Iron extraction process for producing aluminum oxide based on sintering method / series-parallel method
The iron extraction process for producing alumina by sintering/mixed methods utilizes reducing agents and nucleating agents to generate clinker, followed by magnetic separation and washing. This solves the problems of low iron ore grade and high energy consumption in the comprehensive utilization of red mud, and achieves efficient iron ore extraction and alumina production.
Patent Information
- Application Number
- CN202411145639.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
In the current comprehensive utilization of red mud, the iron ore obtained by the wet magnetic separation method of red mud slurry is of low grade and poor economic benefits, while the red mud roasting magnetic separation method has high energy consumption and the tailings are difficult to handle.
The iron extraction process for alumina production using the sintering/hybrid method involves adding a reducing agent and a nucleating agent to the raw slurry, roasting it to produce clinker, separating the magnetic tailings and iron concentrate using dry magnetic separation, using the tailings for alumina extraction, and washing the iron concentrate to improve its purity.
It improved the grade of refined iron ore, reduced the production costs of iron extraction and alumina, solved the problem of tailings disposal, increased alumina production, and reduced energy consumption.
Smart Images

Figure CN119020585A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alumina production, and in particular relates to an iron extraction process for producing alumina based on a sintering method / hybrid method. Background Art
[0002] Red mud is a strongly alkaline solid waste discharged during the production of alumina. The output of red mud is large and the difficulty of storage is high, which not only wastes land resources but also consumes a lot of money. In addition, red mud is highly alkaline, and long-term storage will alkalize the soil and pollute groundwater. Therefore, the comprehensive utilization of red mud is of great significance.
[0003] Among them, iron extraction from red mud is a method of comprehensive utilization of red mud.
[0004] At present, the main ways of comprehensive utilization of red mud in China are: 1. Wet magnetic separation of red mud slurry, 2. Red mud roasting magnetic separation. However, the iron ore selected by wet magnetic separation of red mud slurry has low grade and poor economic benefits. The red mud roasting magnetic separation method requires the red mud to be roasted again, which has high energy consumption, high operating costs, and difficult to handle tailings. Summary of the invention
[0005] In view of the above problems, the present invention provides an iron extraction process for producing alumina based on a sintering method / hybrid method.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A process for producing alumina by sintering / mixing method comprises the following steps:
[0008] S1, adding the reducing agent and nucleating agent required for iron extraction into the raw material slurry, and sending it into the mixing tank for thorough mixing;
[0009] S2, sending the raw material slurry with the reducing agent and the nucleating agent into a rotary kiln for roasting to produce clinker;
[0010] S3, crushing and grinding the clinker;
[0011] S4, using a dry magnetic separation method to magnetically separate the ground clinker to separate the clinker into magnetic tailings and iron ore concentrate;
[0012] S5, sending the magnetic separation tailings to the alumina production system for alumina extraction;
[0013] S6, washing the iron ore concentrate to improve the purity of the iron ore concentrate to obtain finished iron ore concentrate, and the washing liquid after washing is sent to the alumina production system.
[0014] Furthermore, the reducing agent in S1 is activated carbon powder, and the amount of the reducing agent added is 5-8% of the total mass of bauxite and Bayer process dry red mud in the raw slurry.
[0015] Furthermore, the nucleating agent in S1 is iron ore concentrate, and the amount of the nucleating agent added is 3-6% of the total mass of bauxite and Bayer process dry red mud in the raw slurry.
[0016] Furthermore, in S2, the calcination temperature is 1050-1150° C., and the calcination time is 70-90 minutes.
[0017] Furthermore, in S3, the particle size of the clinker after crushing is less than 20 mm, and the particle size of the clinker after grinding is 0.07-0.08 mm.
[0018] Furthermore, in S6, the purity of the finished iron ore concentrate after washing is 90-99%.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] The present invention extracts iron from clinker. After the iron is extracted from the clinker, alumina can be continuously extracted without affecting the extraction of alumina. The use of clinker to extract iron can save the roasting process and economic cost of the red mud roasting and magnetic separation method, and solve the problem that tailings are difficult to handle. At the same time, after the iron is extracted from the clinker, the total amount of clinker is reduced, and the aluminum content is increased, which is conducive to the extraction of alumina, and the cost of alumina is greatly reduced, and the output of alumina is increased.
[0021] The finished iron ore concentrate of the present invention has high grade, greatly reduces the cost of iron extraction, and also greatly reduces the cost of alumina extraction. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0023] In order to further illustrate the technical solution of the present invention, the present invention is further described below through embodiments.
[0024] Example 1
[0025] A process for producing aluminum oxide by sintering method comprises the following steps:
[0026] S1, adding a reducing agent and a nucleating agent to the raw material slurry, and sending the raw material slurry into a mixing tank for thorough mixing, wherein the raw material slurry is composed of bauxite, lime, soda ash, anthracite and carbon denominator liquid; bauxite is a raw material, and can be prepared in any proportion according to actual production conditions, soda ash is added at an alkali ratio of 0.92, lime is added at a calcium ratio of 1.9, anthracite is added at a fixed carbon content of 3% of the total mass, and carbon denominator liquid is added at a total solid content of 63% in the raw material slurry;
[0027] The reducing agent is activated carbon powder, and the amount of the reducing agent added is 5% of the mass of the bauxite in the raw slurry; the nucleating agent is iron ore powder, and the amount of the nucleating agent added is 3% of the mass of the bauxite in the raw slurry;
[0028] S2, sending the raw material slurry with the reducing agent and the nucleating agent into a rotary kiln for roasting to produce clinker, the roasting temperature is 1050°C, and the roasting time is 90 minutes;
[0029] S3, crushing and grinding the clinker, the particle size of the clinker after crushing is less than 20 mm, and the particle size of the clinker after grinding is 0.07 mm;
[0030] S4, using a dry magnetic separation method to magnetically separate the ground clinker to separate the clinker into magnetic tailings and iron ore concentrate;
[0031] S5, sending the magnetic separation tailings to the alumina production system for alumina extraction;
[0032] S6, washing the iron ore concentrate to improve the purity of the iron ore concentrate to obtain a finished iron ore concentrate. The washing liquid after washing is sent to the alumina production system. The purity of the finished iron ore concentrate after washing is 90%.
[0033] Example 2
[0034] A process for producing alumina by a hybrid method comprises the following steps:
[0035] S1, adding a reducing agent and a nucleating agent to the raw material slurry, and sending it into a mixing tank for thorough mixing. The raw material slurry is composed of bauxite, Bayer red mud, lime, soda ash, anthracite, activated carbon powder, iron ore concentrate and carbon denominator liquid; bauxite and Bayer red mud are both raw materials, and can be mixed in any proportion according to actual production conditions: soda ash is added at an alkali ratio of 0.98, lime is added at a calcium ratio of 2.05, and anthracite is added at a fixed carbon content of 5% of the total. The carbon denominator liquid is added at a solid content of 67%;
[0036] The reducing agent is activated carbon powder, and the amount of the reducing agent added is 8% of the total mass of bauxite and Bayer process dry red mud in the raw slurry; the nucleating agent is iron concentrate, and the amount of the nucleating agent added is 6% of the total mass of bauxite and Bayer process dry red mud in the raw slurry;
[0037] S2, sending the raw material slurry with the reducing agent and the nucleating agent into a rotary kiln for roasting to produce clinker, the roasting temperature is 1150° C., and the roasting time is 70 minutes;
[0038] S3, crushing and grinding the clinker, the particle size of the clinker after crushing is less than 20 mm, and the particle size of the clinker after grinding is 0.08 mm;
[0039] S4, using a dry magnetic separation method to magnetically separate the ground clinker to separate the clinker into magnetic tailings and iron ore concentrate;
[0040] S5, sending the magnetic separation tailings to the alumina production system for alumina extraction;
[0041] S6, washing the iron ore concentrate to improve the purity of the iron ore concentrate to obtain a finished iron ore concentrate. The washing liquid after washing is sent to the alumina production system. The purity of the finished iron ore concentrate after washing is 99%.
[0042] Example 3
[0043] A process for producing aluminum oxide by sintering method comprises the following steps:
[0044] S1, adding a reducing agent and a nucleating agent to the raw material slurry, and sending the raw material slurry into a mixing tank for thorough mixing, wherein the raw material slurry is composed of bauxite, lime, soda ash, anthracite, and carbon denominator liquid; bauxite is a raw material, and can be prepared in any proportion according to actual production conditions, soda ash is added at an alkali ratio of 0.95, lime is added at a calcium ratio of 1.95, anthracite is added at a fixed carbon content of 4% of the total mass, and carbon denominator liquid is added at a solid content of 66%;
[0045] The reducing agent is activated carbon powder, and the amount of the reducing agent added is 6% of the mass of the bauxite in the raw slurry; the nucleating agent is iron ore powder, and the amount of the nucleating agent added is 4% of the mass of the bauxite in the raw slurry;
[0046] S2, sending the raw material slurry with the reducing agent and the nucleating agent into a rotary kiln for roasting to produce clinker, the roasting temperature is 1100° C., and the roasting time is 80 minutes;
[0047] S3, crushing and grinding the clinker, the particle size of the clinker after crushing is less than 20 mm, and the particle size of the clinker after grinding is 0.075 mm;
[0048] S4, using a dry magnetic separation method to magnetically separate the ground clinker to separate the clinker into magnetic tailings and iron ore concentrate;
[0049] S5, sending the magnetic separation tailings to the alumina production system for alumina extraction;
[0050] S6, washing the iron ore concentrate to improve the purity of the iron ore concentrate to obtain a finished iron ore concentrate. The washing liquid after washing is sent to the alumina production system. The purity of the finished iron ore concentrate after washing is 95%.
[0051] Example 4
[0052] A process for producing alumina by a hybrid method comprises the following steps:
[0053] S1, adding reducing agent and nucleating agent to the raw material slurry, and sending it into the mixing tank for thorough mixing. The raw material slurry is composed of bauxite, Bayer red mud, lime, soda ash, anthracite, activated carbon powder, iron ore concentrate and carbon denominator liquid; bauxite and Bayer red mud are both raw materials, and can be mixed in any proportion according to actual production conditions: soda ash is added at an alkali ratio of 0.96, lime is added at a calcium ratio of 2, and anthracite is added at a fixed carbon content of 4% of the total. Carbon denominator liquid is added at a solid content of 65%;
[0054] The reducing agent is activated carbon powder, and the amount of the reducing agent added is 7% of the total mass of bauxite and Bayer process dry red mud in the raw slurry; the nucleating agent is iron concentrate, and the amount of the nucleating agent added is 5% of the total mass of bauxite and Bayer process dry red mud in the raw slurry;
[0055] S2, sending the raw material slurry with the reducing agent and the nucleating agent into a rotary kiln for roasting to produce clinker, the roasting temperature is 1090°C, and the roasting time is 85 minutes;
[0056] S3, crushing and grinding the clinker, the particle size of the clinker after crushing is less than 20 mm, and the particle size of the clinker after grinding is 0.078 mm;
[0057] S4, using a dry magnetic separation method to magnetically separate the ground clinker to separate the clinker into magnetic tailings and iron ore concentrate;
[0058] S5, sending the magnetic separation tailings to the alumina production system for alumina extraction;
[0059] S6, washing the iron ore concentrate to improve the purity of the iron ore concentrate to obtain a finished iron ore concentrate. The washing liquid after washing is sent to the alumina production system. The purity of the finished iron ore concentrate after washing is 98%.
[0060] The above shows and describes the main features and advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes that fall within the meaning and scope of the equivalent elements of the claims are included in the present invention.
[0061] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A process for producing alumina based on sintering method / hybrid method, characterized in that: The following steps are involved: S1, adding the reducing agent and nucleating agent required for iron extraction into the raw material slurry, and sending it into the mixing tank for thorough mixing; S2, sending the raw material slurry with the reducing agent and the nucleating agent into a rotary kiln for roasting to produce clinker; S3, crushing and grinding the clinker; S4, using a dry magnetic separation method to magnetically separate the ground clinker to separate the clinker into magnetic tailings and iron ore concentrate; S5, sending the magnetic separation tailings to the alumina production system for alumina extraction; S6, washing the iron ore concentrate to improve the purity of the iron ore concentrate to obtain finished iron ore concentrate, and the washing liquid after washing is sent to the alumina production system.
2. The iron extraction process for producing alumina based on sintering method / hybrid method according to claim 1, characterized in that: The reducing agent in S1 is activated carbon powder, and the amount of the reducing agent added is 5-8% of the total mass of bauxite and Bayer process dry red mud in the raw slurry.
3. The iron extraction process for producing alumina based on sintering method / hybrid method according to claim 1, characterized in that: The nucleating agent in S1 is iron concentrate, and the amount of the nucleating agent added is 3-6% of the total mass of bauxite and Bayer process dry red mud in the raw slurry.
4. The iron extraction process for producing alumina based on sintering method / hybrid method according to claim 1, characterized in that: In S2, the calcination temperature is 1050-1150° C., and the calcination time is 70-90 minutes.
5. The iron extraction process for producing alumina based on sintering method / hybrid method according to claim 1, characterized in that: In S3, the particle size of the clinker after crushing is less than 20 mm, and the particle size of the clinker after grinding is 0.07-0.08 mm.
6. The iron extraction process for producing alumina based on sintering method / hybrid method according to claim 1, characterized in that: In S6, the purity of the finished iron ore concentrate after washing is 90-99%.