Aluminum alloy investment casting shell
By adopting a multi-layer structure of aluminum alloy investment casting molded shells in aluminum alloy investment casting, the combination of silicon sol, water, corundum powder, talc powder and chromite sand is solved, the problem of poor thermal conductivity of traditional shells is solved. The tensile strength and elongation after break of aluminum alloy parts are improved, achieving more efficient sand cleaning and performance improvement.
Patent Information
- Application Number
- CN202411196859.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional gypsum casting and ceramic shells have poor breathability, thermal conductivity and dispersion in aluminum alloy investment casting, resulting in a decrease in the tensile strength and elongation after breaking of aluminum alloy parts, limiting the application range of investment casting process. .
Aluminum alloy investment cast shell consisting of a surface layer, transition layer, reinforcement layer and sealing layer is adopted to form specific coating formulations and hierarchies, including silicon sol, water, corundum powder, talc, coal powder and ferrochrome Ore sand optimizes the structure and material combination of the shell to improve its collapse, breathability and thermal conductivity.
It significantly improves the comprehensive performance of the aluminum alloy investment cast molded shell, solves the performance degradation caused by poor thermal conductivity, and improves sand cleaning efficiency, ensuring that the tensile strength and elongation after break of the aluminum alloy reach or exceeds that of the traditional shell. 1.27 times and 1.83 times.
Smart Images

Figure BDA0005016698290000101 
Figure BDA0005016698290000111
Abstract
Description
Technical Field
[0001] The invention relates to the field of investment casting, and in particular to an aluminum alloy investment casting shell. Background Art
[0002] Investment casting is an advanced process of near-net-shape forming, which is more suitable for the production of small and medium-sized complex precision castings. The materials of the castings cover carbon steel, stainless steel, high-temperature alloys, cast iron, copper alloys, aluminum alloys, magnesium alloys and titanium alloys, etc. Its main process flow is to repeatedly dip paint, sprinkle sand and dry the surface of a disposable fusible mold (usually a wax mold) to form a shell of a certain thickness. After the processes of shell dewaxing, shell roasting, pouring molten metal, solidification cooling and shelling, the precision casting is obtained.
[0003] When using the investment casting process to produce aluminum alloy castings, the industry mainly uses gypsum molds or traditional ceramic shells (i.e., traditional investment casting shells), both of which have inherent deficiencies. The advantage of gypsum molds is good disintegration, but the disadvantage is poor air permeability and thermal conductivity. The use of grouting molding to make molds consumes a lot of raw materials, and the mold roasting needs to be heated and kept warm according to a special temperature control curve. The process is relatively complicated and the production flexibility is poor. The advantage of traditional investment casting shells is good production flexibility, but the disadvantage is that the shells have poor air permeability, thermal conductivity, and disintegration, the efficiency of shell sand cleaning is low, and compared with metal molds, the investment casting shells have poor thermal conductivity, which brings the most direct problem of reduced comprehensive performance of aluminum alloy parts, and the tensile strength and elongation after fracture will drop by more than 10%. The existence of these problems restricts the application scope of aluminum alloy investment casting process. Summary of the invention
[0004] In order to overcome the above-mentioned technical problems, the purpose of the present invention is to provide an aluminum alloy investment casting mold shell, which solves the problems that the traditional investment casting mold shell has poor air permeability, thermal conductivity and collapsibility, low mold shell sand cleaning efficiency, and poor thermal conductivity, resulting in a significant decrease in the tensile strength and elongation after fracture of the aluminum alloy parts.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] An aluminum alloy investment casting shell, the aluminum alloy investment casting shell consisting of a surface layer, a transition layer, a reinforcement layer and a sealing slurry layer;
[0007] The aluminum alloy investment casting shell is prepared by the following steps:
[0008] Step S10: weighing raw materials according to the surface coating formula to prepare the surface coating;
[0009] Step S20: evenly coating the wax mold module with a surface coating, then sprinkling chromite sand with a particle size of 60-80 mesh, and then placing the wax mold module sprinkled with chromite sand in a drying room for drying and solidifying to form a surface layer, thereby obtaining a surface layer mold shell;
[0010] Step S30: weighing raw materials according to the transition layer coating formula to prepare a transition layer coating;
[0011] Step S40: uniformly coating the surface shell with a transition layer coating, then sprinkling chromite sand with a particle size of 30-60 mesh, and then placing the surface shell with the chromite sand in a drying room for drying and solidifying to form a transition layer, thereby obtaining a transition layer mold shell;
[0012] Step S50: weighing raw materials according to the reinforcement layer coating formula to prepare a reinforcement layer coating;
[0013] Step S60: uniformly coating the transition layer shell with the reinforcement layer coating, and then sprinkling chromite sand with a particle size of 16-30 mesh, and then placing the transition layer shell sprinkled with the chromite sand in a drying room for drying, solidifying to form a reinforcement layer, and obtaining a reinforcement layer mold shell;
[0014] Step S70: weighing raw materials according to the formula of the sealing layer coating to prepare the sealing layer coating;
[0015] Step S80: uniformly coating the reinforcement layer shell with a sealing layer coating, and then placing it in a drying room for drying and solidifying to form a sealing layer, thereby obtaining a sealing layer mold shell;
[0016] Step S90: dewaxing and calcining the sealing layer mold shell to obtain an aluminum alloy investment casting mold shell.
[0017] As a further solution of the present invention: the surface coating formula in step S10 includes the following components in parts by weight:
[0018] 10 parts of silica sol, 11-18 parts of water, 54-67 parts of corundum powder, 4-6 parts of talc, 2-3 parts of coal powder, 0.02-0.03 parts of carboxymethyl cellulose, 0.03-0.04 parts of wetting agent, 0.04-0.05 parts of defoaming agent, and 0.05-0.07 parts of bactericide.
[0019] As a further solution of the present invention: the conductivity of the silica sol in the surface coating formula in step S10 is 3.0-5.6ms / cm; the wetting agent is one of wetting agent wet245, wetting agent wet270 and wetting agent wet510; the defoaming agent is one of defoaming agent BYK-024, defoaming agent BYK-028 and defoaming agent BYK-530; the bactericide is one of bactericide CL-39, bactericide CL-129 and bactericide MD-146.
[0020] As a further solution of the present invention: the transition layer coating formula in step S30 includes the following components in parts by weight:
[0021] 12 parts of silica sol, 13-22 parts of water, 50-61 parts of corundum powder, 5-6.5 parts of talc, 2.5-3.5 parts of coal powder, 0.02-0.03 parts of carboxymethyl cellulose, 0.02-0.03 parts of wetting agent, 0.03-0.04 parts of defoaming agent, and 0.05-0.07 parts of bactericide.
[0022] As a further solution of the present invention: the conductivity of the silica sol in the transition layer coating formula in step S30 is 3.0-5.6ms / cm; the wetting agent is one of wetting agent wet245, wetting agent wet270 and wetting agent wet510; the defoaming agent is one of defoaming agent BYK-024, defoaming agent BYK-028 and defoaming agent BYK-530; the bactericide is one of bactericide CL-39, bactericide CL-129 and bactericide MD-146.
[0023] As a further solution of the present invention: the reinforcement layer coating formula in step S50 includes the following components in parts by weight:
[0024] 28 parts of silica sol, 62-68 parts of corundum powder, 5.2-6.0 parts of talc, 6.2-6.8 parts of coal powder, 0.02-0.03 parts of carboxymethyl cellulose, 0.02-0.03 parts of wetting agent, 0.03-0.04 parts of defoaming agent, and 0.04-0.06 parts of bactericide.
[0025] As a further solution of the present invention: the conductivity of the silica sol in the reinforcement layer coating formula in step S50 is 3.0-5.6ms / cm; the wetting agent is one of wetting agent wet245, wetting agent wet270 and wetting agent wet510; the defoaming agent is one of defoaming agent BYK-024, defoaming agent BYK-028 and defoaming agent BYK-530; the bactericide is one of bactericide CL-39, bactericide CL-129 and bactericide MD-146.
[0026] As a further solution of the present invention: the sealing layer coating formula in step S70 includes the following components in parts by weight:
[0027] 28 parts of silica sol, 62-68 parts of corundum powder, 5.2-6.0 parts of talc, 6.2-6.8 parts of coal powder, 0.02-0.03 parts of carboxymethyl cellulose, 0.02-0.03 parts of wetting agent, 0.03-0.04 parts of defoaming agent, and 0.04-0.06 parts of bactericide.
[0028] As a further solution of the present invention: the conductivity of the silica sol in the sealing layer coating formula in step S70 is 3.0-5.6ms / cm; the wetting agent is one of wetting agent wet245, wetting agent wet270 and wetting agent wet510; the defoaming agent is one of defoaming agent BYK-024, defoaming agent BYK-028 and defoaming agent BYK-530; the bactericide is one of bactericide CL-39, bactericide CL-129 and bactericide MD-146.
[0029] Beneficial effects of the present invention:
[0030] The aluminum alloy investment casting mold shell of the present invention improves the comprehensive performance of the aluminum alloy investment casting mold shell through the optimized combination of several materials. The mold shell has good disintegration, air permeability and thermal conductivity, effectively solving the problem of poor thermal conductivity of traditional mold shells leading to decreased performance of the aluminum alloy, and also solving the problem of low sand cleaning efficiency after pouring.
[0031] Silica sol is used as the main binder and water as the diluent, which can reduce the viscosity and bonding strength of silica sol. Corundum powder, talcum powder and chromite sand are mold shell aggregates. Coal powder burns to form micropores during the shell roasting process, which can improve the shell's disintegration and air permeability. The heat generated by the combustion can shorten the shell roasting time. Carboxymethyl cellulose plays the role of thickening, suspension, moisture retention and crack prevention and auxiliary binder. The main function of talcum powder is to adjust the thermal conductivity of the coating so that the shell has a suitable thermal conductivity, ensuring that its thermal conductivity is much higher than that of the traditional shell, while preventing the chromite sand from causing cold shut and insufficient pouring defects in the casting due to excessive chilling; another function of talcum powder is to improve the dispersibility of the coating and reduce stirring resistance and energy consumption.
[0032] During the technical development process, the present invention found that the collapsibility of the aluminum alloy shell surface layer and transition layer determines the collapsibility of the entire shell. Based on this discovery, the coating formula is designed according to the general idea of "weak at the front and strong at the back", which is exactly the opposite of the traditional shell idea of "strong at the front and weak at the back", which greatly improves the comprehensive performance of the shell. The combination of silica sol, water, corundum powder and coal powder makes the surface layer and transition layer have very good collapsibility and air permeability; the reinforcement layer is made of silica sol stock solution, corundum powder and coal powder to ensure that the coating has good strength and air permeability; the three materials with large differences in thermal conductivity, corundum powder, talcum powder and chromite sand, are optimized and combined to ensure that the shell has good thermal conductivity and filling performance. DETAILED DESCRIPTION
[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Embodiment 1:
[0035] This embodiment is a method for preparing an aluminum alloy investment casting shell, comprising the following steps:
[0036] Step S10: weighing raw materials according to the surface coating formula to prepare the surface coating;
[0037] The surface coating formula includes the following components in parts by weight:
[0038] 10 parts of silica sol, 11 parts of water, 54 parts of corundum powder, 4 parts of talc, 2 parts of coal powder, 0.02 parts of carboxymethyl cellulose, 0.03 parts of wetting agent, 0.04 parts of defoaming agent, 0.05 parts of bactericide;
[0039] The conductivity of the silica sol is 3.0 ms / cm; the wetting agent is wetting agent wet245; the defoaming agent is defoaming agent BYK-024; the bactericide is bactericide CL-39;
[0040] Step S20: evenly coating the wax mold module with a surface coating, then sprinkling chromite sand with a particle size of 60 mesh, and then placing the wax mold module sprinkled with chromite sand in a drying room for drying and solidifying to form a surface layer, thereby obtaining a surface layer mold shell;
[0041] Step S30: weighing raw materials according to the transition layer coating formula to prepare a transition layer coating;
[0042] The transition layer coating formula includes the following components in parts by weight:
[0043] 12 parts of silica sol, 13 parts of water, 50 parts of corundum powder, 5 parts of talc, 2.5 parts of coal powder, 0.02 parts of carboxymethyl cellulose, 0.02 parts of wetting agent, 0.03 parts of defoaming agent, 0.05 parts of bactericide;
[0044] The conductivity of the silica sol is 3.0 ms / cm; the wetting agent is wetting agent wet245; the defoaming agent is defoaming agent BYK-024; the bactericide is bactericide CL-39;
[0045] Step S40: uniformly coating the surface shell with a transition layer coating, and then sprinkling chromite sand with a particle size of 30 meshes, and then placing the surface shell with the chromite sand in a drying room for drying, solidifying to form a transition layer, and obtaining a transition layer mold shell;
[0046] Step S50: weighing raw materials according to the reinforcement layer coating formula to prepare a reinforcement layer coating;
[0047] The reinforcement layer coating formula includes the following components in parts by weight:
[0048] 28 parts of silica sol, 62 parts of corundum powder, 5.2 parts of talc, 6.2 parts of coal powder, 0.03 parts of carboxymethyl cellulose, 0.02 parts of wetting agent, 0.03 parts of defoaming agent, 0.04 parts of bactericide;
[0049] The conductivity of the silica sol is 3.0 ms / cm; the wetting agent is wetting agent wet245; the defoaming agent is defoaming agent BYK-024; the bactericide is bactericide CL-39;
[0050] Step S60: uniformly coating the transition layer shell with the reinforcement layer coating, and then sprinkling chromite sand with a particle size of 16 meshes, and then placing the transition layer shell sprinkled with the chromite sand in a drying room for drying, solidifying to form a reinforcement layer, and obtaining a reinforcement layer mold shell;
[0051] Step S70: weighing raw materials according to the formula of the sealing layer coating to prepare the sealing layer coating;
[0052] The sealing layer coating formula comprises the following components in parts by weight:
[0053] 28 parts of silica sol, 62 parts of corundum powder, 5.2 parts of talc, 6.2 parts of coal powder, 0.03 parts of carboxymethyl cellulose, 0.02 parts of wetting agent, 0.03 parts of defoaming agent, 0.04 parts of bactericide;
[0054] The conductivity of the silica sol is 3.0 ms / cm; the wetting agent is wetting agent wet245; the defoaming agent is defoaming agent BYK-024; the bactericide is bactericide CL-39;
[0055] Step S80: uniformly coating the reinforcement layer shell with a sealing layer coating, and then placing it in a drying room for drying and solidifying to form a sealing layer, thereby obtaining a sealing layer mold shell;
[0056] Step S90: dewaxing and calcining the sealing layer mold shell to obtain an aluminum alloy investment casting mold shell.
[0057] Embodiment 2:
[0058] This embodiment is a method for preparing an aluminum alloy investment casting shell, comprising the following steps:
[0059] Step S10: weighing raw materials according to the surface coating formula to prepare the surface coating;
[0060] The surface coating formula includes the following components in parts by weight:
[0061] 10 parts of silica sol, 15 parts of water, 61 parts of corundum powder, 5 parts of talc, 2.5 parts of coal powder, 0.025 parts of carboxymethyl cellulose, 0.035 parts of wetting agent, 0.045 parts of defoaming agent, 0.06 parts of bactericide;
[0062] The conductivity of the silica sol is 4.3 ms / cm; the wetting agent is wetting agent wet270; the defoaming agent is defoaming agent BYK-028; the bactericide is bactericide CL-129;
[0063] Step S20: evenly coating the wax mold module with a surface coating, then sprinkling chromite sand with a particle size of 70 mesh, and then placing the wax mold module sprinkled with chromite sand in a drying room for drying and solidifying to form a surface layer, thereby obtaining a surface layer mold shell;
[0064] Step S30: weighing raw materials according to the transition layer coating formula to prepare a transition layer coating;
[0065] The transition layer coating formula includes the following components in parts by weight:
[0066] 12 parts of silica sol, 18 parts of water, 56 parts of corundum powder, 6 parts of talc, 3 parts of coal powder, 0.025 parts of carboxymethyl cellulose, 0.025 parts of wetting agent, 0.035 parts of defoaming agent, 0.06 parts of bactericide;
[0067] The conductivity of the silica sol is 4.3 ms / cm; the wetting agent is wetting agent wet270; the defoaming agent is defoaming agent BYK-028; the bactericide is bactericide CL-129;
[0068] Step S40: uniformly coating the surface shell with a transition layer coating, then sprinkling chromite sand with a particle size of 45 mesh, and then placing the surface shell with the chromite sand in a drying room for drying and solidifying to form a transition layer, thereby obtaining a transition layer mold shell;
[0069] Step S50: weighing raw materials according to the reinforcement layer coating formula to prepare a reinforcement layer coating;
[0070] The reinforcement layer coating formula includes the following components in parts by weight:
[0071] 28 parts of silica sol, 65 parts of corundum powder, 5.6 parts of talc, 6.5 parts of coal powder, 0.025 parts of carboxymethyl cellulose, 0.025 parts of wetting agent, 0.035 parts of defoaming agent, 0.05 parts of bactericide;
[0072] The conductivity of the silica sol is 4.3 ms / cm; the wetting agent is wetting agent wet270; the defoaming agent is defoaming agent BYK-028; the bactericide is bactericide CL-129;
[0073] Step S60: uniformly coating the transition layer shell with the reinforcement layer coating, and then sprinkling chromite sand with a particle size of 23 meshes, and then placing the transition layer shell sprinkled with the chromite sand in a drying room for drying, solidifying to form a reinforcement layer, and obtaining a reinforcement layer mold shell;
[0074] Step S70: weighing raw materials according to the formula of the sealing layer coating to prepare the sealing layer coating;
[0075] The sealing layer coating formula comprises the following components in parts by weight:
[0076] 28 parts of silica sol, 65 parts of corundum powder, 5.6 parts of talc, 6.5 parts of coal powder, 0.025 parts of carboxymethyl cellulose, 0.025 parts of wetting agent, 0.035 parts of defoaming agent, 0.05 parts of bactericide;
[0077] The conductivity of the silica sol is 4.3 ms / cm; the wetting agent is wetting agent wet270; the defoaming agent is defoaming agent BYK-028; the bactericide is bactericide CL-129;
[0078] Step S80: uniformly coating the reinforcement layer shell with a sealing layer coating, and then placing it in a drying room for drying and solidifying to form a sealing layer, thereby obtaining a sealing layer mold shell;
[0079] Step S90: dewaxing and calcining the sealing layer mold shell to obtain an aluminum alloy investment casting mold shell.
[0080] Embodiment 3:
[0081] This embodiment is a method for preparing an aluminum alloy investment casting shell, comprising the following steps:
[0082] Step S10: weighing raw materials according to the surface coating formula to prepare the surface coating;
[0083] The surface coating formula includes the following components in parts by weight:
[0084] 10 parts of silica sol, 18 parts of water, 67 parts of corundum powder, 6 parts of talc, 3 parts of coal powder, 0.03 parts of carboxymethyl cellulose, 0.04 parts of wetting agent, 0.05 parts of defoaming agent, 0.07 parts of bactericide;
[0085] The conductivity of the silica sol is 5.6 ms / cm; the wetting agent is wetting agent wet510; the defoaming agent is defoaming agent BYK-530; the bactericide is bactericide MD-146;
[0086] Step S20: evenly coating the wax mold module with a surface coating, then sprinkling chromite sand with a particle size of 80 mesh, and then placing the wax mold module sprinkled with the chromite sand in a drying room for drying and solidifying to form a surface layer, thereby obtaining a surface layer mold shell;
[0087] Step S30: weighing raw materials according to the transition layer coating formula to prepare a transition layer coating;
[0088] The transition layer coating formula includes the following components in parts by weight:
[0089] 12 parts of silica sol, 22 parts of water, 61 parts of corundum powder, 6.5 parts of talc, 3.5 parts of coal powder, 0.03 parts of carboxymethyl cellulose, 0.03 parts of wetting agent, 0.04 parts of defoaming agent, 0.07 parts of bactericide;
[0090] The conductivity of the silica sol is 5.6 ms / cm; the wetting agent is wetting agent wet510; the defoaming agent is defoaming agent BYK-530; the bactericide is bactericide MD-146;
[0091] Step S40: uniformly coating the surface shell with a transition layer coating, then sprinkling chromite sand with a particle size of 60 mesh, and then placing the surface shell with the chromite sand in a drying room for drying and solidifying to form a transition layer, thereby obtaining a transition layer mold shell;
[0092] Step S50: weighing raw materials according to the reinforcement layer coating formula to prepare a reinforcement layer coating;
[0093] The reinforcement layer coating formula includes the following components in parts by weight:
[0094] 28 parts of silica sol, 68 parts of corundum powder, 6.0 parts of talc, 6.8 parts of coal powder, 0.02 parts of carboxymethyl cellulose, 0.03 parts of wetting agent, 0.04 parts of defoaming agent, 0.06 parts of bactericide;
[0095] The conductivity of the silica sol is 5.6 ms / cm; the wetting agent is wetting agent wet510; the defoaming agent is defoaming agent BYK-530; the bactericide is bactericide MD-146;
[0096] Step S60: uniformly coating the transition layer shell with the reinforcement layer coating, and then sprinkling chromite sand with a particle size of 30 meshes, and then placing the transition layer shell sprinkled with the chromite sand in a drying room for drying, solidifying to form a reinforcement layer, and obtaining a reinforcement layer mold shell;
[0097] Step S70: weighing raw materials according to the formula of the sealing layer coating to prepare the sealing layer coating;
[0098] The sealing layer coating formula comprises the following components in parts by weight:
[0099] 28 parts of silica sol, 68 parts of corundum powder, 6.0 parts of talc, 6.8 parts of coal powder, 0.02 parts of carboxymethyl cellulose, 0.03 parts of wetting agent, 0.04 parts of defoaming agent, 0.06 parts of bactericide;
[0100] The conductivity of the silica sol is 5.6 ms / cm; the wetting agent is wetting agent wet510; the defoaming agent is defoaming agent BYK-530; the bactericide is bactericide MD-146;
[0101] Step S80: uniformly coating the reinforcement layer shell with a sealing layer coating, and then placing it in a drying room for drying and solidifying to form a sealing layer, thereby obtaining a sealing layer mold shell;
[0102] Step S90: dewaxing and calcining the sealing layer mold shell to obtain an aluminum alloy investment casting mold shell.
[0103] Production verification:
[0104] Three groups of ZL101A aluminum alloy castings were produced using the aluminum alloy investment casting shells of Example 1, Example 2 and Example 3, respectively. At the same time, three groups of ZL101A aluminum alloy castings were produced using the traditional investment casting shell as a control group. The sand cleaning effect was compared and verified by a 10-minute sandblasting method. After the castings were subjected to T6 heat treatment, the body test bars were taken for mechanical property comparison and verification. The verification results are shown in the following table:
[0105]
[0106]
[0107] The qualification judgment method is as follows: when the tensile strength is ≥275MPa and the elongation after fracture is ≥2, it is qualified; when the tensile strength is <275MPa or the elongation after fracture is <2, it is unqualified;
[0108] From the above comparative verification results, it can be seen that the mechanical properties of the embodiments of the present invention are qualified, the average tensile strength is 1.27 times the average of the control group, and the elongation after fracture is 1.83 times the average of the control group. Under the same conditions, the sand cleaning effect of the mold shell of the present invention is far better than that of the traditional mold shell.
[0109] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0110] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. An aluminum alloy investment casting shell, characterized in that: The aluminum alloy investment casting shell is composed of a surface layer, a transition layer, a reinforcement layer and a sealing layer; The aluminum alloy investment casting shell is prepared by the following steps: Step S10: weighing raw materials according to the surface coating formula to prepare the surface coating; Step S20: evenly coating the wax mold module with a surface coating, then sprinkling chromite sand with a particle size of 60-80 mesh, and then placing the wax mold module sprinkled with chromite sand in a drying room for drying and solidifying to form a surface layer, thereby obtaining a surface layer mold shell; Step S30: weighing raw materials according to the transition layer coating formula to prepare a transition layer coating; Step S40: uniformly coating the surface shell with a transition layer coating, then sprinkling chromite sand with a particle size of 30-60 mesh, and then placing the surface shell with the chromite sand in a drying room for drying and solidifying to form a transition layer, thereby obtaining a transition layer mold shell; Step S50: weighing raw materials according to the reinforcement layer coating formula to prepare a reinforcement layer coating; Step S60: uniformly coating the transition layer shell with the reinforcement layer coating, and then sprinkling chromite sand with a particle size of 16-30 mesh, and then placing the transition layer shell sprinkled with the chromite sand in a drying room for drying, solidifying to form a reinforcement layer, and obtaining a reinforcement layer mold shell; Step S70: weighing raw materials according to the formula of the sealing layer coating to prepare the sealing layer coating; Step S80: uniformly coating the reinforcement layer shell with a sealing layer coating, and then placing it in a drying room for drying and solidifying to form a sealing layer, thereby obtaining a sealing layer mold shell; Step S90: dewaxing and calcining the sealing layer mold shell to obtain an aluminum alloy investment casting mold shell.
2. The aluminum alloy investment casting shell according to claim 1, characterized in that: The surface coating formulation in step S10 includes the following components in parts by weight: 10 parts of silica sol, 11-18 parts of water, 54-67 parts of corundum powder, 4-6 parts of talc, 2-3 parts of coal powder, 0.02-0.03 parts of carboxymethyl cellulose, 0.03-0.04 parts of wetting agent, 0.04-0.05 parts of defoaming agent, and 0.05-0.07 parts of bactericide.
3. The aluminum alloy investment casting shell according to claim 2, characterized in that: The conductivity of the silica sol in the surface coating formula in step S10 is 3.0-5.6ms / cm; the wetting agent is one of wetting agent wet245, wetting agent wet270 and wetting agent wet510; the defoaming agent is one of defoaming agent BYK-024, defoaming agent BYK-028 and defoaming agent BYK-530; the bactericide is one of bactericide CL-39, bactericide CL-129 and bactericide MD-146.
4. The aluminum alloy investment casting shell according to claim 1, characterized in that: The transition layer coating formulation in step S30 includes the following components in parts by weight: 12 parts of silica sol, 13-22 parts of water, 50-61 parts of corundum powder, 5-6.5 parts of talc, 2.5-3.5 parts of coal powder, 0.02-0.03 parts of carboxymethyl cellulose, 0.02-0.03 parts of wetting agent, 0.03-0.04 parts of defoaming agent, and 0.05-0.07 parts of bactericide.
5. The aluminum alloy investment casting shell according to claim 4, characterized in that: The conductivity of the silica sol in the transition layer coating formula in step S30 is 3.0-5.6ms / cm; the wetting agent is one of wetting agent wet245, wetting agent wet270 and wetting agent wet510; the defoaming agent is one of defoaming agent BYK-024, defoaming agent BYK-028 and defoaming agent BYK-530; the bactericide is one of bactericide CL-39, bactericide CL-129 and bactericide MD-146.
6. The aluminum alloy investment casting shell according to claim 1, characterized in that: The reinforcement layer coating formula in step S50 includes the following components in parts by weight: 28 parts of silica sol, 62-68 parts of corundum powder, 5.2-6.0 parts of talc, 6.2-6.8 parts of coal powder, 0.02-0.03 parts of carboxymethyl cellulose, 0.02-0.03 parts of wetting agent, 0.03-0.04 parts of defoaming agent, and 0.04-0.06 parts of bactericide.
7. The aluminum alloy investment casting shell according to claim 6, characterized in that: The conductivity of the silica sol in the reinforcement layer coating formula in step S50 is 3.0-5.6ms / cm; the wetting agent is one of wetting agent wet245, wetting agent wet270 and wetting agent wet510; the defoaming agent is one of defoaming agent BYK-024, defoaming agent BYK-028 and defoaming agent BYK-530; the bactericide is one of bactericide CL-39, bactericide CL-129 and bactericide MD-146.
8. The aluminum alloy investment casting shell according to claim 1, characterized in that: The sealing layer coating formula in step S70 includes the following components in parts by weight: 28 parts of silica sol, 62-68 parts of corundum powder, 5.2-6.0 parts of talc, 6.2-6.8 parts of coal powder, 0.02-0.03 parts of carboxymethyl cellulose, 0.02-0.03 parts of wetting agent, 0.03-0.04 parts of defoaming agent, and 0.04-0.06 parts of bactericide.
9. The aluminum alloy investment casting shell according to claim 8, characterized in that: The conductivity of the silica sol in the sealing layer coating formula in step S70 is 3.0-5.6ms / cm; the wetting agent is one of wetting agent wet245, wetting agent wet270 and wetting agent wet510; the defoaming agent is one of defoaming agent BYK-024, defoaming agent BYK-028 and defoaming agent BYK-530; the bactericide is one of bactericide CL-39, bactericide CL-129 and bactericide MD-146.