Method for processing hairspring of timepiece movement

By evaporating the Nb-Ti alloy hairspring in a climate-steamed environment in a relative humidity and temperature-controlled environment, the problem of large time difference deviation of the Nb-Ti alloy hairspring is solved, and the time stability is significantly improved.

CN119024668APending Publication Date: 2024-11-26NIVAROX FAR SA
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410615280.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-17
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the hairspring made of Nb-Ti alloy still has the problem of a time difference of more than 6s/d after one year, and the standard steam treatment effect is limited.

Method used

The climate steam steaming step is carried out to process the hairspring made of Nb-Ti alloy in an atmosphere with a relative humidity of 60% to 99%, and the temperature range is 30°C to 100°C. The climate steam steaming step is carried out to treat the hairspring made of Nb-Ti alloy to promote the formation of TiO2 and Adsorption of water molecules.

Benefits of technology

Through climate steam treatment, the time difference of the hairspring is reduced to less than or equal to 3s/d after 5 months, which significantly improves the time stability of the watch movement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119024668A_ABST
    Figure CN119024668A_ABST
Patent Text Reader

Abstract

The invention relates to a treatment method for treating at least one hairspring for equipping a timepiece movement, said hairspring being made of an Nb-Ti alloy, said treatment method comprising a steaming step, referred to as a climate steaming step, i.e. A step of performing steaming in an atmosphere with a relative humidity of between 60% and 99% at a temperature in the range of 30 DEG C to 100 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for treating a hairspring of a timepiece movement and also to a hairspring obtained by such treatment method. Background Art

[0002] Watchmakers are well aware that the frequency of a hairspring oscillator will drift over time.

[0003] To reduce this deviation, it is common practice to carry out a steam treatment, which consists in heating the balance spring to a temperature between 100°C and 250°C for a period of 6 to 24 hours. The steam treatment has the effect of restoring the material, also allowing the diffusion and rearrangement of interstitial elements (i.e. carbon, nitrogen and oxygen), as well as stabilizing the native oxide layer. Despite the steam treatment, deviations of more than 6 s / d (seconds / day) were observed in balance springs made of Nb-Ti alloy after one year. Summary of the invention

[0004] The object of the present invention is to propose a new method for treating a balance spring in order to reduce the deviation of the travel time. The method is applicable to balance springs made of paramagnetic alloys, in particular Nb-Ti alloys, wherein the weight percentage of Ti relative to the total weight of the alloy is between 40% and 90%, preferably between 40% and 50%.

[0005] According to the invention, the balance spring treatment method comprises a steaming step known as climatic steaming, since the steaming is carried out in an atmosphere with a controlled relative humidity level.

[0006] More specifically, the invention relates to a method for treating at least one balance spring intended to equip a timepiece movement, said balance spring being made of a Nb-Ti alloy, comprising a steaming step known as climatic steaming, carried out at a temperature ranging from 30° C. to 100° C. in an atmosphere having a relative humidity between 60% and 99%.

[0007] Tests have shown that the deviation of the balance spring treated with the method according to the invention is significantly reduced. This improvement can be attributed to the generation and growth of TiO2 in different forms on the balance spring surface in response to humidity. It may also be related to the presence of water molecules adsorbed on the balance spring surface.

[0008] The invention also relates to a balance spring having the following characteristics: after 5 months of use from the time when the climate steaming step is performed, the balance spring has a rate error less than or equal to 3 s / d.

[0009] Other features and advantages of the present invention will become apparent from the following description and accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 The relationship between the travel time error (s / d) of a hairspring treated by the method of the present invention and the function of time (month) is shown. For comparison, two hairsprings, one untreated and one treated by a standard steaming method, are shown. DETAILED DESCRIPTION

[0011] The invention relates to a method for treating a balance spring intended to be mounted on a balance wheel of a timepiece movement.

[0012] According to the invention, the treatment method can be carried out on a single balance spring, or in batches on a plurality of balance springs. For example, it can be carried out in a barrel on a base plate comprising a plurality of balance springs. It can also be carried out on a whole timepiece movement equipped with a balance spring. For example, it can be an assembly comprising a balance spring and a collet, or an assembly formed by an oscillator comprising a balance wheel, a balance spring, a disc and an axle.

[0013] The balance spring is made of a paramagnetic alloy, in particular a Nb-Ti alloy. This alloy comprises 40-90% by weight of titanium and may also contain traces of one or more elements selected from O, H, C, Fe, Ta, N, Ni, Si, Cu, Al, each of which represents 0 to 1600 ppm of the total weight, the remainder being niobium to constitute 100%.

[0014] According to the invention, the hairspring treatment method comprises a steaming step carried out at a temperature ranging from 30° C. to 100° C. in an atmosphere with a relative humidity between 60% and 99%. Preferably, the temperature range is between 40° C. and 80° C., more preferably between 40° C. and 60° C. Preferably, the relative humidity is between 70% and 97%, preferably between 85% and 95%, more preferably between 87% and 95%. More preferably, the test is carried out at ambient pressure. It is also possible to carry out the test at a partial pressure ranging from 1 to 1000 mbar. It is also possible to carry out the test at an overpressure, for example in a steam generator, at a pressure ranging from 1 to 5 bar. Different holding times are possible, ranging from a fairly wide range of 10 minutes to 100 hours, the time not significantly affecting the result.

[0015] The climatic steaming treatment according to the invention is preferably carried out after the standard steaming treatment known in the prior art. The standard steaming treatment is carried out at ambient humidity and at a temperature of 100° C. to 250° C. Preferably, it is carried out for a period of 1 to 30 hours.

[0016] Standard steaming and climate steaming are carried out after the balance spring fixing step, which is a heat treatment well known to those skilled in the art.

[0017] The method for manufacturing a balance spring according to the invention thus comprises the following steps, wherein steps a) to f) are known to a person skilled in the art:

[0018] a) producing a billet made of a Nb-Ti alloy having the above-mentioned chemical composition,

[0019] b) subjecting the blank to a dissolution and quenching treatment (referred to as β-type) so that titanium and niobium are substantially in the form of a solid solution in the β phase,

[0020] c) applying a deformation step to the alloy, optionally accompanied by one or more heat treatments. "Deformation" means deformation produced by stretching and / or rolling. If necessary, stretching may require the use of one or more dies during the same step or during different steps. The wire is stretched to have an inverted circular cross-section. Rolling can be carried out according to the same deformation step as the stretching, or according to a different step. Advantageously, the last step applied to the alloy is rolling, preferably rolling to have a rectangular profile adapted to the inlet cross-section of the winding mandrel,

[0021] d) winding to form a balance spring,

[0022] e) final heat treatment for fixation,

[0023] f) optionally subjected to standard steam treatment,

[0024] g) Carrying out the climate steam treatment according to the invention.

[0025] The invention also relates to a balance spring obtained by the treatment method according to the invention. This balance spring is characterized by having titanium oxide on its surface and the possibility of adsorbing water molecules. It is also characterized by having a time difference of less than 3 s / d or even 2 s / d after 5 months of use after the climate steaming step.

[0026] The test was performed after the climate steaming step. Figure 1, where the ordinate is the rate difference expressed in s / d measured at room temperature using a Witschi Chronomaster device and the abscissa is the time measured in months. The tests were carried out on a balance spring made of an Nb-Ti alloy with a Ti weight percentage of 47%. According to the method of the invention, the balance spring was subjected to a standard steaming method according to step f), carried out at 150°C for 24 hours at ambient humidity, followed by a climatic steaming method according to step g), carried out at a temperature of 50°C for 4 hours at ambient pressure in an atmosphere containing 93% relative humidity. For comparison, a balance spring with the same chemical composition but not subjected to the treatment according to steps f) or g) was tested. A balance spring with the same chemical composition but subjected only to the standard steaming treatment according to step f) (treatment at 150°C for 24 hours at ambient humidity) was also tested. A significant reduction in the rate difference deviation was observed for the balance spring manufactured using the treatment method according to the invention. After 5 months, its rate difference was about 2 s / d, compared to a value of about 5 s / d for the control balance spring.

Claims

1. A method for treating at least one hairspring intended to equip a watch movement, said hairspring being made of a Nb-Ti alloy, said method comprising a steaming step known as a climatic steaming step, i.e. a steaming step carried out at a temperature ranging from 30° C. to 100° C. in an atmosphere having a relative humidity between 60% and 99%.

2. The processing method according to claim 1, characterized in that: The climatic steaming step is preceded by a standard steaming step performed in ambient air at a temperature range of 100°C to 250°C.

3. The treatment method according to any one of the preceding claims, characterized in that For the climate steaming step, the temperature range is 40°C to 80°C, preferably 40°C to 60°C.

4. The treatment method according to any one of the preceding claims, characterized in that The relative humidity is between 70% and 97%, preferably between 85% and 95%, more preferably between 87% and 95%.

5. The treatment method according to any one of the preceding claims, characterized in that The treatment process is performed at ambient pressure.

6. The processing method according to any one of claims 1 to 4, characterized in that: The treatment method is carried out at a partial pressure of 1 mbar to 1000 mbar or at an overpressure of 1 bar to 5 bar.

7. The processing method according to any one of claims 1 to 5, characterized in that: The treatment method is performed at ambient pressure in an atmosphere with a relative humidity between 87% and 95% at a temperature between 40°C and 60°C.

8. Process according to any one of the preceding claims, characterized in that The Nb-Ti alloy contains Ti in a weight percentage between 40% and 90%, preferably between 40% and 50%, and possibly one or more other trace elements selected from O, H, C, Fe, Ta, N, Ni, Si, Cu and Al, each of which accounts for 0 to 1600 ppm of the total weight, and the balance of 100% is composed of Nb.

9. The treatment method according to any one of the preceding claims, characterized in that The treatment method is performed on a single balance spring or on a plurality of balance springs simultaneously, including balance springs in a base plate or in a component mounted in a timepiece movement, wherein the treatment is applied to the base plate or the component, respectively.

10. The processing method according to claim 9, characterized in that: The assembly comprises a balance spring and a collet, or the assembly is formed by an oscillator comprising a balance wheel, a balance spring, a disc and an axle.

11. A manufacturing method for manufacturing at least one balance spring, comprising a fixing step and a subsequent treatment method according to any one of the preceding claims.

12. A balance spring obtained by the manufacturing method according to claim 11, characterized in that after 5 months of use from the climate steaming step, the rate variation of the balance spring is less than or equal to 3 seconds / day.

Citation Information

Patent Citations

  • Thermally compensated hairspring made from ceramic comprising silicon in the composition of same and method for adjusting same

    CN106104393A

  • Balance-spring stud for fixing spiral spring of timepiece movement and method for manufacturing such balance-spring stud

    CN110488592A

  • Self-compensating spring for clockwork movement spring balance and method for treating the same

    EP1039352A1

  • Spring and method for manufacturing same

    EP3667433A1

  • Balance spring and method for manufacturing balance spring

    JP2020095027A