Surface acoustic wave device including IDT electrode formed with oxide electrode layer and manufacturing method
By forming an oxidation electrode layer on the IDT electrode of the surface acoustic wave device to control its thickness and density, the problem of difficulty in frequency distribution control in the prior art is solved, and precise adjustment of the frequency distribution of the surface acoustic wave device and the improvement of performance margin are achieved. .
Patent Information
- Application Number
- CN202410652736.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
Existing surface acoustic devices have difficulties in frequency distribution control, especially when supporting high-performance communications such as carrier aggregation in 5G, the allowable range of individually controlled resonant frequency becomes increasingly narrow and difficult to effectively adjust.
The frequency distribution of the surface acoustic wave device is accurately adjusted by forming an oxidation electrode layer on the IDT electrode, controlling its thickness, and maintaining peak losses and bandwidth within the performance tolerance range by adjusting the thickness and density of the oxidation electrode layer.
It realizes precise control of the frequency distribution of surface acoustic wave devices, meets high-performance communication needs, ensures peak loss and bandwidth within a reasonable range, and improves the performance margin of the device.
Smart Images

Figure CN119030496A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a surface acoustic wave device including an IDT (interdigitated) electrode formed with an oxidized electrode layer, and more particularly, to a surface acoustic wave device and a method for manufacturing the surface acoustic wave device, wherein the frequency characteristics of the surface acoustic wave device can be controlled by controlling the thickness of the oxidized electrode layer formed on the IDT electrode by performing an oxidation process. Background Art
[0002] The term "surface acoustic wave (SAW)" refers to waves that propagate along the surface of an elastic solid. These surface acoustic waves propagate when the wave energy is concentrated near the surface and correspond to mechanical waves. Surface acoustic wave devices are electromechanical devices based on the interaction of surface acoustic waves with semiconductor conduction electrons, utilizing surface acoustic waves transmitted to the surface of a piezoelectric crystal. These surface acoustic wave devices can be used in a very wide range of industrial applications such as sensors, oscillators, and filters, and can be miniaturized and lightweight. In addition, these devices may have various advantages such as ruggedness, stability, sensitivity, low price, and real-time performance.
[0003] The surface acoustic wave device includes a plurality of IDT electrodes extending alternately from parallel busbars, and each of the plurality of IDT electrodes includes at least one material selected from conductive metal materials and alloys thereof. The resonant frequency of the surface acoustic wave device is determined by the thickness of the piezoelectric layer, the thickness of the energy confinement layer under the piezoelectric layer, and in particular the thickness of the IDT electrode and the width of the electrode.
[0004] As communication technology develops, the performance requirements of surface acoustic wave devices become more and more complex to support carrier aggregation (CA) in 5G, for example. Correspondingly, the allowable range of resonant frequency is getting narrower and narrower, and the difficulty of controlling each of the above factors individually to improve frequency distribution is increasing. Summary of the invention
[0005] An object of the present disclosure is to provide a surface acoustic wave device whose frequency distribution can be precisely controlled by including an oxidized electrode layer formed by oxidizing an upper electrode layer on an IDT electrode and a method for manufacturing the same.
[0006] Another object of the present disclosure is to provide a surface acoustic wave device and a method for manufacturing the same, wherein the frequency distribution of the surface acoustic wave device can be effectively controlled by adjusting the thickness of an oxide electrode layer formed on an IDT electrode while maintaining the peak loss and bandwidth within a performance tolerance range.
[0007] The objects of the present disclosure are not limited to the above objects, and other objects not mentioned above will be clearly understood by those skilled in the art from the following description.
[0008] To achieve the above-mentioned purpose, according to some embodiments of the present disclosure, a surface acoustic wave device including an IDT electrode having an oxidized electrode layer formed thereon includes a piezoelectric substrate; and a plurality of IDT electrodes formed on the piezoelectric substrate, wherein each of the plurality of IDT electrodes includes: a main electrode layer formed on the upper surface of the piezoelectric substrate; an upper electrode layer formed on the main electrode layer; and an oxidized electrode layer formed on the upper surface of the upper electrode layer by oxidation of the upper electrode layer, wherein the thickness (t e ) relative to the thickness of the oxide electrode layer (to) satisfies 0.011≤to / t e ≤0.333.
[0009] In some embodiments of the present disclosure, the oxidation electrode layer may include: a first oxidation electrode layer having a first density and forming an upper portion of the oxidation electrode layer; and a second oxidation electrode layer having a second density lower than the first density and located below the first oxidation electrode layer.
[0010] In some embodiments of the present disclosure, the first oxidized electrode layer may be a natural oxide layer, and the second oxidized electrode layer may be formed by an oxidation process of irradiating an upper electrode layer with an ion beam.
[0011] In some embodiments of the present disclosure, the upper electrode layer may include titanium (Ti), and the oxidized electrode layer may include titanium oxide.
[0012] In some embodiments of the present disclosure, the upper electrode layer may include aluminum (Al), and the oxidized electrode layer may include aluminum oxide.
[0013] In some embodiments of the present disclosure, the main electrode layer may include at least one metal material selected from aluminum (Al), copper (Cu), titanium (Ti), tungsten (W), molybdenum (Mo), platinum (Pt), and gold (Au).
[0014] In order to achieve the above-mentioned purpose, according to some embodiments of the present disclosure, a surface acoustic wave device including an IDT electrode having an oxidized electrode layer formed thereon includes: a piezoelectric substrate having a first area and a second area defined thereon; a plurality of first IDT electrodes formed in the first area; and a plurality of second IDT electrodes formed in the second area, each of the plurality of first IDT electrodes having a first thickness, and including: a first main electrode layer formed on the upper surface of the piezoelectric substrate in the first area; a first upper electrode layer formed on the first main electrode layer; and a first oxidized electrode layer formed on the upper surface of the first upper electrode layer by oxidation of the first upper electrode layer, each of the plurality of second IDT electrodes having a second thickness, and including: a second main electrode layer formed on the upper surface of the piezoelectric substrate in the second area; a second upper electrode layer formed on the second main electrode layer; and a second oxidized electrode layer formed on the upper surface of the second upper electrode layer by oxidation of the second upper electrode layer, wherein the first thickness and the second thickness are different.
[0015] In some embodiments of the present disclosure, the plurality of first IDT electrodes may correspond to a first center frequency, the plurality of second IDT electrodes may correspond to a second center frequency lower than the first center frequency, and the first thickness may be smaller than the second thickness.
[0016] In some embodiments of the present disclosure, the thickness of the first oxidized electrode layer may be smaller than the thickness of the second oxidized electrode layer.
[0017] In some embodiments of the present disclosure, the first thickness (t e1 ) can be relative to the thickness of the first oxide electrode layer (t o1 ) satisfies 0.011≤t o1 / t e1 ≤0.333, the second thickness (te2) can be relative to the thickness of the second oxide electrode layer (t o2 ) satisfies 0.011≤t o2 / t e2 ≤0.333.
[0018] In some embodiments of the present disclosure, the density of the first oxidized electrode layer may be greater than the density of the second oxidized electrode layer.
[0019] In order to achieve the above-mentioned objectives, according to some embodiments of the present disclosure, a method for manufacturing a surface acoustic wave filter formed on a substrate with a multilayer structure includes the following steps: preparing a piezoelectric substrate; forming an IDT electrode film including a main electrode layer and an upper electrode layer on the piezoelectric substrate; forming an oxidized electrode layer by oxidizing the upper surface of the upper electrode layer; and forming an IDT electrode by patterning the IDT electrode film.
[0020] In some embodiments of the present disclosure, the step of forming the oxidized electrode layer by oxidizing the upper surface of the upper electrode layer may include the step of forming the oxidized electrode layer by irradiating the upper electrode layer with an ion beam.
[0021] In some embodiments of the present disclosure, the piezoelectric substrate may have a first region and a second region defined thereon, and the step of forming an IDT electrode film may include: a step of forming a first IDT electrode film having a first thickness in the first region, and a step of forming a second IDT electrode film having a second thickness in the second region, wherein the first thickness and the second thickness are different.
[0022] In some embodiments of the present disclosure, the step of forming an oxidized electrode layer by oxidizing the upper surface of the upper electrode layer may include:
[0023] forming a first oxidized electrode layer by irradiating an upper surface of a first upper electrode layer included in a first IDT electrode film with an ion beam at a first scanning rate; and
[0024] The second oxidized electrode layer is formed by irradiating an upper surface of a second upper electrode layer included in the second IDT electrode film with an ion beam at a second scanning rate different from the first scanning rate.
[0025] In some embodiments of the present disclosure, the thickness of the first IDT electrode and the thickness of the first oxidation electrode layer may be respectively smaller than the thickness of the second IDT electrode and the thickness of the second oxidation electrode layer, the first IDT electrode may correspond to a first center frequency, and the second IDT electrode may correspond to a second center frequency lower than the first center frequency.
[0026] In some embodiments of the present disclosure, the density of the first oxidized electrode layer may be greater than the density of the second oxidized electrode layer.
[0027] Specific details of other embodiments are included in the following detailed description and accompanying drawings.
[0028] According to an embodiment of the present disclosure, a surface acoustic wave filter is formed on a substrate with a multi-layer structure and a manufacturing method thereof. By adjusting the thickness of the oxide electrode layer, the distribution of the resonant frequency can be effectively controlled. The resonant frequency may vary with the thickness and width of the IDT electrode, the thickness of the piezoelectric layer, and the thickness of the energy limiting layer under the piezoelectric layer.
[0029] The effects of the present disclosure are not limited to the above-mentioned effects, and other effects not mentioned above will be clearly understood by those skilled in the art from the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 A surface acoustic wave device including an IDT electrode having an oxidized electrode layer formed thereon according to an embodiment of the present disclosure is shown.
[0031] Figure 2a The transmission electron microscope (TEM) image and energy dispersive spectrometer (EDS) image of the upper metal layer of each IDT electrode of the surface acoustic wave device before the oxidation process are shown. Figure 2b TEM images of IDT electrodes with thickness values are shown.
[0032] Figure 3a TEM photos and EDS images showing the oxidation process of the upper metal layer of each IDT electrode of the surface acoustic wave device according to one embodiment of the present disclosure, Figure 3b TEM photographs of IDT electrodes having thickness values after performing an oxidation process are shown.
[0033] Figure 4a TEM photos and EDS images showing the oxidation process of the upper metal layer of each IDT electrode of the surface acoustic wave device according to one embodiment of the present disclosure, Figure 4b TEM photographs of IDT electrodes having thickness values after performing an oxidation process are shown.
[0034] Figure 5a and 5b : is a graph showing the relationship between the frequency change of the oxidation process performed on the upper metal layer of each IDT electrode of the surface acoustic wave device according to an embodiment of the present disclosure and each scanning rate and dwell time.
[0035] Figures 6a to 6c The peak loss, bandwidth, and frequency variation are respectively shown as a function of the dwell time of an oxidation process performed on the upper metal layer of each IDT electrode of a surface acoustic wave device according to an embodiment of the present disclosure.
[0036] Figures 7a to 7c Graph showing the XRR analysis and simulation results of the upper electrode layer and the oxidized electrode layer.
[0037] Figure 8 A surface acoustic wave device according to another embodiment of the present disclosure is shown.
[0038] Fig. 9 is a flow chart showing a method of manufacturing a surface acoustic wave device according to an embodiment of the present disclosure.
[0039] Figures 10 to 12 The intermediate steps of a method for manufacturing a surface acoustic wave device according to an embodiment of the present disclosure are shown. DETAILED DESCRIPTION
[0040] The advantages and features of the present disclosure and the methods for achieving them will become apparent by reference to the embodiments described below in conjunction with the accompanying drawings. However, the present disclosure is not limited to the embodiments disclosed below and may be embodied in various different forms. On the contrary, these embodiments are provided so that the present disclosure will be thorough and complete and the scope of the present disclosure will be fully conveyed to those skilled in the art. The scope of the present disclosure will be defined by the appended claims. Throughout the specification, similar reference numerals refer to similar components.
[0041] It should be understood that when a component is referred to as being "connected" or "coupled" to another component, it can be directly connected or coupled to the other component, or intervening components may be present. Conversely, it should be understood that when a component is referred to as being "directly connected" or "directly coupled" to another component, there are no intervening components. The term "and / or" includes any and all combinations of one or more of the associated listed items.
[0042] The terms used herein are used to describe the embodiments and are not intended to limit the present disclosure. Unless otherwise indicated in the context, singular expressions include plural expressions. As used herein, the terms "comprise", "include", "including ..." and "comprising ..." are intended to indicate the presence of the components, steps, operations and / or devices, but do not exclude the possibility of the presence or addition of one or more other components, steps, operations and / or devices.
[0043] Although terms such as first, second, etc. are used to describe various components, these components should not be limited by these terms. These terms are only used to distinguish one component from another component. Therefore, the first component mentioned below can also be the second component within the technical spirit of the present disclosure.
[0044] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs. It should be further understood that terms, such as those defined in commonly used dictionaries, will not be interpreted in an idealized or overly formal sense unless explicitly defined as such herein.
[0045] Figure 1 A surface acoustic wave device including an IDT electrode having an oxidized electrode layer formed thereon according to an embodiment of the present disclosure is shown.
[0046] Reference Figure 1 , the surface acoustic wave device 10 according to an embodiment of the present disclosure may include a plurality of IDT electrodes 200 formed on a piezoelectric substrate 100. Meanwhile, although Figure 1 Although not shown, a dielectric layer may be further formed to cover the piezoelectric substrate 100 and the plurality of IDT electrodes 200 .
[0047] The piezoelectric substrate 100 may be a multi-layer substrate that may include a plurality of layers. These layers may include, for example, a supporting substrate comprising silicon, a high acoustic velocity layer comprising amorphous silicon (a-Si) or polycrystalline silicon, a low acoustic velocity layer comprising silicon dioxide (SiO2) or aluminum nitride (AlN), and a piezoelectric layer comprising a material such as LiTaO3 (LT) or LiNbO3 (LN) located on the low acoustic velocity layer and constituting the uppermost layer, but the present disclosure is not limited thereto. In some embodiments, the piezoelectric substrate 100 may be configured by omitting at least one high acoustic velocity layer and a low acoustic velocity layer. Figure 1 In the drawings, a plurality of layers are omitted and shown as the piezoelectric substrate 100 .
[0048] A plurality of IDT electrodes 200 may be formed on the piezoelectric substrate 100. The IDT electrodes 200 may correspond to a plurality of electrodes alternately extending from two generatrixes on the surface of the piezoelectric substrate 100 that are opposite to each other.
[0049] Each IDT electrode 200 may include a conductive material, and in particular, may be divided into two or more metal layers. Figure 1 As shown, the IDT electrode 200 may include three parts: a main electrode layer 210 , an upper electrode layer 220 , and an oxidized electrode layer 230 .
[0050] The main electrode layer 210 may be formed to contact the piezoelectric substrate 100 and may include at least one metal material selected from, for example, aluminum (Al), copper (Cu), titanium (Ti), tungsten (W), molybdenum (Mo), platinum (Pt), gold (Au), etc.
[0051] The upper electrode layer 220 may be formed to cover the upper surface of the main electrode layer 210 and may include, for example, a titanium (Ti) layer or an alloy of titanium (Ti) and one or more metal materials. Alternatively, the upper electrode layer 220 may include an aluminum (Al) layer or an alloy of aluminum (Al) and one or more metal materials.
[0052] The upper electrode layer 220 can prevent oxidation of the main electrode layer 210 and reduce contact loss with the wiring layer that can be formed on the IDT electrode 200. That is, when the upper surface of the main electrode layer 210 is exposed, an oxide (e.g., aluminum oxide (Al2O3)) of the main electrode layer 210 is naturally formed, which may form a capacitive junction when in contact with the wiring layer, resulting in increased contact loss and performance degradation. Therefore, the upper electrode layer 220 can be formed on the main electrode layer 210 to minimize the contact resistance when in contact with the lower portion of the wiring layer and prevent performance degradation due to contact loss.
[0053] The oxidized electrode layer 230 may be formed on the upper surface of the upper electrode layer 220. The oxidized electrode layer 230 may be formed by oxidizing the upper electrode layer 220. Therefore, the material forming the oxidized electrode layer 230 may be an oxide of the material constituting the upper electrode layer 220. With the formation of the oxidized electrode layer 230, the density of the IDT electrode 200, especially the upper electrode layer 220 and the oxidized electrode layer 230, is reduced, the surface acoustic wave velocity is reduced, and the resonant frequency of the surface acoustic wave device 10 is moved to a low frequency. Using this principle, the frequency distribution of the surface acoustic wave device 10 according to an embodiment of the present disclosure is improved.
[0054] As described above, the resonant frequency of the surface acoustic wave device 10 can be determined by the thickness (t o ) is determined by the IDT electrode 200. Since the IDT electrode 200 is used for a higher bandwidth, it has a smaller thickness (t o ), in this case, due to the thickness of the IDT electrode 200 (t o ) changes increase toward a higher bandwidth. In extreme cases, even if the thickness of the IDT electrode 200 changes at the level of several nanometers (nm) during the thin film formation process, there are cases where the frequency distribution is several MHz or more.
[0055] By forming the IDT electrode 200 in which the main electrode layer 210 and the upper electrode layer 220 are sequentially stacked to have a desired bandwidth or more and then adjusting the frequency downward by oxidation of the upper electrode layer 220 , the yield of the surface acoustic wave device 10 satisfying the frequency margin can be improved.
[0056] In particular, in the case where the piezoelectric substrate 100 has a structure consisting of a support substrate, a high acoustic velocity layer, a low acoustic velocity layer, and a piezoelectric layer, the structure of the IDT electrode 200 according to an embodiment of the present disclosure has a greater effect. Since the piezoelectric substrate 100 including an energy confinement layer consisting of a high acoustic velocity layer and / or a low acoustic velocity layer has a very thin piezoelectric layer, it is more difficult to control the frequency distribution due to the influence of the thickness distribution of the piezoelectric layer and the thickness distribution of the energy confinement layer. Therefore, by forming a structure of the upper electrode layer 220 and the anode layer 230, such as the IDT electrode 200 included in the surface acoustic wave device 10 of the present disclosure, process control that satisfies the frequency margin can be performed.
[0057] Figure 2a The transmission electron microscope (TEM) image and energy dispersive spectrometer (EDS) image of the upper metal layer of each IDT electrode of the surface acoustic wave device before the oxidation process are shown. Figure 2b TEM images of IDT electrodes with thickness values are shown.
[0058] Reference Figure 2a, the main electrode layer 210 and the upper electrode layer 225 are stacked in sequence to form the IDT electrode 200. The main electrode layer 210 includes aluminum (Al), and the upper electrode layer 225 includes titanium (Ti). The boundary of each layer can be distinguished in the TEM photo. As shown in the EDS graph, the upper electrode layer 225 contains a certain atomic percentage (at%) of oxygen, which means that it is a natural oxide layer formed by oxidation of the upper part of the upper metal layer by oxygen in the atmosphere. As shown in the EDS graph and Figure 2b As shown, the thickness of the upper metal layer 221 is about 15.7 nanometers, and the native oxide layer is formed to have a thickness of about 4.6 nanometers.
[0059] Figure 3a TEM photos and EDS images showing the oxidation process of the upper metal layer of each IDT electrode of the surface acoustic wave device according to one embodiment of the present disclosure, Figure 3b TEM photographs of IDT electrodes having thickness values after performing an oxidation process are shown.
[0060] Reference Figure 3a , due to Figure 2a The upper metal layer 221 is oxidized to form an oxidized electrode layer 230, so that an oxidized electrode layer 230 with a thickness of about 9.1 nanometers is formed on the upper electrode layer 220. It can be seen that due to oxidation, the oxidized electrode layer 230 Figure 2a and 2b In addition to the native oxide layer of about 4.6 nanometers thick shown, a thickness of about 4.5 nanometers is added, and the top electrode layer 220 maintains a thickness of about 7.0 nanometers.
[0061] The thickness of the oxide electrode layer 230 ( Figure 1 t in o ) increases as the oxidation time of the upper metal layer 221 increases. The oxidation process of the upper metal layer 221 can be performed in various ways, but in the case of using an ion beam for the oxidation process, it can be seen that the residence time of the ion beam on each IDT electrode 200 and the power of the ion beam determine the oxidation amount of the upper metal layer 221, that is, the thickness (t o ).
[0062] In the present disclosure, it is proposed to control the residence time of the ion beam by fixing the power of the ion beam and changing the scanning rate, and adjust the thickness (t o ). Figure 3a and 3b The case where the dwell time of each IDT electrode is controlled to be 0.003 seconds is shown. When the dwell time increases, the thickness (t o ) may increase.
[0063] Figure 4aTEM photos and EDS images of the upper metal layer of the IDT electrode of the surface acoustic wave device after the oxidation process according to one embodiment of the present disclosure are shown, Figure 4b TEM photographs of IDT electrodes with thickness values after performing an oxidation process are shown.
[0064] Reference Figure 4a and 4b This embodiment corresponds to the case where the residence time is controlled to 0.02 seconds, so that the upper electrode layer 220 is completely oxidized and the oxidized electrode layer 230 is formed only on the main electrode layer 210, wherein the thickness (t o ) is 13.3 nanometers.
[0065] Therefore, the thickness (t e ), and the resonant frequency of the surface acoustic wave device 10 moves to a lower frequency. The relationship between the frequency change and each scanning rate and dwell time will be Figure 5a and 5b is described in.
[0066] Figure 5a and 5b is a graph showing a relationship between a frequency change and each scanning rate and a dwell time when an oxidation process is performed on an upper metal layer of each IDT electrode of a surface acoustic wave device according to an embodiment of the present disclosure.
[0067] Reference Figure 5a and 5b , Figure 5a shows the change in frequency (ΔFc) when the scan rate is changed, Figure 5b The change in frequency (ΔFc) when the dwell time changes is shown. As the scan rate of the ion beam increases, the time the ion beam stays on each IDT electrode 200 decreases. Therefore, the frequency change diagram according to the scan rate and the dwell time has an inverse relationship. At the same time, as the dwell time increases, that is, as the thickness of the oxidized electrode layer 230 increases, the frequency change increases, but no linear relationship is observed between the two.
[0068] In addition, if Figure 5a and 5bAs shown, the frequency change (ΔFc) caused by forming the oxidation electrode layer 230 increases from the low frequency band (LB) to the middle frequency band (MB) and the high frequency band (HB). That is, since the thickness of the IDT electrode of the high frequency band is the smallest, when the oxidation electrode layer 230 is formed using the same dwell time, the proportion of the thickness of the oxidation electrode layer 230 in the total thickness of the IDT electrode 200 increases, so its influence becomes more significant. In this case, the thickness of the oxidation electrode layer 230 can be adjusted by changing the scanning speed or dwell time of each frequency band, that is, for IDT electrodes 200 with different thicknesses.
[0069] Figures 6a to 6c The peak loss, bandwidth and frequency variation are shown as a function of the dwell time of performing an oxidation process on the upper metal layer of each IDT electrode of a surface acoustic wave device according to an embodiment of the present disclosure. It can be seen that as the dwell time increases, the variation of the peak loss (ΔPek) and bandwidth (ΔBW) also increases.
[0070] Therefore, when the oxidation process is performed, not only frequency shift occurs, but also bandwidth reduction occurs, which is due to the reduction of peak loss and electromechanical coupling factor (K2). Therefore, it is necessary to adjust the thickness (t o ).
[0071] Therefore, the frequency is adjusted by forming the oxide electrode layer 230. However, in order to meet the performance required by the surface acoustic wave device 10, the bandwidth variation is within 1%, the peak loss variation is within 0.03 dB, and the frequency variation range is determined to be within Figure 6c -2,500ppm level shown.
[0072] Table 1 below shows the results of determining the thickness range of the oxidation electrode layer 230, which satisfies the thickness (t e ) related bandwidth changes, peak loss changes, and frequency changes.
[0073] [Table 1]
[0074]
[0075]
[0076] According to the above results, the thickness of the oxide electrode layer 230 (t o ) and the thickness of the IDT electrode 200 (t e ) is expressed by the following related equation:
[0077] 0.011≤t o / t e≤0.333
[0078] Regarding the surface acoustic wave device 10 in one embodiment of the present disclosure, the density change due to the formation of the oxidized electrode layer 230 will be referred to as Figures 7a to 7c Give a description.
[0079] Figure 7a It shows that it is not executed Figure 2a and 2b FIG. 1 is a graph showing the results of XRR analysis in a state where a native oxide layer is formed by a single oxidation process.
[0080] Reference Figure 7a , shows the X-ray reflectivity (XRR) simulation result of the upper metal layer 221 before performing the oxidation process. The upper metal layer 221 including titanium (Ti) was tested, and as described above, titanium oxide (TiO2) formed of a native oxide layer was formed on the upper metal layer 221. In the upper metal layer 221, the thickness of the Ti thin film layer was measured to be 53.6 nanometers, and the density of the Ti thin film layer was measured to be 4.41 g / cm 3 The thickness of the native oxide layer was measured to be 3.4 nm, and the density of the native oxide layer was measured to be 3.70 g / cm 3 .
[0081] At the same time, refer to Figure 7b The results of XRR analysis and simulation at a scan rate of 400 mm / s and a dwell time of 0.0025 s are shown in the figure. The thickness of the Ti film layer (corresponding to the upper electrode layer 220) has almost no change and is measured to be 53.3 nm. The density of the Ti film layer is measured to be 4.41 g / cm 3 The thickness of the native oxide film was reduced to 2.4 nm and its density was measured to be 3.70 g / cm 3 Due to the oxidation process, there is an oxidized electrode layer between the native oxide layer and the Ti film layer, and its thickness and density are measured to be 2.3 nm and 3.4 g / cm 3 .
[0082] When the scanning speed is reduced, such as Figure 7c As shown in FIG. 1 (250 mm / s), the thickness of the Ti film layer (corresponding to the upper electrode layer 220) is reduced to 50.8 nm, and its density remains unchanged at 4.41 g / cm 3 The thickness of the native oxide layer was reduced to 2.5 nm and its density was measured to be 3.70 g / cm 3 Due to the oxidation process, an oxide electrode layer is formed between the native oxide film layer and the Ti thin film layer, and its thickness and density are measured to be 3.5 nm and 2.73 g / cm 3 , which means that Figure 7b Compared with , the thickness increases and the density decreases.
[0083] Therefore, the IDT electrode 200 may include an upper electrode layer 220 formed on the main electrode layer 210, and an oxidized electrode layer 230 including an oxide of the upper electrode layer 220, wherein the oxidized electrode layer 230 may be divided into a first oxidized electrode layer composed of a natural oxide layer formed after the upper electrode layer 220 is formed, and a second oxidized electrode layer formed on the upper electrode layer 220 by an oxidation process such as ion beam irradiation, and the density of the second oxidized electrode layer is lower than that of the first oxidized electrode layer.
[0084] Figure 8 A surface acoustic wave device according to another embodiment of the present disclosure is shown.
[0085] Reference Figure 8 , a surface acoustic wave device 20 according to another embodiment of the present disclosure may include a plurality of first IDT electrodes 200 and a plurality of second IDT electrodes 300 formed on a piezoelectric substrate 100. The plurality of first IDT electrodes 200 and the plurality of second IDT electrodes 300 may be formed at different regions of the piezoelectric substrate 100. For example, the plurality of first IDT electrodes 200 may be arranged at an active region defined on the piezoelectric substrate 100, and the plurality of second IDT electrodes 300 may be arranged at a wiring region defined on the piezoelectric substrate 100, and thus wiring may be additionally formed on the plurality of second IDT electrodes 300.
[0086] The first IDT electrode 200 may include three parts: a first main electrode layer 210, a first upper electrode layer 220, and a first oxidized electrode layer 230. The second IDT electrode 300 may include a second main electrode layer 310, a second upper electrode layer 320, and a second oxidized electrode layer 330. The layers constituting each of the first IDT electrode 200 and the second IDT electrode 300 may be the same as those described above with reference to FIG. Figure 1 The described configuration of layers constituting the IDT electrode 200 is similar.
[0087] However, the thickness (t e1 ) and the thickness (t e2 ) may be different from each other. Specifically, the thickness (t e2 ) may be greater than the thickness (t e1 ). As described above, the IDT electrode can be adjusted to control the center frequency of the surface acoustic wave device. In particular, in order to have a high-band center frequency, it is necessary to form the IDT electrode thinner.
[0088] Therefore, in a surface acoustic wave device 20 according to an embodiment of the present disclosure, a filter having a first center frequency can be provided on a piezoelectric substrate 100 through a plurality of first IDT electrodes 200, and a filter having a second center frequency can be provided through a plurality of second IDT electrodes 300, wherein the first center frequency may be higher than the second center frequency.
[0089] In addition, as described above, the center frequency is adjusted during the formation of the first oxidation electrode layer 230 and the second oxidation electrode layer 330, and the thickness of the first oxidation electrode layer 230 and the second oxidation electrode layer 330 also needs to be changed according to the thickness of the first IDT electrode 200 and the second IDT electrode 300, so as to control the peak loss and bandwidth to be reduced within a specific range. Specifically, the thickness of the first oxidation electrode layer 230 (t o1 ) may be smaller than the thickness of the second oxide electrode layer 330 (t o2 ). Therefore, in the oxidation process, the ion beam irradiation rate of the first IDT electrode 200 may be higher than the irradiation rate of the second IDT electrode 300.
[0090] like Figures 7a to 7c As shown, as the irradiance decreases and the thickness of the oxidized electrode layer increases, the density of the oxidized electrode layer decreases. Therefore, the density of the first oxidized electrode layer 230 may be greater than the density of the second oxidized electrode layer 330.
[0091] The thickness of the first oxide electrode layer 230 (t o1 ) and the thickness of the first IDT electrode 200 (t e1 ) can satisfy the following related equation:
[0092] 0.011≤t o1 / t e1 ≤0.333
[0093] The thickness of the second oxide electrode layer 330 (t o2 ) and the thickness of the second IDT electrode 300 (t e2 ) can satisfy the following related equation:
[0094] 0.011≤t o2 / t e2 ≤0.333
[0095] Fig. 9 is a flow chart illustrating a method of manufacturing a surface acoustic wave device according to an embodiment of the present disclosure.
[0096] Reference Fig. 9According to an embodiment of the present disclosure, a method for manufacturing a surface acoustic wave device includes the following steps: S110 preparing a piezoelectric substrate; S120 forming an IDT electrode film including a main electrode layer and an upper electrode layer on the piezoelectric substrate; S130 forming an oxidized electrode layer by oxidizing the upper surface of the upper electrode layer; and S140 forming an IDT electrode by patterning the IDT electrode film.
[0097] Figures 10 to 12 Intermediate steps of a method for manufacturing a surface acoustic wave device according to an embodiment of the present disclosure are shown.
[0098] First, refer to Fig.10 , prepare a piezoelectric substrate S110. The piezoelectric substrate 100 may be a multi-layer substrate and may include a plurality of layers. These layers may include, for example, a support substrate including silicon, a high acoustic velocity layer including materials such as amorphous silicon or polycrystalline silicon, a low acoustic velocity layer including materials such as silicon dioxide or aluminum nitride, and a piezoelectric layer including materials such as LT or LN located on the low acoustic velocity layer to form the uppermost layer, but the present disclosure is not limited thereto. In some embodiments, the piezoelectric substrate 100 may be configured by omitting at least one high acoustic velocity layer and a low acoustic velocity layer.
[0099] The piezoelectric substrate 100 may be formed by, for example, sequentially forming the above-described high acoustic velocity layer, low acoustic velocity layer, and piezoelectric layer on a support substrate or by a process of combining at least one layer with other layers.
[0100] Reference Fig.11 , an IDT electrode film 201S120 including a main electrode layer 211 and an upper electrode layer 221 is formed on the piezoelectric substrate 100. The main electrode layer 211 can be formed by radio frequency (RF) sputtering or electron beam deposition of at least one metal material, such as aluminum (Al), copper (Cu), titanium (Ti), tungsten (W), molybdenum (Mo), platinum (Pt), gold (Au), etc., and the upper electrode layer 221 can be formed by radio frequency (RF) sputtering or electron beam deposition, such as titanium (Ti) or an alloy of titanium (Ti) and one or more metal materials.
[0101] at the same time, Fig.11 The manufacturing method shown is used to explain the subsequent conventional patterning process, including forming a photoresist on the IDT electrode film 201 by exposure and development, and using the photoresist as an etching mask to form the IDT electrode 200. In some other embodiments, the manufacturing method of the present disclosure may include forming the IDT electrode 200 by a lift-off process. In this case, for the lift-off process, it is possible to first form a photoresist on the piezoelectric substrate 100 by exposure and development, and then form the IDT electrode film 201 to cover the photoresist and the surface of the piezoelectric substrate 100 selectively exposed by the photoresist.
[0102] Reference Fig.12The oxidized electrode layer 231 is formed by oxidizing (O) the upper surface of the upper electrode layer 221 (S130). For example, the oxidized electrode layer 231 may be formed by oxidizing the upper electrode layer 221 by irradiating the upper surface of the upper electrode layer 221 with an ion beam.
[0103] At this time, the thickness of the oxidized electrode layer 231 can be controlled by controlling the scanning rate (or dwell time) of ion beam irradiation. The dwell time of the ion beam on one IDT electrode film 201 is determined according to the scanning rate, so the thickness of the oxidized electrode layer 231 can also be controlled.
[0104] Reference Figure 1 The IDT electrode 200 is formed by patterning the IDT electrode film 201 S140. Patterning the IDT electrode film 201 may include, for example, etching the IDT electrode film 201 using a photoresist pattern formed on the IDT electrode film 201 as an etching mask.
[0105] Alternatively, in the case of the above-described lift-off process, the IDT electrode 200 may be formed by removing a photoresist pattern formed on the piezoelectric substrate 100 and a portion of the IDT electrode film 201 formed on the photoresist pattern.
[0106] Through the above-mentioned manufacturing process, a surface acoustic wave device in which many characteristics of the filter including the center frequency have been controlled can be manufactured. In this case, the thickness (t o ) and the thickness of the IDT electrode 200 (t e ) satisfies 0.011≤t o / t e ≤0.333.
[0107] At the same time, if Figure 8 The surface acoustic wave device 20 of another embodiment of the present disclosure shown includes a first IDT electrode 200 and a second IDT electrode 200 formed on a piezoelectric substrate 100, which have different thicknesses. In order to manufacture such a surface acoustic wave device 20, a first IDT electrode film and a second IDT electrode film having different thicknesses are formed in a first region and a second region defined on the piezoelectric substrate 100, respectively, and the IDT electrode film can be subjected to an oxidation process at different scanning rates to form a first oxidized electrode layer 230 and a second oxidized electrode layer 330 having different thicknesses. In this case, the thickness (t o1 ) may be higher than the scanning rate (t o2 ) of the ion beam irradiation.
[0108] Although the present disclosure has been described with reference to specific exemplary embodiments, it will be appreciated by those skilled in the art that the present disclosure may be embodied in other specific forms without departing from the technical spirit or essential features of the present disclosure. Therefore, the above embodiments are considered to be illustrative and not restrictive in all aspects.
Claims
1. A surface acoustic wave device, characterized in that: include: Piezoelectric substrate; as well as a plurality of IDT electrodes formed on the piezoelectric substrate, Wherein, each of the plurality of IDT electrodes comprises: A main electrode layer formed on the upper surface of the piezoelectric substrate; an upper electrode layer formed on the main electrode layer; and an oxidized electrode layer formed on an upper surface of the upper electrode layer by oxidation of the upper electrode layer, The thickness of each of the plurality of IDT electrodes (t e ) relative to the thickness of the oxide electrode layer (t o ) satisfies 0.011≤t o / t e ≤0.
333.
2. The surface acoustic wave device according to claim 1, characterized in that The oxidized electrode layer comprises: a first oxidized electrode layer having a first density and forming an upper portion of the oxidized electrode layer; and The second oxidized electrode layer has a second density lower than the first density and is located below the first oxidized electrode layer.
3. The surface acoustic wave device according to claim 2, characterized in that: The first oxidized electrode layer is a natural oxide layer, and the second oxidized electrode layer is formed by an oxidation process of irradiating an upper electrode layer with an ion beam.
4. The surface acoustic wave device according to claim 1, characterized in that The upper electrode layer includes titanium (Ti), and the oxidized electrode layer includes titanium oxide.
5. The surface acoustic wave device according to claim 1, characterized in that: The upper electrode layer includes aluminum (Al), and the oxidized electrode layer includes aluminum oxide.
6. The surface acoustic wave device according to claim 1, characterized in that The main electrode layer includes at least one metal material selected from aluminum (Al), copper (Cu), titanium (Ti), tungsten (W), molybdenum (Mo), platinum (Pt), and gold (Au).
7. A surface acoustic wave device, characterized in that: include: a piezoelectric substrate having a first region and a second region defined thereon; a plurality of first IDT electrodes formed in the first region; as well as a plurality of second IDT electrodes formed in the second region, Each of the plurality of first IDT electrodes has a first thickness and includes: A first main electrode layer formed on an upper surface of the piezoelectric substrate in the first region; a first upper electrode layer formed on the first main electrode layer; and a first oxidized electrode layer formed on an upper surface of the first upper electrode layer by oxidation of the first upper electrode layer, Each of the plurality of second IDT electrodes has a second thickness and includes: a second main electrode layer formed on the upper surface of the piezoelectric substrate in the second region; a second upper electrode layer formed on the second main electrode layer; as well as a second oxidized electrode layer formed on an upper surface of the second upper electrode layer by oxidation of the second upper electrode layer, The first thickness and the second thickness are different.
8. The surface acoustic wave device according to claim 7, characterized in that: The plurality of first IDT electrodes correspond to a first center frequency, the plurality of second IDT electrodes correspond to a second center frequency lower than the first center frequency, and the first thickness is smaller than the second thickness.
9. The surface acoustic wave device according to claim 8, characterized in that: The thickness of the first oxidized electrode layer is smaller than the thickness of the second oxidized electrode layer.
10. The surface acoustic wave device according to claim 9, characterized in that: The first thickness (t e1 ) relative to the thickness of the first oxide electrode layer (t o1 ) satisfies 0.011≤t o1 / t e1 ≤0.333, the second thickness (te2) is relative to the thickness of the second oxide electrode layer (t o2 ) satisfies 0.011≤t o2 / t e2 ≤0.
333.
11. The surface acoustic wave device according to claim 9, characterized in that The density of the first oxidized electrode layer is greater than the density of the second oxidized electrode layer.
12. A method for manufacturing a surface acoustic wave device, characterized in that: The following steps are involved: Preparing a piezoelectric substrate; forming an IDT electrode film including a main electrode layer and an upper electrode layer on a piezoelectric substrate; forming an oxidized electrode layer by oxidizing an upper surface of the upper electrode layer; and The IDT electrode is formed by patterning the IDT electrode film.
13. The method for manufacturing a surface acoustic wave device according to claim 12, characterized in that: The step of forming the oxidized electrode layer by oxidizing the upper surface of the upper electrode layer includes the step of forming the oxidized electrode layer by irradiating the upper electrode layer with an ion beam.
14. The method for manufacturing a surface acoustic wave device according to claim 12, characterized in that: The piezoelectric substrate has a first region and a second region defined thereon, The step of forming the IDT electrode film includes: forming a first IDT electrode film having a first thickness in the first region, and forming a second IDT electrode film having a second thickness in the second region. The first thickness and the second thickness are different.
15. The method for manufacturing a surface acoustic wave device according to claim 14, characterized in that: The step of forming an oxidized electrode layer by oxidizing the upper surface of the upper electrode layer comprises: forming a first oxidized electrode layer by irradiating an upper surface of a first upper electrode layer included in a first IDT electrode film with an ion beam at a first scanning rate; as well as The second oxidized electrode layer is formed by irradiating an upper surface of a second upper electrode layer included in the second IDT electrode film with an ion beam at a second scanning rate different from the first scanning rate.
16. The method for manufacturing a surface acoustic wave device according to claim 15, characterized in that: The thickness of the first IDT electrode and the thickness of the first oxidized electrode layer are respectively smaller than the thickness of the second IDT electrode and the thickness of the second oxidized electrode layer. The first IDT electrode corresponds to a first center frequency, and the second IDT electrode corresponds to a second center frequency lower than the first center frequency.
17. The method for manufacturing a surface acoustic wave device according to claim 16, characterized in that: The density of the first oxidized electrode layer is greater than the density of the second oxidized electrode layer.
18. The method for manufacturing a surface acoustic wave device according to claim 12, characterized in that: The upper electrode layer includes titanium (Ti), and the oxidized electrode layer includes titanium oxide.
19. The method for manufacturing a surface acoustic wave device according to claim 12, characterized in that: The upper electrode layer includes aluminum (Al), and the oxidized electrode layer includes aluminum oxide.
20. The method for manufacturing a surface acoustic wave device according to claim 12, characterized in that: The main electrode layer includes at least one metal material selected from aluminum (Al), copper (Cu), titanium (Ti), tungsten (W), molybdenum (Mo), platinum (Pt), and gold (Au).