Residue-free silver etching solution and preparation method, etching method and application thereof
By rationally preparing phosphoric acid, citric acid, nitric acid and nitrosylates in the etching solution, the problem of unstable performance of ITO-Ag-ITO etching solution is solved, and efficient and stable silver and ITO etching is achieved, avoiding silver residues and overetching improves etching efficiency and film flatness.
Patent Information
- Application Number
- CN202411164989.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
The existing ITO-Ag-ITO etching liquid has unstable performance during the etching process, resulting in incomplete etching, silver residue, overetching, uneven etching and unstable silver etching rate during service life.
A silver etching liquid without residue was used, containing 30.00 wt% to 40.00 wt% phosphoric acid, 10.00 wt% to 20.00 wt% citric acid, 5.00 wt% to 10.00 wt% nitric acid, 10.00 wt% to 20.00 wt% Sulfonic acid and 0.10% to 5.00% by weight of nitroso acid salts, through the combination of these components, provide an acidic environment and redox reactions, ensuring the etching efficiency and stability of silver and ITO.
The etching performance is improved, silver residue and overetching are avoided, etching efficiency and film flatness are improved, and the etching rate stability of silver and ITO is ensured, and it is suitable for single-layer and multi-layer etching.
Smart Images

Figure CN119040893A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of etching solutions, and in particular to a residue-free silver etching solution and a preparation method, an etching method and application thereof. Background Art
[0002] The ITO-Ag-ITO etching solution provided by the related technology (i.e., ITO-Ag-ITO etching solution for AMOLED) is mostly used to etch pixel electrodes during the manufacturing process of liquid crystal displays (TFT-LCD) and organic light-emitting diodes (OLED). The etching methods using ITO-Ag-ITO can be divided into one-step method, two-step method, and three-step method according to the process steps.
[0003] However, when etching using the ITO-Ag-ITO etching solution provided by the related art, whether a one-step method, a two-step method or a three-step method is adopted, there will be problems such as unstable etching performance leading to incomplete etching, silver residue, over-etching, uneven etching and unstable silver etching rate during the service life. Summary of the invention
[0004] The object of the present invention is to provide a residue-free silver etching solution and a preparation method, an etching method and application thereof. The residue-free silver etching solution can be used to etch a film structure composed of silver and an indium tin oxide film, and the residue-free silver etching solution can improve the problems of incomplete etching, silver residue, over-etching, uneven etching and unstable silver etching rate during the service life caused by unstable etching performance; the corresponding preparation method of the residue-free silver etching solution is simple and easy to operate. The etching method of the present invention is simple and easy to operate, and can improve etching efficiency and save etching solution. The application of the etching solution provided by the present invention can be used for etching a single layer or a multilayer, and has a wide range of applications and strong flexibility.
[0005] The present invention is achieved in that:
[0006] In a first aspect, the present invention provides a residue-free silver etching solution, which comprises, by mass percentage:
[0007] 30.00wt% to 40.00wt% of phosphoric acid;
[0008] 10.00wt% to 20.00wt% citric acid;
[0009] 5.00wt% to 10.00wt% nitric acid;
[0010] 10.00 wt% to 20.00 wt% of sulfonic acid;
[0011] 0.10wt% to 5.00wt% of a nitrosate;
[0012] The balance is water.
[0013] In an alternative embodiment, the nitrosyl acid salt includes at least one of potassium hexanitrosocobaltate, diaminetetranitrosocobaltate, and potassium tetranitrosoplatinate.
[0014] In an alternative embodiment, the nitrosyl acid salt is potassium tetranitrosoplatinate.
[0015] In an optional embodiment, the mass percentage of the nitrosoic acid salt is 0.20 wt% to 0.50 wt%.
[0016] In an alternative embodiment, the mass percentage of the nitrosoic acid salt is 0.30 wt %.
[0017] In an alternative embodiment, the sulfonic acid comprises at least one of methanesulfonic acid, 2-hydroxyethylsulfonic acid, and linear alkylbenzenesulfonic acid.
[0018] In an alternative embodiment, the sulfonic acid is methanesulfonic acid.
[0019] In an optional embodiment, the silver etching solution without residue comprises, by mass percentage:
[0020] 30.00wt%, 37.00wt% or 40.00wt% phosphoric acid;
[0021] 10.00wt%, 15.00wt% or 20.00wt% of citric acid;
[0022] 5.00wt%, 7.00wt% or 10.00wt% nitric acid;
[0023] 10.00 wt%, 15.00 wt% or 20.00 wt% of sulfonic acid;
[0024] 0.10wt%, 0.30wt% or 5.00wt% of nitrosate.
[0025] In an alternative embodiment, the sulfonic acid comprises methanesulfonic acid and the nitrosyl acid salt is potassium tetranitrosoplatinate.
[0026] In a second aspect, the present invention provides a method for preparing a residue-free silver etching solution, comprising: mixing nitric acid, citric acid and phosphoric acid to obtain a mixed acid; then dissolving a nitrosyl acid salt in water, adding sulfonic acid and the mixed acid, and stirring.
[0027] In a third aspect, the present invention provides an etching method, comprising: maintaining the residue-free silver etching solution of any of the above items at a preset temperature, and circulating and spraying the substrate to be etched.
[0028] In a fourth aspect, the present invention further provides an application of a residue-free silver etching solution, which is used to etch a single layer formed of silver or a silver alloy, or to simultaneously etch the above-mentioned single layer and an indium oxide layer that are stacked.
[0029] The present invention has the following beneficial effects:
[0030] The residue-free silver etching solution of the invention comprises, by mass percentage, 30.00wt%-40.00wt% of phosphoric acid, 10.00wt%-20.00wt% of citric acid, 5.00wt%-10.00wt% of nitric acid, 10.00wt%-20.00wt% of sulfonic acid, 0.10wt%-5.00wt% of nitrosyl acid salt, and the balance is water.Phosphoric acid, citric acid and nitric acid mainly provide an acidic environment for etching, so as to penetrate and acid-lyze Ag, and dissolve and diffuse the formed Ag ions in the etching solution; among them, nitric acid is a monobasic inorganic strong acid with strong oxidizing and corrosive properties, and is one of the six major inorganic strong acids. When the concentration of nitric acid is higher than 10.00wt%, its oxidizing property is too strong, and the stability of the silver etching rate becomes difficult to control. When the content of nitric acid is lower than 5.00wt%, the etching rate is significantly reduced, thereby prolonging the etching time and failing to meet the requirements of etching efficiency. Therefore, the content of nitric acid in the residual silver etching solution is 5.00wt% to 10.00wt%, which can ensure the controllability of silver etching and ensure high etching efficiency; phosphoric acid It can not only provide acidity and perform oxidation and reduction reactions with silver, but also the phosphate ions can combine with the oxidized silver ions to perform complex reactions to generate stable complexes, quickly migrate to the bulk solution, play the role of silver ion stabilizer, and etch the indium oxide layer at the same time, that is, the addition of phosphoric acid can ensure the etching efficiency of the indium oxide layer at the same time, and when the content of phosphoric acid is lower than 30.00wt%, the acidity of the etching solution is insufficient and the etching rate is slow, and when the content of phosphoric acid is higher than 40.00wt%, the viscosity of the etching solution increases and it is easy to over-etch, so the content of phosphoric acid in the residue-free silver etching solution is 30.00wt% to 40.00wt%, which can ensure a higher etching efficiency and improve the problem of over-etching; citric acid can As an auxiliary oxidant, indium tin oxide ITO (In2O3:SnO2=9:1, molar ratio) reacts under acidic conditions to generate indium ions and tin ions. As the etching reaction proceeds, the indium ions and tin ions in the etching solution increase, and the etching reaction rate of ITO decreases. The citrate ions in citric acid form a complex with the metal cations, that is, the citrate ions form a complex with the indium ions in the etching solution, so that the indium ions and tin ions in the etching solution are reduced, and the reaction is promoted to proceed in the forward direction, that is, the etching rate of ITO can be accelerated by citric acid; it should be noted that since the reaction rate of silver is faster, after the reaction rate of ITO is accelerated by the addition of citric acid, the etching rate difference between silver and ITO can be reduced accordingly, so that the top The risk of collapse of the top layer ITO will not occur due to slow etching, thereby improving the yield of the etched product; when the citric acid content is lower than 10.00wt%, the complexation effect of citric acid and indium ions is limited, and it is difficult to promote the forward reaction, that is, it cannot play a role in accelerating the ITO etching rate, and the top layer ITO still has the risk of collapse; when the citric acid content is higher than 20.00wt%, the ITO etching rate is too fast, which will cause the edge of the ITO / Ag / ITO film to be uneven. Therefore, the citric acid content is 10.00wt% to 20.00wt%, which can reduce the etching rate difference between silver and ITO, so that the risk of collapse of the top layer ITO will not occur due to slow etching, and the flatness of the edge of the film after etching can be improved.
[0031] Sulfonic acid can be used as a buffer, which contains one or more sulfate groups (-SO3H) and has a certain acidity, which can effectively buffer the speed of the oxidation reaction of silver, thereby playing a role in adjusting the silver etching rate in the etching solution in the form of a buffer; however, when the sulfonic acid content is lower than 10.00wt%, the acidity provided by it is limited and it is difficult to play an effective buffering role; when the sulfonic acid content is higher than 20.00wt%, the acidity provided by it is too high, which will cause the solution etching rate to be too slow; therefore, the sulfonic acid content is 10.00wt% to 20.00wt%, which can play a good etching buffering role and avoid excessive buffering, which will cause the etching rate to be too slow.
[0032] Nitroso acid salts have strong oxidizing properties. The addition of nitroso acid salts can further ensure that silver is oxidized into soluble silver ions and form a more stable complex between silver ions and nitroso acid salts. At the same time, the oxidizing effect of nitroso acid salts can also promote the dissolution of ITO, that is, indium ions and tin ions are produced through redox reactions and dissolved in the etching solution, thereby improving the problem of excessive difference in etching rates between silver and ITO, improving etching efficiency, ensuring the adequacy of etching, and effectively improving the problem of etching residues. When the content of nitroso acid salts is lower than 0.10wt%, the oxidizing property provided by nitroso acid salts in the etching solution is limited, which is easy to cause residues. When the content of nitroso acid salts is higher than 5.00wt%, the oxidizing property provided by nitroso acid salts in the etching solution is too strong, which is easy to cause over-etching.
[0033] Obviously, the residue-free silver etching solution of the present invention can be used to etch a film structure composed of silver and indium tin oxide film, and through the coordination between various raw materials and corresponding components, the problems of incomplete etching, silver residue, over-etching, uneven etching and unstable silver etching rate during the service life caused by unstable etching performance are improved.
[0034] The preparation method of the silver etching liquid without residue of the present invention comprises: mixing nitric acid, citric acid and phosphoric acid to obtain a mixed acid; then dissolving a nitrosyl acid salt in water, adding sulfonic acid and the mixed acid, and stirring. The method can prepare the silver etching liquid without residue by simply mixing the raw materials, is simple and easy to operate; and can improve the safety problem caused by directly adding nitric acid into water to generate heat.
[0035] The etching method of the present invention requires heating the aforementioned etching solution to a preset temperature, and circulating and spraying the substrate to be etched. The method is simple and easy to operate, and etching at a certain temperature can improve the etching efficiency. The recycling of the etching solution can also save the etching solution.
[0036] The etching solution provided by the present invention can be used for etching a single layer or a multilayer, and has a wide application range and strong flexibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0038] Figure 1 This is a CD bias diagram of a product after the etching solution of Example 1 of the present invention is used to etch the product;
[0039] Figure 2 This is a CD bias diagram of a product after the etching solution of Comparative Example 2 of the present invention is used to etch the product;
[0040] Figure 3 This is a SEM image of a product after the etching solution of Example 1 of the present invention is used to etch the product;
[0041] Figure 4 This is an OM image of a product after the etching solution of Example 1 of the present invention is used to etch the product;
[0042] Figure 5 This is an OM image of a product after the etching solution of Example 2 of the present invention is used to etch the product;
[0043] Figure 6 This is a SEM picture of the product after the etching solution of comparative example 10 of the present invention is used to etch the product. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0045] The etching methods using etching liquid provided in the related technology include a one-step method, a two-step method and a three-step method, wherein the one-step method is to use ITO-Ag-ITO etching liquid to achieve the etching of ITO and Ag stacks through one process step. The advantage is that the process is simple and the equipment requirements are low. The disadvantage is that the same etching liquid is used to etch two material stacks with huge differences in corrosion rates, which can easily lead to morphological defects. The difference between the two-step method and the one-step method is that the etching is divided into a two-step process, wherein the ITO-Ag etching liquid is used to complete the etching of top-ITO and Ag, and a special ITO etching liquid is used to complete the etching of bottom-ITO and the morphology modification of top-ITO. Similarly, the difference between the three-step method and the one-step method is that the etching is divided into a three-step process, wherein the upper and lower layers of ITO (i.e., top-ITO and bottom-ITO) are etched using ITO etching liquid, and the middle layer of Ag and the very small amount of remaining ITO are etched using Ag etching liquid.
[0046] The ITO-Ag-ITO etching solution provided by the related art is mostly a phosphoric acid-nitric acid-acetic acid system. Regardless of whether a one-step method, a two-step method or a three-step method is used, there will be problems such as unstable etching performance leading to incomplete etching, silver residue, over-etching, uneven etching and unstable silver etching rate during the service life. The inventors have found that in the etching solution containing nitric acid, phosphoric acid and polycarboxylic acid, replacing acetic acid with polycarboxylic acid can improve the problem of poor working environment caused by the strong smell of acetic acid, but it does not solve the problem of stable silver etching rate during use. At the same time, the poor solubility of organic polycarboxylic acid in the system also causes the instability of etching rate; and further studies have found that the etching solution containing nitric acid, propionic acid, phosphoric acid azole compounds can replace acetic acid with propionic acid to increase wettability and improve etching uniformity, but this etching solution introduces azole compounds. Due to the adsorption of azole compounds, the etching solution is easier to over-etch, resulting in the defect of small black spots in the subsequent process, and may also cause local areas to turn black, reducing the yield rate.
[0047] In order to improve the above problems, the inventors have studied and obtained a residue-free silver etching solution provided by an embodiment of the present invention. The residue-free silver etching solution comprises, by mass percentage, 30.00wt% to 40.00wt% of phosphoric acid, 10.00wt% to 20.00wt% of citric acid, 5.00wt% to 10.00wt% of nitric acid, 10.00wt% to 20.00wt% of sulfonic acid, 0.10wt% to 5.00wt% of nitrosyl acid salt, and the balance is water.
[0048] Phosphoric acid, citric acid and nitric acid mainly provide an acidic environment for etching to penetrate and acid-lyze Ag, and to dissolve and diffuse the formed Ag ions in the etching solution.
[0049] Among them, nitric acid is a monobasic inorganic strong acid with strong oxidizing and corrosive properties, and is one of the six major inorganic strong acids. When the concentration of nitric acid is higher than 10.00wt%, its oxidizing property is too strong and the stability of the silver etching rate becomes difficult to control. When the content of nitric acid is lower than 5.00wt%, the etching rate will be significantly reduced, thereby extending the etching time and failing to meet the requirements of etching efficiency. Therefore, the content of nitric acid in the residue-free silver etching solution is 5.00wt% to 10.00wt%, which can ensure controllability during silver etching and ensure high etching efficiency.
[0050] Phosphoric acid can not only provide acidity and perform oxidation and reduction reactions with silver, but also phosphate ions can combine with oxidized silver ions to perform complex reactions to generate stable complexes, quickly migrate to the bulk solution, play the role of silver ion stabilizer, and etch the indium oxide layer at the same time, that is, the addition of phosphoric acid can ensure the etching efficiency of the indium oxide layer at the same time, and when the content of phosphoric acid is lower than 30.00wt%, the acidity of the etching solution is insufficient and the etching rate is slow, and when the content of phosphoric acid is higher than 40.00wt%, the viscosity of the etching solution increases and it is easy to over-etch, so the content of phosphoric acid in the silver etching solution without residue is 30.00wt% to 40.00wt%, which can ensure higher etching efficiency and improve the problem of over-etching.
[0051] Citric acid can be used as an auxiliary oxidant. For example, indium tin oxide ITO (In2O3:SnO2=9:1, molar ratio) reacts under acidic conditions to generate indium ions and tin ions. As the etching reaction proceeds, the indium ions and tin ions in the etching solution increase, and the etching reaction rate of ITO decreases. The citrate ions in citric acid form a complex with the metal cations, that is, the citrate ions form a complex with the indium ions in the etching solution, so that the indium ions and tin ions in the etching solution are reduced, and the reaction is promoted to proceed in the forward direction, that is, the etching rate of ITO can be accelerated by citric acid. It should be noted that since the reaction rate of silver is faster, the addition of citric acid to accelerate the reaction rate of ITO can correspondingly reduce the etching rate difference between silver and ITO. , so that the top layer of ITO will not have the risk of collapse due to slow etching, thereby improving the yield of the etching product; when the citric acid content is lower than 10.00wt%, the complexing effect of citric acid and indium ions is limited, and it is difficult to promote the forward reaction, that is, it cannot play a role in accelerating the ITO etching rate, and the top layer of ITO still has the risk of collapse; when the citric acid content is higher than 20.00wt%, the ITO etching rate is too fast, which will cause the edge of the ITO / Ag / ITO film to be uneven. Therefore, the citric acid content is 10.00wt% to 20.00wt%, which can reduce the etching rate difference between silver and ITO, so that the top layer of ITO will not have the risk of collapse due to slow etching, and can improve the flatness of the edge of the film after etching.
[0052] It should be noted that indium oxide may also refer to indium zinc oxide, indium tin zinc oxide, indium gallium zinc oxide, and the like.
[0053] Sulfonic acid can be used as a buffer, which contains one or more sulfate groups (-SO3H) and has a certain acidity, which can effectively buffer the speed of the oxidation reaction of silver, thereby playing a role in adjusting the silver etching rate in the etching solution in the form of a buffer; however, when the sulfonic acid content is lower than 10.00wt%, the acidity provided by it is limited and it is difficult to play an effective buffering role; when the sulfonic acid content is higher than 20.00wt%, the acidity provided by it is too high, which will cause the solution etching rate to be too slow; therefore, the sulfonic acid content is 10.00wt% to 20.00wt%, which can play a good etching buffering role and avoid excessive buffering, which will cause the etching rate to be too slow.
[0054] Nitroso acid salts have strong oxidizing properties. The addition of nitroso acid salts can further ensure that silver is oxidized into soluble silver ions and form a more stable complex between silver ions and nitroso acid salts. At the same time, the oxidizing effect of nitroso acid salts can also promote the dissolution of ITO, that is, indium ions and tin ions are produced through redox reactions and dissolved in the etching solution, thereby improving the problem of excessive difference in etching rates between silver and ITO, improving etching efficiency, ensuring the adequacy of etching, and effectively improving the problem of etching residues. When the content of nitroso acid salts is lower than 0.10wt%, the oxidizing property provided by nitroso acid salts in the etching solution is limited, which is easy to cause residues. When the content of nitroso acid salts is higher than 5.00wt%, the oxidizing property provided by nitroso acid salts in the etching solution is too strong, which is easy to cause over-etching.
[0055] Obviously, the residue-free silver etching solution of the present invention can be used to etch a film structure composed of silver and indium tin oxide film, and through the coordination between various raw materials and corresponding components, the problems of incomplete etching, silver residue, over-etching, uneven etching and unstable silver etching rate during the service life caused by unstable etching performance are improved.
[0056] Optionally, the nitrosyl acid salt includes at least one of potassium hexanitrocobaltate, diamine tetranitrosyl cobaltate and potassium tetranitrosoplatinate. By using the nitrosyl acid salt with strong oxidizing property, ITO can be fully oxidized and reduced to generate indium particles and tin ions, which are dissolved in the etching solution, thereby reducing etching residues.
[0057] In some embodiments, the nitrosyl acid salt is potassium tetranitrosoplatinate, which has relatively stronger oxidizing properties and can more efficiently and reliably cause ITO to undergo a redox reaction to generate indium particles and tin ions, which are dissolved in the etching solution, thereby ensuring the cleanliness of the etching and reducing residues.
[0058] Optionally, the mass percentage of the nitrosyl acid salt is 0.20wt% to 0.50wt%. Under a better weight percentage, the strong oxidizing property of the nitrosyl acid salt can be used to improve the etching effect, reduce the residue, and reduce the probability of over-etching.
[0059] In some embodiments, the mass percentage of the nitrosoic acid salt is 0.30 wt %; at this mass percentage, the etching effect can be substantially improved, the residue can be reduced, and the over-etching problem can be substantially improved.
[0060] Optionally, the sulfonic acid includes at least one of methanesulfonic acid, 2-hydroxyethylsulfonic acid and linear alkylbenzenesulfonic acid. The organic acid properties of methanesulfonic acid, 2-hydroxyethylsulfonic acid and linear alkylbenzenesulfonic acid can accelerate the removal of silver ion compounds and improve the problem of re-adsorption of oxidized silver, that is, the organic acid can play a certain silver dissolution effect, thereby improving the etching efficiency, effectively improving the residual problem, and improving the problem of instability of silver etching rate during the service life.
[0061] In some embodiments, the sulfonic acid is selected from methanesulfonic acid to ensure a higher efficiency of removing the silver ion compound, more reliably avoid the re-adsorption of oxidized silver, and improve the dissolution-aiding effect.
[0062] The embodiment of the present invention also provides a method for preparing a residue-free silver etching solution, which includes: mixing nitric acid, citric acid and phosphoric acid to obtain a mixed acid; then dissolving a nitrosyl acid salt in water, and sequentially adding sulfonic acid and the mixed acid, and stirring. The method can prepare a residue-free silver etching solution by simply mixing the raw materials, which is simple and easy to operate; and can improve the safety problem caused by directly adding nitric acid to water to generate heat.
[0063] The embodiment of the present invention also provides an etching method, which requires heating the aforementioned etching solution to a preset temperature and circulating and spraying the substrate to be etched. The method is simple and easy to operate, and etching at a certain temperature can improve the etching efficiency. The recycling of the etching solution can also save the etching solution.
[0064] The above preset temperature is not specifically limited and can be 30-50, for example: 30, 32, 35, 37, 40, 43, 45, 48, 50, etc., and is not specifically limited here.
[0065] The residue-free silver etching solution of the embodiment of the present invention can be used to etch a single layer formed by silver or a silver alloy, or to simultaneously etch the above-mentioned single layer and an indium oxide layer that are stacked (i.e., etching of ITO and Ag stacks can be achieved through one process step), and has a wide range of applications and strong flexibility.
[0066] The above-mentioned silver alloy may refer to silver-copper alloy, tungsten-silver alloy, silver-tin alloy, etc., and is not specifically limited here.
[0067] The present invention will be further described in detail below in conjunction with embodiments.
[0068] Embodiment 1
[0069] Weigh deionized water, phosphoric acid, citric acid, nitric acid, sulfonic acid and nitrite respectively according to the raw material ratios recorded in Table 1.
[0070] 1) Add the weighed nitric acid, citric acid and phosphoric acid to a beaker and mix evenly to obtain a mixed acid; 2) Dissolve the weighed nitrite in the deionized water contained in the beaker and stir evenly; 3) Add the weighed sulfonic acid to the beaker in step 2), and then add the mixed acid, and stir for 60 minutes to obtain a silver etchant without residue.
[0071] The preparation methods of Embodiments 2 - 15 and Comparative Examples 1 - 13 are similar to that of Embodiment 1, and the differences are recorded in the component ratios in Table 1.
[0072] Table 1
[0073]
[0074]
[0075] Etching detection was carried out on each embodiment and comparative example; experimental conditions: Add 10 L of each etchant to be detected to the production line simulation cleaning equipment, keep the etchant at a constant temperature of 40 °C, turn on the spray, circulate the etchant, and after the etchant temperature is stably circulated at 40 °C, place a 10 cm × 10 cm ITO / Ag / ITO substrate on the spray table to start the test. After etching, transfer the substrate to the water spray table for cleaning. After cleaning, dry the sample with an air knife, and confirm the etching effect under OM and SEM, that is, observe the etching characteristics and residue situation; among them, the time when the etching of the TO / Ag / ITO film ends is EPD, and the total etching time is 1.5 times of the EPD of the TO / Ag / ITO film. After etching, rinse it with deionized water within 2 seconds and dry the moisture on the surface. After the end, observe with a scanning electron microscope and further evaluate the performance parameters after etching.
[0076] The performance parameter evaluation criteria are as follows:
[0077] 1. The CD bias evaluation criteria are as follows:
[0078] ○: Excellent [0.2 μm < CD bias < 0.3 μm];
[0079] △: Good [0.1 μm < CD bias < 0.2 μm or 0.3 μm < CD bias < 0.4 μm];
[0080] ×: Defect [CD bias < 0.1μm or CD bias > 0.4μm].
[0081] Among them, Figure 1 is the CD bias map of the product after etching the product with the etching solution of Comparative Example 1 of the present invention; Figure 2 is the CD bias map of the product after etching the product with the etching solution of Comparative Example 2 of the present invention.
[0082] 2. The ITO residue evaluation criteria are as follows:
[0083] ○: Excellent [ITO residue particles < 5];
[0084] △: Good [5 < ITO residue particles < 20];
[0085] ×: Defect [number of ITO residue particles > 20].
[0086] 3. The Ag residue evaluation criteria are as follows:
[0087] ○: Excellent [Ag residue particles < 5];
[0088] △: Good [5 < Ag residue particles < 20]; ×: Defect [number of Ag residue particles > 20].
[0089] The test results are shown in Table 2
[0090] Table 2
[0091]
[0092]
[0093] According to the comparison of Examples 1 and 2 with Comparative Examples 1 and 2 in Table 2, it can be seen that phosphoric acid has a very large impact on CD bias in the etching solution. Among them, Examples 1 and 2 are the upper and lower limits of the formula. When the phosphoric acid is at the best mass percentage of 30.00wt% - 40.00wt%, the etching rate is slow when the content of phosphoric acid is lower than 30.00wt%, and the viscosity of the etching solution increases and it is easy to over-etch when the content is higher than 40.00wt%.
[0094] According to the comparison of Examples 4 and 5 with Comparative Examples 3 and 4 in Table 2, it can be seen that citric acid has a relatively large impact on ITO residue in the etching solution; among them, citric acid is an auxiliary oxidant, which can significantly accelerate the etching rate of ITO and reduce the etching rate difference between silver and ITO. If the mass percentage of citric acid is less than 10.00wt%, ITO residue will occur.
[0095] According to Table 2, comparing Examples 6 and 7 with Comparative Examples 5 and 6, when the concentration of nitric acid is lower than 5.00 wt %, the etching rate is significantly reduced, resulting in incomplete etching residues and ITO residues.
[0096] According to Table 2, by comparing Examples 8-10 with Comparative Examples 7-10, it can be seen that methanesulfonic acid has a certain effect on CD bias in the etching solution, but when the methanesulfonic acid content is lower than 10.00wt%, it cannot play an effective buffering role. When the methanesulfonic acid content is higher than 20.00wt%, the solution etching rate will be very slow. Therefore, the mass percentage of sulfonic acid is less than 10.00wt% to 20.00wt% to ensure a good etching effect.
[0097] Moreover, by comparing Examples 8-10 and 15, it can be seen that methanesulfonic acid is more effective than other sulfonic acids, and other sulfonic acids will cause certain residues to occur.
[0098] According to Table 2, when the content of potassium tetranitrosoplatinate is between 0.10wt% and 5.00wt%, little residue occurs. When the content of potassium tetranitrosoplatinate is between 0.30wt%, even less residue occurs.
[0099] According to Table 2, comparing Example 3 with Examples 13 and 14, it can be seen that potassium tetranitrosoplatinate is better than other nitroso acid salts in removing residues. Other nitroso acid salts also have oxidizing properties and can remove residues, but the effects are slightly worse.
[0100] At the same time, by comparing Examples 13 and 14 with Comparative Examples 12 and 13, it can be further proved that when the weight portion of the nitrosyl acid salt is not greater than 5wt%, it has a better etching effect.
[0101] Figure 1 The CD bias shown is 0.21 μm. Figure 2 The CD bias shown is 0.37 μm. The comparison of the CD bias results between Example 1 and Comparative Example 2 shows that the etching solution of the present invention can remove and etch materials more accurately and has a better etching effect.
[0102] Figure 3 , Figure 4 and Figure 5 The etching of Example 1 and Example 2 shown does not leave any residue. Figure 6 The etching of Comparative Example 10 shown has a residue; therefore, according to Figure 3-6 It can be seen that the addition of nitrosyl salts can effectively improve the problem of etching residues.
[0103] In summary, the residue-free silver etching solution of the present invention can be used to etch a film structure composed of silver and an indium tin oxide film, and the residue-free silver etching solution can improve the problems of incomplete etching, silver residue, over-etching, uneven etching and unstable silver etching rate during the service life caused by unstable etching performance; the corresponding preparation method of the residue-free silver etching solution is simple and easy to operate.
[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A residue-free silver etching solution, characterized in that: The silver etching solution without residue comprises, by mass percentage: 30.00wt% to 40.00wt% of phosphoric acid; 10.00wt% to 20.00wt% citric acid; 5.00wt% to 10.00wt% nitric acid; 10.00 wt% to 20.00 wt% of sulfonic acid; 0.10wt% to 5.00wt% of a nitrosate; The balance is water.
2. The residue-free silver etching solution according to claim 1, characterized in that The nitrosyl acid salt comprises at least one of potassium hexanitrocobaltate, diaminetetranitrosocobaltate and potassium tetranitrosoplatinate; and / or, The sulfonic acid includes at least one of methanesulfonic acid, 2-hydroxyethylsulfonic acid and linear alkylbenzenesulfonic acid.
3. The residue-free silver etching solution according to claim 2, characterized in that: The nitrosyl acid salt is potassium tetranitrosoplatinate.
4. The residue-free silver etching solution according to claim 1, characterized in that The mass percentage of the nitrosyl acid salt is 0.20wt% to 0.50wt%.
5. The residue-free silver etching solution according to claim 4, characterized in that: The mass percentage of the nitrosyl acid salt is 0.30wt%.
6. The residue-free silver etching solution according to claim 2, characterized in that: The sulfonic acid is the methanesulfonic acid.
7. The residue-free silver etching solution according to claim 1, characterized in that: The silver etching solution without residue comprises, by mass percentage: 30.00wt%, 37.00wt% or 40.00wt% of said phosphoric acid; 10.00wt%, 15.00wt% or 20.00wt% of said citric acid; 5.00wt%, 7.00wt% or 10.00wt% of said nitric acid; 10.00wt%, 15.00wt% or 20.00wt% of the sulfonic acid; 0.10wt%, 0.30wt% or 5.00wt% of the nitrosate; and / or, The sulfonic acid includes methanesulfonic acid, and the nitrosate is potassium tetranitrosoplatinate.
8. The method for preparing a residue-free silver etching solution according to any one of claims 1 to 7, wherein: include: The nitric acid, the citric acid and the phosphoric acid are mixed to obtain a mixed acid; the nitrosyl salt is dissolved in water, and the sulfonic acid and the mixed acid are added and stirred.
9. An etching method, characterized in that: include: The residue-free silver etching solution according to any one of claims 1 to 7 is maintained at a preset temperature and circulated and sprayed on the substrate to be etched.
10. The use of the residue-free silver etching solution according to any one of claims 1 to 7, characterized in that: The silver etching solution without residue is used for etching a single layer formed of silver or a silver alloy, or for simultaneously etching the single layer and an indium oxide layer which are stacked.
Citation Information
Cited By
High-selectivity silver etching solution and preparation method and etching process thereof