.91×[η]+2.265<SR<2.1 (5);

[0126] If [η] ≥ 1.20,

[0127] 1.15<SR<2.1 (6)

[0128] In a preferred embodiment of the present invention, the ethylene-α-olefin copolymer may be a polymer having a structure similar to closely wound long chain branches, and it is believed that due to the above structure, and the [η] and SR of the ethylene-α-olefin copolymer of the present invention satisfy the above formula (5) or (6), the SR of the ethylene-α-olefin copolymer of the present invention is higher than that of a conventional ethylene-α-olefin copolymer having the same intrinsic viscosity as the ethylene-α-olefin copolymer of the present invention. If the ethylene-α-olefin copolymer provided by the present invention satisfies the relationship of the above formula (5) or (6), the ethylene-α-olefin copolymer has a low extrusion torque and excellent stability during extrusion processing, and an extruded product (such as a film) obtained from the ethylene-α-olefin copolymer has an excellent appearance and no surface unevenness.

[0129] In the present invention, the expansion ratio (SR) in the above formula (5) is a value (D / D0) obtained by dividing the diameter D (D measured at any point between 1 and 6 mm from the end of the wire) by the hole diameter (D0) of 2.095 mm, wherein the wire is extruded in a linear shape and cooled and solidified, during which the above MFR is measured (190°C, 21.18N (2.16kg) load). The diameter D is obtained by the average value of three wire samples.

[0130] In view of extrusion torque, extrusion molding processability, smoke generation and fluidity during extrusion molding, the molecular weight distribution of the ethylene-α-olefin copolymer of the present invention is preferably 2 to 3.5, more preferably 2 to 3, and even more preferably 2 to 2.5. The numerical value of the above molecular weight distribution is obtained by calculating the weight average molecular weight (Mw) and the number average molecular weight (Mn) based on the polystyrene calibration standard (obtained from the chain length distribution measured by the above gel permeation chromatography), and then dividing Mw by Mn (Mw / Mn).

[0131] The density of the ethylene-α-olefin copolymer provided by the present invention is generally 830-890 kg / cm 3 (Value measured by the method defined in JIS K6760-1981). In view of the balance between rigidity and impact strength of the film obtained from the ethylene-α-olefin copolymer of the present invention, the density is preferably 840 to 880 kg / m 3 , more preferably 850~870kg / m 3 .

[0132] From the perspective of improving fluidity and reducing extrusion torque to improve extrusion processing performance, the melt flow rate ratio (MFRR) of the ethylene-α-olefin copolymer of the present invention is preferably 1-20, more preferably 2-10, and even more preferably 4-6.

[0133] The melt flow rate ratio (MFRR) is a value obtained by dividing the melt flow rate value measured at 190°C and 211.82N (21.6kg) by the melt flow rate value measured under a load of 21.18N (2.16kg) according to JIS K7210-1995. For the measurement of the melt flow rate, 1000ppm of an antioxidant was previously added to the polymer used.

[0134] When the melting point of the ethylene-α-olefin copolymer of the present invention is 40-60°C, more preferably 45-55°C, and even more preferably 48-50°C.

[0135] The above melting point includes the melting peak temperature observed by compacting 8 to 12 mg of a sample in an aluminum pan, keeping the sample at 150° C. for 2 minutes, then cooling the sample to 40° C. at 5° C. / min using a differential scanning calorimeter DSC-7 type apparatus (manufactured by PerkinElmer), keeping the sample at 40° C. for 2 minutes, and then heating the sample to 150° C. at 5° C. / min. Among them, the temperature at the highest temperature melting peak is the maximum melting point (Tmax).

[0136] The present invention also provides a method for preparing the ethylene-α-olefin copolymer described in the above technical solution, comprising the following steps:

[0137] Ethylene and α-olefin are copolymerized in the presence of hydrogen using a metallocene olefin polymerization catalyst and a co-catalyst, and then filtered, washed and devolatilized in sequence to obtain an ethylene-α-olefin copolymer.

[0138] In the present invention, the α-olefin is preferably an α-olefin of 3 to 20 carbon atoms, such as 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, etc., more preferably 4-methyl-1-pentene and / or 1-hexene. Among the above α-olefins, two or more α-olefins can be used together, for example: a combination of 1-butene and 4-methyl-1-pentene, a combination of 1-butene and 1-hexene, a combination of 1-butene and 1-octene, a combination of 1-butene and 1-decene, etc., and a preferred combination is a combination of 1-butene and 4-methyl-1-pentene, and a combination of 1-butene and 1-hexene.

[0139] The present invention adds hydrogen as a molecular weight regulator to adjust the melt fluidity of the copolymer; in addition, an inert gas is allowed to coexist in the mixed gas.

[0140] The present invention has no particular limitation on the sources of the ethylene, α-olefin and hydrogen, and any commercially available products or self-made products known to those skilled in the art may be used.

[0141] In the present invention, the preparation method further comprises mixing the raw materials in the presence of an organic solvent; the organic solvent is preferably a linear alkane, isoalkane, cycloalkane or aromatic alkane with 6 to 10 carbon atoms, more preferably one or more of n-hexane, cyclohexane, methylcyclohexane, n-heptane, isoheptane, n-octane, isooctane, n-decane, isoalkane oil (Ispoar), toluene and xylene. The present invention has no particular restrictions on the source of the organic solvent, and commercially available products known to those skilled in the art can be used.

[0142] In the present invention, the organic solvent, ethylene and α-olefin used need to be dehydrated and deoxygenated, and the present invention has no special restrictions on the specific implementation method.

[0143] In the present invention, the metallocene olefin polymerization catalyst is preferably selected from dimethylsilyl bridge group-tetramethylcyclopentadienyl-tert-butylamino-titanium dichloride and / or dimethylsilyl bridge group-tetramethylcyclopentadienyl-tert-butylamino-dimethyltitanium, more preferably dimethylsilyl bridge group-tetramethylcyclopentadienyl-tert-butylamino-titanium dichloride or dimethylsilyl bridge group-tetramethylcyclopentadienyl-tert-butylamino-dimethyltitanium. The present invention has no particular restrictions on the source of the catalyst, and commercially available products well known to those skilled in the art can be used.

[0144] In the present invention, the cocatalyst is preferably selected from one or more of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride, ethylaluminum dichloride, methylaluminoxane (MAO), modified methylaluminoxane (MMAO), perfluorophenylboron, triphenylcarbon tetrakis (pentafluorophenyl) borate, N,N-dimethylanilinium tetrakis (pentafluorophenyl) borate, and N,N-di(hexadecyl)anilinium tetrakis (pentafluorophenyl) borate, more preferably methylaluminoxane (MAO) or modified methylaluminoxane (MMAO). The present invention has no particular restrictions on the source of the cocatalyst, and commercially available products known to those skilled in the art can be used.

[0145] In the present invention, the temperature of the copolymerization reaction must be higher than the supercritical temperature of the ethane, and the polymerization temperature must be lower than the supercritical temperature of the organic solvent. The polymerization temperature must also ensure that the polymerization system is in a homogeneous solution state, preferably 65°C~250°C, more preferably 80°C~150°C; the pressure of the copolymerization reaction must be higher than the supercritical pressure of the ethane, and the polymerization pressure must ensure that the polymerization system is in a homogeneous solution state, preferably 1MPa~15MPa, more preferably 4MPa~12MPa; the time of the copolymerization reaction is preferably 6h~10h.

[0146] In the present invention, the devolatilization method is preferably oven vacuum heating; the temperature of the oven vacuum heating is preferably 50°C~100°C, the pressure is preferably ≤-0.08MPa (vacuum pump is used to evacuate to maintain negative pressure), and the time is preferably ≥5h; finally, the heating and vacuuming are stopped, and the temperature is naturally lowered. When the temperature is <80°C, the oven is opened under nitrogen protection to obtain ethylene-α-olefin copolymer.

[0147] The present invention provides an ethylene-α-olefin copolymer having a melt index of 0.1 to 100 g / 10 min, a melt flow activation energy of 50 kJ / mol or more, and MT, [η], A and τ satisfying formulas (1) to (4):

[0148] 2.1×MFR -0.59 <MT<18×MFR -0.59 (1);

[0149] 1.03×MFR -0.094 <[η]<1.52×MFR -0.156 (2);

[0150] logA≥-0.0815×log(MFR)+4.06 (3);

[0151] τ≥8.15×MFR -0.746 (4);

[0152] Wherein, MFR is melt index, MT is melt tension at 190°C, [η] is intrinsic viscosity, A is chain length, and τ is characteristic relaxation time.

[0153] Compared with the prior art, the ethylene-α-olefin copolymer provided by the present invention meets the requirements of specific index parameters, and has not only a high melt flow rate, but also excellent tensile strength and elongation at break.

[0154] In addition, the preparation method provided by the present invention has simple process, easily controllable conditions and broad application prospects.

[0155] In order to further illustrate the present invention, the following examples are provided for detailed description.

[0156] Example 1

[0157] In this experiment, the main catalyst used was dimethylsilyl bridge-tetramethylcyclopentadienyl-tert-butylamino-dimethyltitanium, the co-catalyst used was modified methylaluminoxane, the organic solvent was n-hexane, and the co-monomer was 1-butene. The n-hexane and 1-butene were refined in advance, and the ethylene ethane mixture entered the device after refining. The main catalyst and n-hexane were used as a solution, and the co-catalyst was diluted with n-hexane. Before the experiment, the pipeline, mixing kettle, and reactor were replaced with nitrogen three times, and then the reactor was repeatedly vacuumed and replaced with nitrogen at 140°C for 6 hours, and then vacuumed and replaced with ethylene twice, and the kettle was filled with normal pressure ethylene atmosphere, and the entire pipeline and reactor were sealed and anhydrous and oxygen-free.

[0158] The experimental steps are as follows: the reactor is used alone and connected in series with the mixing kettle. The process of n-hexane entering the mixing kettle is opened, the n-hexane pump is started, and the n-hexane flow rate is controlled at 1kg / h to supplement n-hexane; when the reactor is filled with n-hexane, the reactor pressure is set to 4MPa and automatically controlled; the process of 1-butene entering the mixing kettle is opened, the 1-butene pump is started, and the 1-butene flow rate is controlled at 0.5kg / h to supplement 1-butene; the process of ethylene entering the mixing kettle is opened, and the ethylene flow rate is controlled at 0.5kg / h to supplement the mixed gas; the process of the co-catalyst entering the mixing kettle is opened, the co-catalyst pump is started, and the co-catalyst flow rate is controlled at 2.5g / min to supplement the catalyst. The oil bath heating of the reactor is turned on and the temperature is set to 140℃. After the system runs for 2h, the mixing of each component is stable, and the catalyst is added. The catalyst is opened to the reactor process, the catalyst pump is started, and the catalyst flow rate is controlled at 1ml / min. After the reaction starts, the temperature in the reactor will rise, and the reaction temperature is controlled to be stable at 140℃ by changing the oil bath temperature. After the system reaction was stable for 8 h, sampling was carried out, and each sampling time was 15 min. The samples were filtered, washed with ethanol several times, and then vacuum dried at 60 °C for more than 8 h.

[0159] In this experiment, the main catalyst in the kettle was prepared in a ratio of 0.5g catalyst + 800ml n-hexane, the co-catalyst was prepared in a ratio of 50ml MAO-7 + 950ml n-hexane, the molar concentration ratio of the co-catalyst to the main catalyst was 180:1, and the feed mass ratio of 1-butene to ethylene was 1.2:1. All materials used in this experiment were treated with dehydration and deoxygenation.

[0160] The experimental results are listed in Table 1.

[0161] Example 2

[0162] The experimental conditions were as follows: the 1-butene flow rate was changed to 0.6 kg / h, the ethylene flow rate was changed to 0.45 kg / h, and the others were the same as in Example 1.

[0163] The experimental results are listed in Table 1.

[0164] Example 3

[0165] The experimental conditions were as follows: the 1-butene flow rate was changed to 0.7 kg / h, the ethylene flow rate was changed to 0.4 kg / h, and the others were the same as in Example 1.

[0166] The experimental results are listed in Table 1.

[0167] Example 4

[0168] The experimental conditions were as follows: the 1-butene flow rate was changed to 0.8 kg / h, the ethylene flow rate was changed to 0.35 kg / h, and the others were the same as in Example 1.

[0169] The experimental results are listed in Table 1.

[0170] Example 5

[0171] The experimental conditions were as follows: the 1-butene flow rate was changed to 0.9 kg / h, the ethylene flow rate was changed to 0.3 kg / h, and the others were the same as in Example 1.

[0172] The experimental results are listed in Table 1.

[0173] Table 1 Experimental results

[0174]

[0175] It can be seen from the above examples that the ethylene-α-olefin copolymer provided by the present invention has excellent tensile strength and elongation at break, and satisfies the following formula:

[0176] 2.8×MFR -0.59 <MT<8×MFR -0.59 ;

[0177] 1.09×MFR -0.094 <[η]<1.42×MFR -0.156 ;

[0178] logA≥-0.0815×log(MFR)+4.08;

[0179] τ≥8.45×MFR -0.746 ;

[0180] -0.91×[η]+2.265<SR<2.1.

[0181] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. An ethylene-α-olefin copolymer, characterized in that It has a melt index of 0.1 to 100 g / 10 min, a melt flow activation energy greater than or equal to 50 kJ / mol, and MT, [η], A and τ satisfy formulas (1) to (4): 2.1×MFR -0.59 <MT<18×MFR -0.59 (1); 1.03×MFR -0.094 <[η]<1.52×MFR -0.156 (2); logA≥-0.0815×log(MFR)+4.06 (3); τ≥8.15×MFR -0.746 (4); Wherein, MFR is melt index, MT is melt tension at 190°C, [η] is intrinsic viscosity, A is chain length, and τ is characteristic relaxation time.

2. The ethylene-α-olefin copolymer according to claim 1, characterized in that The ethylene-α-olefin copolymer is an ethylene-α-olefin copolymer comprising repeating units derived from ethylene and repeating units derived from α-olefins with 3 to 20 carbon atoms; wherein the repeating units derived from ethylene account for 70 mol% to 99.9 mol%, and the repeating units derived from α-olefins with 3 to 20 carbon atoms account for 0.1 mol% to 30 mol%.

3. The ethylene-α-olefin copolymer according to claim 1, characterized in that The MFR is 1-30 g / 10 min, and the melt flow activation energy is 60 kJ / mol-100 kJ / mol.

4. The ethylene-α-olefin copolymer according to claim 1, characterized in that The MT, [η], A and τ satisfy the formula: 2.3×MFR -0.59 <MT<13×MFR -0.59 ; 1.06×MFR -0.094 <[η]<1.47×MFR -0.156 ; logA≥-0.0815×log(MFR)+4.07; τ≥8.25×MFR -0.746 。 5. The ethylene-α-olefin copolymer according to any one of claims 1 to 4, characterized in that The SR and intrinsic viscosity of the ethylene-α-olefin copolymer satisfy formulas (5) to (6): If [η] < 1.20, -0.91×[η]+2.265<SR<2.1 (5); If [η] ≥ 1.20, 1.15<SR<2.1 (6); Wherein, SR is the expansion ratio.

6. A method for preparing an ethylene-α-olefin copolymer according to any one of claims 1 to 4, characterized in that: The following steps are involved: Ethylene and α-olefin are copolymerized in the presence of hydrogen using a metallocene olefin polymerization catalyst and a co-catalyst, and then filtered, washed and devolatilized in sequence to obtain an ethylene-α-olefin copolymer.

7. The preparation method according to claim 6, characterized in that: The metallocene olefin polymerization catalyst is selected from dimethylsilyl bridge group-tetramethylcyclopentadienyl-tert-butylamino-titanium dichloride and / or dimethylsilyl bridge group-tetramethylcyclopentadienyl-tert-butylamino-dimethyltitanium.

8. The preparation method according to claim 6, characterized in that: The co-catalyst is selected from one or more of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride, ethylaluminum dichloride, methylaluminoxane, modified methylaluminoxane, perfluorophenylboron, triphenylcarbon tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, and N,N-dicetylanilinium tetrakis(pentafluorophenyl)borate.

9. The preparation method according to claim 6, characterized in that: The copolymerization reaction is carried out at a temperature of 65° C. to 250° C., a pressure of 1 MPa to 15 MPa, and a reaction time of 6 h to 10 h.

10. The preparation method according to claim 6, characterized in that: The devolatilization method is oven vacuum heating; the temperature of the oven vacuum heating is 50°C to 100°C, the pressure is ≤-0.08MPa, and the time is ≥5h.

Citation Information

Patent Citations

  • Ethylene copolymer

    CN100404564C