Layered oxide positive electrode material of sodium-ion battery as well as preparation method and application of layered oxide positive electrode material
By introducing trivalent manganese and/or tetravalent manganese into the positive electrode material of sodium ion battery and using inert atmosphere high-temperature sintering technology, the problem of material structural instability is solved, and the circulation and electrochemical properties of sodium ion battery are improved.
Patent Information
- Application Number
- CN202411165815.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
The cyclic stability and rate performance of existing sodium ion battery layered oxide positive electrode materials are poor, mainly due to the instability of the body phase and surface interface structure, resulting in sodium ion transport obstacles and material fragmentation.
By introducing trivalent manganese and/or tetravalent manganese into the layered oxide positive electrode material of sodium ion battery, and using inert atmosphere high-temperature sintering technology, Mn3+ and Na+ are retained in the material body phase, and at the same time, low-valent elements are used to replace Mn4+. Improve the structural stability and electrochemical properties of sodium ion batteries.
The reversible specific capacity and cycling performance of the positive electrode material of sodium ion battery are significantly improved, the structural stability and electrochemical performance of the material are enhanced, and the sodium ion transport efficiency is improved.
Smart Images

Figure CN119050342A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion battery layered oxide positive electrode material, a preparation method and application thereof. Background Art
[0002] A complete sodium-ion battery is mainly composed of positive electrode materials, negative electrode materials, electrolytes, separators, current collectors, and passivation films formed on the surface of positive and negative electrode material particles during the battery cycle. The key characteristics of the battery, such as reversible specific capacity, cycle stability, air stability, and operating voltage, are mainly determined by the inherent electrochemical properties of the positive and negative electrode materials. Therefore, seeking suitable positive and negative electrode materials has become the key to the development of high-performance sodium-ion batteries, especially positive electrode materials, which largely determine the energy density and safety performance of the battery. At present, several different types of sodium-ion battery positive electrode materials have been discovered, including Prussian blue analogs, polyanion compounds, tunnel-type transition metal oxides, and layered transition metal oxide materials. Among them, layered transition metal oxide positive electrode materials have attracted widespread attention due to their many types, easy synthesis, low cost, and high reversible capacity.
[0003] According to the research of scholars, layered transition metal oxide materials can be divided into P2, O3, O3', P3, P3', O2, etc. Among them, P2 and O3 are two common types of layered oxides. Generally speaking, when the sodium content is 0.6-0.8, the material tends to form a P2 structure, and when the sodium content is 0.8-1.0, the material tends to form an O3 structure. The P-type structure has a larger interlayer spacing than the O-type material, so the P2-type material usually has a better rate performance. And because the initial sodium content of the O3-type material is higher than that of the P2-type material, more sodium can be inserted and removed during the charge and discharge process, and the energy density is large, so it has obvious advantages in the subsequent matching of the negative electrode material to assemble the sodium ion full battery. However, the poor kinetic ability of the O3-type material and the irreversible large volume phase change during the charge and discharge process lead to its poor rate performance and cycle performance; the P2-type structure has a larger interlayer spacing than the O3-type material, so the P2-type material usually has a better rate performance.
[0004] But in fact, both P2 and O3 layered oxide cathode materials still have the problems of poor cycle stability and poor rate performance. The reasons for the poor cycle stability of the materials can be summarized as follows: (1) Bulk phase structure stability: Layered cathode materials will undergo complex phase changes during the sodium ion extraction and insertion process. In particular, under high pressure, the layered structure will undergo interlayer slippage, causing irreversible structural changes that affect the transmission of sodium ions, increase polarization, and lead to rapid capacity decay; in addition, complex phase changes will cause changes in lattice constants, induce stress, and cause microcracks inside the material particles and material fragmentation, which will directly lead to poor cycle stability. (2) Surface interface structure stability: The material surface is prone to side reactions when in contact with the electrolyte, resulting in the dissolution of transition metals, the formation of an inert layer on the surface, which hinders the transmission of sodium ions and deteriorates the material performance. In addition, in P2 layered oxides, the sodium content is relatively low. Under the condition of deep sodium removal at high voltage, the crystal structure lacks sodium ion support, resulting in the destruction of the integrity of the crystal structure or even collapse.
[0005] Element doping has been proven to be an effective means to improve the structural stability and rate performance of materials. By introducing impurity elements into the transition metal layer or alkali metal layer, complex phase changes can be suppressed and structural stability can be improved. However, most element doping methods enrich the elements in the bulk phase or on the surface and distribute them unevenly. For example, elements with ionic radius close to the main element are easy to enter the bulk phase to replace the main element and suppress the irreversible phase change of the material; while elements with larger ionic radius are difficult to enter the bulk phase and are easy to enrich on the surface to form an inert layer or impurity phase. It is difficult to achieve the stability of the bulk phase and surface interface structure at the same time by conventional element doping methods. In addition, surface coating can effectively prevent the contact between the material surface and the electrolyte, but there is a lattice mismatch between the surface coating and the main material, and the coating is easy to peel off during the material cycle.
[0006] Therefore, there is an urgent need to provide sodium ion battery positive electrode materials that can significantly improve structural stability and good electrochemical performance.
[0007] In view of this, the present invention is proposed. Summary of the invention
[0008] The object of the present invention is to provide a sodium ion battery layered oxide positive electrode material, a preparation method and application thereof, aiming to improve the structural stability and electrochemical performance of the sodium ion battery positive electrode material.
[0009] The present invention is achieved in that:
[0010] In a first aspect, the present invention provides a sodium ion battery layered oxide positive electrode material, the chemical formula of which is Na X Ni A Mn 3+ B Mn 4+ C TMD O2;
[0011] Wherein 0.6≤X≤0.8, 0≤A≤0.5, 0≤B≤0.3, 0≤C≤0.7, 0≤D≤0.3, and A+B+C+D=1;
[0012] TM is selected from at least one of Li, K, Mg, Ca, Zn, Cu, Sr, Fe, Al, Co, Y, La and Bi.
[0013] Preferably, TM is selected from at least one of Li, K, Mg and Fe.
[0014] In a second aspect, the present invention provides a method for preparing the layered oxide positive electrode material of a sodium ion battery according to the aforementioned embodiment, comprising: mixing a sodium source, a nickel source, a trivalent manganese source, a tetravalent manganese source and a TM source according to a stoichiometric ratio, and then sintering at a high temperature.
[0015] In an optional embodiment, the raw materials are first mixed uniformly and then pressed into tablets, and then sintered at high temperature;
[0016] The high temperature sintering process includes: first sintering at 300℃-700℃, controlling the holding time to be 2h-16h, and then performing secondary sintering at 700℃-1150℃, controlling the holding time to be 8h-24h;
[0017] Preferably, the atmosphere during the high temperature sintering process is selected from at least one of an air atmosphere, an oxygen atmosphere, an argon atmosphere and a nitrogen atmosphere;
[0018] Preferably, during the high temperature sintering process, the heating rate is controlled to be 1° C. / min-10° C. / min.
[0019] In an optional embodiment, after high temperature sintering, the material is ground into a powder;
[0020] Preferably, after high-temperature sintering, the temperature is lowered to 120° C.-280° C., and then ground into powder in an environment with a relative humidity of less than 1%, and the grinding time is controlled to be 15 min-30 min.
[0021] In an optional embodiment, the raw materials are mixed uniformly by grinding, and then tabletted under a pressure of 40 MPa-120 MPa for 15 min-35 min;
[0022] Preferably, during the grinding of the raw material, an organic solvent is added to wet the powder in the mortar, and the grinding time is controlled to be 0.5h-2.0h;
[0023] More preferably, the organic solvent is selected from at least one of anhydrous ethanol and acetone.
[0024] In an optional embodiment, the nickel and manganese elements are added according to the theoretical amounts by adjusting the amounts of the nickel source, the trivalent manganese source and the tetravalent manganese source, and the sodium element is added in an excess of 1%-15% compared to the theoretical amount by adjusting the amount of the sodium source;
[0025] Preferably, the sodium source is selected from at least one of Na2CO3, Na2CO3·H2O, NaHCO3, NaOH, CH3COONa, NaNO3, Na2O2, NaO2 and Na2C2O4;
[0026] Preferably, the nickel source is selected from at least one of NiO and Ni(OH)2;
[0027] Preferably, the manganese source is selected from at least one of MnO, Mn2O3, MnO2, MnCO3 and Mn3O4;
[0028] Preferably, the TM source is selected from at least one of oxides, hydroxides and carbonates containing TM elements.
[0029] In a third aspect, the present invention provides a positive electrode sheet, comprising any one of the sodium ion battery layered oxide positive electrode materials in the aforementioned embodiments or a sodium ion battery layered oxide positive electrode material prepared by any one of the preparation methods in the aforementioned embodiments.
[0030] In a fourth aspect, the present invention provides a sodium ion battery comprising the positive electrode sheet of the aforementioned embodiment.
[0031] In a fifth aspect, the present invention provides an electrical device comprising the sodium ion battery of the aforementioned embodiment.
[0032] The present invention has the following beneficial effects:
[0033] The present invention optimizes the components of the layered oxide positive electrode material for sodium ion batteries, contains trivalent manganese and / or tetravalent manganese in the P2 type material, and can convert Mn into 3+ and Na + At the same time, it remains in the bulk of the material and utilizes the Mn charged in the first cycle. 3+ / Mn 4+ The redox pairs provide more sodium ions to the negative electrode, thereby compensating for the sodium ions lost by the negative electrode due to the formation of SEI film, thereby improving the reversible specific capacity of the material;
[0034] Substituting Mn by low-valent elements 4+ , thereby increasing the sodium content of the material and allowing more sodium to remain in the bulk phase of the material, thereby improving the structural stability of the layered oxide positive electrode material for sodium ion batteries and improving the cycle performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0036] Figure 1 This is a scanning electron microscope image of the positive electrode material prepared in Example 1 of the present invention;
[0037] Figure 2 This is a scanning electron microscope image of the positive electrode material prepared in Comparative Example 1 of the present invention;
[0038] Figure 3 This is a scanning electron microscope image of the positive electrode material prepared in Example 9 of the present invention;
[0039] Figure 4 This is a scanning electron microscope image of the positive electrode material prepared in Example 10 of the present invention;
[0040] Figure 5 The charge-discharge curves of the button cell of the self-sodium-supplementing P2-type layered oxide positive electrode material prepared in Example 1 of the present invention in the first two cycles of the test;
[0041] Figure 6 The charge-discharge curves of the button cell of the self-supplementing sodium P2-type layered oxide positive electrode material prepared in Example 6 of the present invention in the first two cycles of the test;
[0042] Figure 7 The charge-discharge curves of the button cell of the self-sodium-complementary P2-type layered oxide positive electrode material prepared in Example 11 of the present invention in the first two cycles of the test;
[0043] Figure 8 A comparison chart of the first cycle charge and discharge curves of button cell tests of the self-sodium-complementary P2-type layered oxide positive electrode materials prepared in Examples 1, 9 and 10 of the present invention;
[0044] Fig. 9 A comparison chart of the first cycle charge and discharge curves of button cell tests of the self-sodium-complementary P2-type layered oxide positive electrode materials prepared in Examples 1, 14 and 15 of the present invention;
[0045] Fig.10 The charge-discharge curves of the button cell test of the mainstream P2-type layered oxide positive electrode material prepared in Comparative Example 1 of the present invention in the first two cycles;
[0046] Fig.11 Cycling performance curves of button cells made of self-supplemented sodium P2-type layered oxide positive electrode materials prepared in Example 1 of the present invention and button cells made of mainstream P2-type layered oxide positive electrode materials prepared in Comparative Example 2;
[0047] Fig.12 The graphs are the cycle performance curves of full batteries prepared by matching the mainstream P2-type layered oxide positive electrode material prepared in Comparative Example 1 of the present invention and the self-sodium-complementary P2-type layered oxide positive electrode material prepared in Example 6 with a hard carbon negative electrode, respectively. DETAILED DESCRIPTION
[0048] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0049] The present invention provides a sodium ion battery layered oxide positive electrode material, the chemical formula of which is Na X Ni A Mn 3+ B Mn 4+ C TM D O2; where 0.6≤X≤0.8, 0≤A≤0.5, 0≤B≤0.3, 0≤C≤0.7, 0≤D≤0.3, and A+B+C+D=1;
[0050] The sodium ion battery layered oxide positive electrode material provided in the embodiment of the present invention is a self-supplementing sodium P2 type positive electrode material, which is prepared by simultaneously introducing trivalent manganese and / or tetravalent manganese, and sintering Mn at high temperature in an inert atmosphere. 3+ and Na + At the same time, it is retained in the bulk phase of the material, and low-valent elements are used to replace tetravalent manganese to increase the sodium content of the layered oxide material for sodium ion batteries, which is beneficial to improving the structural stability of the layered oxide positive electrode material for sodium ion batteries and the electrochemical performance of sodium ion batteries.
[0051] Specifically, the value of X can be 0.60, 0.65, 0.70, 0.75, 0.80, etc., the value of A can be 0.0, 0.1, 0.2, 0.3, 0.4, 0.5, etc., the value of B can be 0.0, 0.1, 0.2, 0.3, etc., the value of C can be 0.0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, etc., and the value of D can be 0.0, 0.1, 0.2, 0.3, etc. (A+B+C+D)=1, and A, B, C, and D cannot be 0 at the same time. The valence state of Mn ion is positive trivalent, positive tetravalent, or a mixed valence state of positive trivalent and positive tetravalent.
[0052] Furthermore, TM is selected from at least one of Li, K, Mg, Ca, Zn, Cu, Fe, Al, Co, Y, La, Ti, Sn, W, Ta and Nb, and TM can be any one or more of the above.
[0053] In a preferred embodiment, TM is selected from at least one of Li, K, Mg and Fe; the electrochemical performance of the positive electrode material is further improved by optimizing the type of TM elements and the proportion of each element.
[0054] The present invention provides a method for preparing a sodium ion battery layered oxide positive electrode material, comprising the following steps:
[0055] S1. Mixing
[0056] The sodium source, nickel source, trivalent manganese source, tetravalent manganese source and TM source are mixed according to the stoichiometric ratio of the positive electrode material so that the molar ratio of sodium, nickel, manganese and TM elements meets the requirements of the chemical formula.
[0057] In some embodiments, the amount of nickel source, trivalent manganese source and tetravalent manganese source is adjusted so that nickel, iron and manganese elements are added according to the theoretical amount, and the amount of sodium source is adjusted so that the sodium element is 1%-15% excessive compared to the theoretical amount, such as 1%, 3%, 5%, 8%, 10%, 13%, 15%, etc. By adjusting the amount of raw materials, an appropriate sodium source (such as sodium carbonate) is excessive to make up for the loss of sodium carbonate under high temperature sintering, but too much excess will cause sodium carbonate residue on the surface of the material, thereby affecting the material properties.
[0058] Specifically, the theoretical amount of each element refers to the molar amount of the element, and the excess of 1%-15% refers to the ratio of the excess molar amount to the theoretical molar amount.
[0059] In some embodiments, the sodium source is selected from at least one of Na2CO3, Na2CO3·H2O, NaHCO3, NaOH, CH3COONa, NaNO3, Na2O2, NaO2 and Na2C2O4, and the sodium source can be any one or more of the above, and the molar amount of the sodium element can be controlled to meet the chemical formula and excess requirements. The nickel source is selected from at least one of NiO and Ni(OH)2, and the nickel source can be any one or two of the above. The manganese source is selected from at least one of MnO, Mn2O3, MnO2, MnCO3 and Mn3O4, and the manganese source can be any one or more of the above.
[0060] In some embodiments, the TM source is selected from at least one of oxides, hydroxides and carbonates containing TM elements. The TM source can be any one or more of the above raw materials containing TM elements, so that the molar amount of the TM element meets the requirements of the chemical formula.
[0061] S2, grinding and tableting
[0062] Mix the raw materials evenly before pressing them into tablets. Pressing them into tablets before high-temperature sintering can promote high-temperature sintering, make the materials sintered more fully, and make the distribution of material elements more uniform.
[0063] In some embodiments, the raw materials are mixed evenly by grinding, and then tabletted for 15min-35min under a pressure of 40MPa-120MPa. The uniformity of the raw material mixing can be improved by grinding, and tabletting under the above pressure and time can make the density meet the requirements. Specifically, the pressure of tabletting can be 40MPa, 50MPa, 60MPa, 70MPa, 80MPa, 90MPa, 100MPa, 110MPa, 120MPa, etc.; if the pressure of tabletting is too small, the pressed tablets will not be compact enough; if the pressure is too large, the material will be too hard after sintering, and it will not be easy to grind into fine powder, thereby affecting the material properties. The tabletting time can be 15min, 20min, 25min, 30min, 35min, etc. If the tabletting time is too short, the corners of the pressed tablets will be broken, and if the tabletting time is too long, the material particles will be broken, thereby affecting the material properties.
[0064] Furthermore, during the grinding of the raw materials, an organic solvent is added to wet the powder in the mortar, and the organic solvent is used as a dispersant to make the grinding more uniform and improve the uniformity of the raw material mixing. The grinding time is controlled to be 0.5h-2.0h, such as 0.5h, 1.0h, 1.5h, 2.0h, etc. If the grinding time is too short, the mixing will be uneven; if the grinding time is too long, the small particles and fine particles of the sintered material will increase, affecting the material properties.
[0065] In some embodiments, the organic solvent is selected from at least one of anhydrous ethanol and acetone, and the organic solvent used in the grinding process can be any one or more of the above.
[0066] S3. High temperature sintering.
[0067] By high temperature sintering, Mn 3+ and Na + At the same time, it is retained in the bulk phase of the material, which is beneficial to improving the structural stability and electrochemical performance of layered oxide positive electrode materials for sodium ion batteries.
[0068] In some embodiments, the temperature can be gradually increased through a two-stage sintering process to prevent the high temperature from rising too fast and affecting the structure and performance of the material. The first sintering can be performed at 300℃-700℃, and the holding time can be controlled to be 2h-16h, and then the second sintering can be performed at 700℃-1150℃, and the holding time can be controlled to be 8h-24h. By adjusting the temperature and time of the two-stage sintering, the electrochemical performance of the positive electrode material can be further improved.
[0069] Specifically, the temperature of the primary sintering can be 300°C, 400°C, 500°C, 600°C, 700°C, etc., and the holding time of the primary sintering can be 2h, 5h, 8h, 10h, 12h, 14h, 16h, etc. The temperature of the secondary sintering can be 700°C, 800°C, 900°C, 1000°C, 1100°C, 1150°C, etc., and the holding time of the secondary sintering can be 8h, 10h, 13h, 15h, 18h, 20h, 24h, etc.
[0070] In some embodiments, during the high temperature sintering process, the heating rate is controlled to be 1°C / min-10°C / min, such as 1°C / min, 3°C / min, 5°C / min, 8°C / min, 10°C / min, etc. The heating rates in the primary sintering stage and the secondary sintering stage can be controlled to be 1°C / min-10°C / min, and the heating rates in the two stages can be the same or different.
[0071] In some embodiments, the atmosphere during the high temperature sintering process is selected from at least one of an air atmosphere, an oxygen atmosphere, an argon atmosphere, and a nitrogen atmosphere. The atmosphere of the high temperature sintering can be any one or more of the above.
[0072] In some embodiments, there may be agglomeration after high-temperature sintering, and the material can be ground into powder after high-temperature sintering. In actual operation, the temperature is lowered to 120°C-280°C after high-temperature sintering, and then ground into powder in an environment with a relative humidity of less than 1%, and the grinding time is controlled to be 15min-30min. After the cooling is completed, it can be immediately transferred to a low-humidity drying room and ground into powder using a mortar to prevent moisture interference during the grinding process.
[0073] Specifically, the temperature after cooling can be 120°C, 150°C, 180°C, 200°C, 230°C, 250°C, 280°C, etc., and the cooling rate is not limited, such as 1°C / min-10°C / min; the grinding time can be 15min, 20min, 25min, 30min, etc. Too short a grinding time will cause the material particles to agglomerate and affect the material properties, while too long a grinding time will cause the material particles to break, which will also affect the material properties.
[0074] The present invention provides a positive electrode plate, comprising the sodium ion battery layered oxide positive electrode material provided by an embodiment of the present invention, and the electrochemical performance of the positive electrode plate is further improved by improving the positive electrode material.
[0075] Specifically, the positive electrode plate may further include a positive electrode current collector, etc., and a positive electrode active coating is formed on the positive electrode current collector. The sodium ion battery layered oxide positive electrode material provided by the embodiment of the present invention is located in the positive electrode active coating.
[0076] An embodiment of the present invention further provides a sodium ion battery, comprising the above-mentioned positive electrode plate, and may further comprise a negative electrode plate, an electrolyte, a separator, etc. Due to the improvement of the electrochemical performance of the positive electrode plate, the sodium ion battery has more excellent electrochemical performance.
[0077] An embodiment of the present invention further provides an electrical device, comprising the above-mentioned sodium ion battery, and using the sodium ion battery for power supply.
[0078] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0079] Example 1
[0080] This embodiment provides a method for preparing a sodium ion battery layered oxide positive electrode material. The chemical formula of the sodium ion battery layered oxide positive electrode material is Na 0.7 Ni 0.33 Mn 3+ 0.03 Mn 4+ 0.64 O2, the steps are as follows:
[0081] Weigh 0.7471g Na2CO3 (sodium ratio is 1:1.05), 0.473g NiO, 1.067g MnO2 and 0.045g Mn2O3 and grind and mix them for 0.5h; pour the evenly ground raw materials into the mold of the tablet press, and then place the mold in the tablet press, select a pressure of 80MPa, and continue for 20min; put the pressed raw material disc into a crucible, place it in a tubular furnace, and in a nitrogen atmosphere, heat up to 550℃ at a rate of 2℃ / min in the first sintering stage, keep warm for 6h, and heat up to 950℃ at a rate of 2℃ / min in the second sintering stage, keep warm for 16h, and then cool down to 200℃ at a rate of 2℃ / min, then immediately transfer the material to a low humidity drying room (relative humidity less than 1%, the same below), and then use a mortar to grind the material for 15min to grind the material into powder, thereby obtaining Na 0.7 Ni 0.33 Mn 3+ 0.03 Mn 4+ 0.64 O2 positive electrode material.
[0082] Example 2
[0083] This embodiment provides a method for preparing a sodium ion battery layered oxide positive electrode material. The chemical formula of the sodium ion battery layered oxide positive electrode material is Na 0.72 Ni 0.33 Mn 3+ 0.05 Mn 4+ 0.62 O2, the steps are as follows:
[0084] Weigh 0.765g Na2CO3 (sodium ratio is 1:1.05), 0.471g NiO, 1.029g MnO2 and 0.075g Mn2O3 for grinding and mixing, the grinding time is 0.5h, the grinding time is 0.5h; the raw material after grinding evenly is poured into the mold of the tablet press, and then the mold is placed in the tablet press, and the pressure of 80MPa is selected for 20min; the pressed raw material disc is placed in a crucible and placed in a tubular furnace. Under a nitrogen atmosphere, the first sintering stage is heated to 550℃ at a rate of 2℃ / min and kept warm for 6h. In the second sintering stage, the temperature is also raised to 950℃ at a rate of 2℃ / min, kept warm for 16h, and then cooled to 200℃ at a rate of 2℃ / min. Then the material is immediately transferred to a low-humidity drying room, and the material is ground in a mortar for 15min to grind the material into powder, thereby obtaining Na 0.72 Ni 0.33 Mn 3+ 0.05 Mn 4+ 0.62 O2 positive electrode material.
[0085] Example 3
[0086] This embodiment provides a method for preparing a sodium ion battery layered oxide positive electrode material. The chemical formula of the sodium ion battery layered oxide positive electrode material is Na 0.73 Ni 0.33 Mn 3+ 0.06 Mn 4+ 0.61 The preparation method of O2, the steps are as follows:
[0087] Weigh 0.774g Na2CO3 (sodium ratio is 1:1.05), 0.470g NiO, 1.011g MnO2 and 0.09g Mn2O3, grind and mix them, and the grinding time is 0.5h; pour the evenly ground raw materials into the mold of the tablet press, and then place the mold in the tablet press, select a pressure of 80MPa, and continue for 20min; put the pressed raw material disc into a crucible, place it in a tubular furnace, and in a nitrogen atmosphere, heat up to 550℃ at a rate of 2℃ / min in the first sintering stage, keep warm for 6h, and heat up to 950℃ at a rate of 2℃ / min in the second sintering stage, keep warm for 16h, and then cool down to 200℃ at a rate of 2℃ / min, then immediately transfer the material to a low humidity drying room, and then use a mortar to grind the material for 15min to grind the material into powder, thereby obtaining Na 0.73 Ni 0.33 Mn 3+ 0.06 Mn 4+ 0.61 O2 positive electrode material.
[0088] Example 4
[0089] This embodiment provides a method for preparing a sodium ion battery layered oxide positive electrode material. The chemical formula of the sodium ion battery layered oxide positive electrode material is Na 0.72 Ni 0.33 Mn 3+ 0.03 Mn 4+ 0.63 Mg 0.01 O2, the steps are as follows:
[0090] Weigh 0.767g Na2CO3 (sodium ratio is 1:1.05), 0.472g NiO, 0.008g MgO, 1.049g MnO2 and 0.045g Mn2O3 and grind and mix them for 0.5h; pour the evenly ground raw materials into the mold of the tablet press, and then place the mold in the tablet press, select a pressure of 80MPa, and continue for 20min; put the pressed raw material disc into a crucible and place it in a tubular furnace. Under a nitrogen atmosphere, the first sintering stage is heated to 550℃ at a rate of 2℃ / min and kept warm for 6h. In the second sintering stage, the temperature is also raised to 950℃ at a rate of 2℃ / min, kept warm for 16h, and then cooled to 200℃ at a rate of 2℃ / min. Then, the material is immediately transferred to a low-humidity drying room, and the material is ground in a mortar for 15min to grind the material into powder, thereby obtaining Na 0.72 Ni 0.33 Mn 3+ 0.03 Mn 4+ 0.63 Mg0.01 O2 positive electrode material.
[0091] Example 5
[0092] This embodiment provides a method for preparing a sodium ion battery layered oxide positive electrode material. The chemical formula of the sodium ion battery layered oxide positive electrode material is Na 0.72 Ni 0.33 Mn 3+ 0.03 Mn 4+ 0.63 Fe 0.01 O2, the steps are as follows:
[0093] Weigh 0.765 Na2CO3 (sodium ratio is 1:1.05), 0.471 NiO, 0.015 g Fe2O3, 1.046 g MnO2 and 0.045 g Mn2O3 and grind and mix them for 0.5 h; pour the evenly ground raw materials into the mold of the tablet press, and then place the mold in the tablet press, select a pressure of 80 MPa, and continue for 20 min; put the pressed raw material disc into a crucible and place it in a tubular furnace. Under a nitrogen atmosphere, the first sintering stage is heated to 550°C at a rate of 2°C / min and kept warm for 6 h. In the second sintering stage, the temperature is also raised to 950°C at a rate of 2°C / min, kept warm for 16 h, and then cooled to 200°C at a rate of 2°C / min. Then, the material is immediately transferred to a low-humidity drying room, and the material is ground in a mortar for 15 min to grind the material into powder, thereby obtaining Na 0.72 Ni 0.33 Mn 3+ 0.03 Mn 4+ 0.63 Fe 0.01 O2 positive electrode material.
[0094] Example 6
[0095] This embodiment provides a method for preparing a sodium ion battery layered oxide positive electrode material. The chemical formula of the sodium ion battery layered oxide positive electrode material is Na 0.73 Ni 0.33 Mn 3+ 0.03 Mn 4+ 0.63 Li 0.01 O2, the steps are as follows:
[0096] Weigh 0.778g Na2CO3 (sodium ratio is 1:1.05), 0.472g NiO, 0.007g Li2CO3, 1.048g MnO2 and 0.045g Mn2O3 and grind and mix them for 0.5h; pour the evenly ground raw materials into the mold of the tablet press, and then place the mold in the tablet press, select a pressure of 80MPa, and continue for 20min; put the pressed raw material disc into a crucible and place it in a tubular furnace. Under a nitrogen atmosphere, the first sintering stage is heated to 550℃ at a rate of 2℃ / min and kept warm for 6h. In the second sintering stage, the temperature is also raised to 950℃ at a rate of 2℃ / min, kept warm for 16h, and then cooled to 200℃ at a rate of 2℃ / min. Then, the material is immediately transferred to a low-humidity drying room, and the material is ground in a mortar for 15min to grind the material into powder, thereby obtaining Na 0.73 Ni 0.33 Mn 3+ 0.03 Mn 4+ 0.63 Li 0.01 O2 positive electrode material.
[0097] Example 7
[0098] This embodiment provides a method for preparing a sodium ion battery layered oxide positive electrode material. The chemical formula of the sodium ion battery layered oxide positive electrode material is Na 0.73 Ni 0.33 Mn 3+ 0.03 Mn 4+ 0.63 K 0.01 The preparation method of O2, the steps are as follows:
[0099] Weigh 0.775 Na2CO3 (sodium ratio is 1:1.05), 0.470 g NiO, 0.013 g K2O3, 1.045 g MnO2 and 0.045 g Mn2O3 and grind and mix them for 0.5 h; pour the evenly ground raw materials into the mold of the tablet press, and then place the mold in the tablet press, select a pressure of 80 MPa, and continue for 20 min; put the pressed raw material discs into a crucible and place it in a tubular furnace. Under a nitrogen atmosphere, the first sintering stage is heated to 550°C at a rate of 2°C / min and kept warm for 6 h. In the second sintering stage, the temperature is also raised to 950°C at a rate of 2°C / min, kept warm for 16 h, and then cooled to 200°C at a rate of 2°C / min. Then, the material is immediately transferred to a low-humidity drying room, and the material is ground in a mortar for 15 min to grind the material into powder, thereby obtaining Na 0.73 Ni 0.33 Mn 3+ 0.03Mn 4+ 0.63 K 0.01 O2 positive electrode material.
[0100] Example 8
[0101] This embodiment provides a method for preparing a sodium ion battery layered oxide positive electrode material. The chemical formula of the sodium ion battery layered oxide positive electrode material is Na 0.74 Ni 0.33 Mn 3+ 0.05 Mn 4+ 0.61 Mg 0.01 The preparation method of O2, the steps are as follows:
[0102] Weigh 0.785 Na2CO3 (sodium ratio is 1:1.05), 0.470 g NiO, 0.008 g MgO, 1.011 g MnO2 and 0.075 g Mn2O3 and grind and mix them for 0.5 h; pour the evenly ground raw materials into the mold of the tablet press, and then place the mold in the tablet press, select a pressure of 80 MPa, and continue for 20 min; put the pressed raw material disc into a crucible and place it in a tubular furnace. Under a nitrogen atmosphere, the first sintering stage is heated to 550 ° C at a rate of 2 ° C / min and kept warm for 6 h. In the second sintering stage, the temperature is also raised to 950 ° C at a rate of 2 ° C / min, kept warm for 16 h, and then cooled to 200 ° C at a rate of 2 ° C / min. Then, the material is immediately transferred to a low-humidity drying room, and the material is ground in a mortar for 15 min to grind the material into powder, thereby obtaining Na 0.74 Ni 0.33 Mn 3+ 0.05 Mn 4+ 0.61 Mg 0.01 O2 positive electrode material.
[0103] Example 9
[0104] The only difference between this embodiment and embodiment 1 is that the sintering temperature in the second sintering stage is 1150°C.
[0105] Example 10
[0106] The only difference between this embodiment and embodiment 1 is that the sintering temperature in the second sintering stage is 700°C.
[0107] Embodiment 11
[0108] The only difference between this embodiment and embodiment 1 is that a muffle furnace is used for sintering the materials and air is used as the sintering atmosphere.
[0109] Example 12
[0110] The only difference between this embodiment and embodiment 1 is that the heating rate used in the two-stage sintering process is 10° C. / min.
[0111] Embodiment 13
[0112] The only difference between this embodiment and embodiment 1 is that the heating rate used in the two-stage sintering process is 1° C. / min.
[0113] Embodiment 14
[0114] The only difference between this embodiment and embodiment 1 is that the holding time of the second sintering stage is 8 hours.
[0115] Embodiment 15
[0116] The only difference between this embodiment and embodiment 1 is that the holding time of the second sintering stage is 24 hours.
[0117] Comparative Example 1
[0118] This comparative example is Na 0.7 Ni 0.33 Mn 0.67 The preparation method of O2, the steps are as follows:
[0119] Weigh 0.747g Na2CO3 (sodium ratio is 1:1.05), 0.473g NiO, 1.117g MnO2, grind and mix, the grinding time is 0.5h; pour the evenly ground raw materials into the mold of the tablet press, and then place the mold in the tablet press, select a pressure of 80MPa, and continue for 15min; put the pressed raw material disc into a crucible, place it in a muffle furnace, and heat it to 550℃ at a rate of 2℃ / min in an air atmosphere, keep it warm for 6h, then heat it to 950℃ at the same rate of 2℃ / min, keep it warm for 16h, and then cool it to 200℃ at a rate of 2℃ / min, then immediately transfer the material to a low-humidity drying room, and then use a mortar to grind the material for 10min to grind the material into powder, thereby obtaining Na 0.7 Ni 0.33 Mn 0.67 O2 positive electrode material.
[0120] Comparative Example 2
[0121] This comparative example is Na 0.7 Ni 0.33 Mn 0.67 The preparation method of O2, in the preparation process, the manganese source only uses Mn2O3. The steps are as follows:
[0122] Weigh 0.747 g Na2CO3 (sodium ratio is 1:1.05), 0.473 g NiO, and 1.014 g Mn2O3, grind and mix, the grinding time is 0.5 h. The remaining steps refer to Example 1.
[0123] Test Example 1
[0124] Test method: The prepared positive electrode material powder is fully mixed with polyvinylidene fluoride and conductive carbon black in a mass ratio of 8:1:1, stirred into a slurry with uniform composition, coated on aluminum foil at a certain thickness of 200μm, dried in a vacuum drying oven at 120℃, rolled and cut into circular positive electrode sheets with a diameter of 12mm. The mass of the active material in the sheet is calculated and transferred to the glove box for use. The cut circular positive electrode sheet, the metal sodium sheet (as the negative electrode), the Whatman Grade GF / D type glass fiber membrane as the diaphragm, the 2025 positive and negative battery shells, the springs, the gaskets and the sodium hexafluorophosphate electrolyte were assembled into a 2025 button half-cell in a glove box filled with an argon atmosphere, and then placed in a battery test cabinet at a constant temperature of 25°C for charge and discharge tests; the positive electrode material sheet prepared in each embodiment and comparative example and the hard carbon negative electrode were matched and assembled into a full battery, wherein the hard carbon first efficiency was 90% and the reversible specific capacity was 300 mAh / g; the scanning electron microscope image of Example 1 is as shown in Figure 1 As shown, the scanning electron microscope image of Comparative Example 1 is as shown Figure 2 As shown, the charge and discharge curves of the button cell assembled in Example 1 in the first two cycles are as follows: Figure 3 As shown, the charge and discharge curves of the button cell assembled in Example 6 in the first two cycles are as follows: Figure 4 As shown, the charge and discharge curves of the button cell assembled in Comparative Example 1 in the first two cycles are as follows Figure 5 As shown, the charge and discharge curves of the button cell assembled in Comparative Example 2 in the first two cycles are as follows Figure 6 As shown, the cycle performance curves of the full battery in which the positive electrode materials prepared in Example 6 and Comparative Example 1 are assembled with the hard carbon negative electrode are as follows Figure 7 shown.
[0125] Figure 1 is a scanning electron microscope image of Example 1 of the present invention, Figure 2 This is a scanning electron microscope image of Comparative Example 1 of the present invention, Figure 3 is a scanning electron microscope image of Example 9 of the present invention, Figure 4This is a scanning electron microscope image of Example 10 of the present invention; it can be seen that the surface of the positive electrode material prepared in Example 1 is very smooth, no residual alkali remains, and the particle size is about 2-4μm; the positive electrode material prepared in Example 9 at a sintering temperature of 700°C has a very small particle size and serious agglomeration, which indicates that the material sintering at 700°C is not sufficient, which will affect the electrochemical properties of the material; the positive electrode material prepared in Example 10 at a sintering temperature of 1150°C has a too large particle size, which is not conducive to the transmission of ions, and the sodium carbonate volatilizes seriously at a high temperature of 1150°C, which may cause the sodium content of the sintered material to be seriously lower than expected, thereby affecting the electrochemical properties of the material; so a more optimal sintering temperature of 950°C was finally determined. At the same time, by comparison Figure 1 and Figure 2 The surface of the positive electrode material prepared in Example 1 is very smooth, and no residual alkali remains; while the surface of the positive electrode material prepared in Comparative Example 1 is enriched with small particles, and more residual alkali remains, which will cause the material to easily absorb water and moisture, deteriorate the processing performance, and thus affect the electrochemical properties of the material.
[0126] Figure 8 The first cycle charge and discharge curve comparison diagram of Example 1, Example 9 and Example 10, Fig. 9 : is a comparison diagram of the first cycle charge and discharge curves of Example 1, Example 14 and Example 15; Figure 8 It can be seen that there are obvious differences in the first cycle charge and discharge of Example 1 sintered at 950°C, Example 9 sintered at 1150°C, and Example 10 sintered at 700°C. The first cycle discharge of Example 9 and Example 10 are 103.7 mAh / g and 101.4 mAh / g, respectively, which are lower than 112.5 mAh / g of Example 1. This also reflects that 950°C is a better sintering temperature in terms of performance. Fig. 9 It can be seen that the first cycle charge and discharge curves of Example 1 with a holding time of 16h and Example 14 with a holding time of 8h are quite different, wherein the first cycle discharge of Example 14 is 101.6mAh / g, which is much lower than 112.5mAh / g of Example 1, indicating that the holding time of 8h is too short, the material is not sintered sufficiently, and the electrochemical performance of the obtained material is poor; the first cycle charge and discharge curves of Example 1 with a holding time of 16h and Example 15 with a holding time of 24h are basically the same, indicating that the holding time of 16h is sufficient to obtain a fully sintered material, and further increasing the sintering time to 24h increases the preparation cost, but does not improve the electrochemical performance of the material. Therefore, a better holding time of 16h was selected.
[0127] Figure 5 The charge and discharge curves of the button cell assembled in Example 1 for the first two cycles are shown in FIG. Figure 6 The charge and discharge curves of the button cell assembled in Example 6 for the first two cycles are shown in FIG. Figure 7The charge and discharge curves of the button cell assembled in Example 11 for the first two cycles are shown in FIG. Fig.10 The charge and discharge curves of the button cell assembled in Comparative Example 1 for the first two cycles; Figure 5 and Figure 6 It can be seen that both Example 1 and Example 6 start to provide charge specific capacity at around 2.5V, which corresponds to Mn 3+ / Mn 4+ redox couple, indicating that Mn 3+ The cathode materials prepared in Example 1 and Example 6 have excellent cycle performance. Fig.10 It can be seen that in the first cycle of comparative example 1, no Mn 3+ / Mn 4+ The charging platform corresponding to redox indicates that there is no Mn in the material 3+ , and the discharge curves of the first two cycles of comparative example 1 are more offset, the discharge specific capacity of the second cycle is much less than that of the first cycle, the irreversible capacity of the surface material is larger, and the cycle performance is poor; Figure 5 and Figure 7 It can be seen that trivalent manganese does not appear in the material of Example 11 sintered in an air atmosphere, while trivalent manganese appears in the material of Example 1 sintered in a nitrogen atmosphere, indicating that using manganese dioxide and manganese trioxide as raw materials and sintering in an inert atmosphere is a simple and easy method to retain trivalent manganese in the bulk phase of the material.
[0128] Fig.11 The figure is a cycle performance curve of button cells of positive electrode materials prepared in Example 1 and Comparative Example 2; the button cell assembled with the positive electrode material prepared in Example 1 has a capacity retention rate of 95.87% after 50 cycles, while the button cell assembled with the positive electrode material prepared in Comparative Example 2 has a capacity retention rate of only 70.87% after 50 cycles. By comparing the button cell performances of Example 1 and Comparative Example 2, it can be seen that the cycle performance of Comparative Example 2 prepared using Mn2O3 as a raw material is poor, which may be attributed to the fact that only Mn2O3 is used as a manganese source in an inert atmosphere, and Mn2O3 provides Mn 3+ This reduces the average valence of the transition metal, causing the sodium content of the prepared material to be far lower than the designed value, resulting in excess Na2O3. The excess Na2O3 accumulates on the surface of the material to form residual alkali, which seriously affects the cyclic stability of the material.
[0129] Fig.12The graph is a cycle performance curve of the full battery assembled with the positive electrode materials prepared in Example 6 and Comparative Example 1 and the hard carbon negative electrode, respectively. The full battery assembled with the positive electrode material prepared in Comparative Example 1 and the hard carbon negative electrode has a capacity retention rate of only 81.58% after 50 cycles, while the full battery assembled with the positive electrode material prepared in Example 6 and the hard carbon negative electrode has a capacity retention rate of 96.44% after 50 cycles. The cycle performance of Example 6 is greatly improved compared with that of Comparative Example 1, which is consistent with the Mn 3+ The introduction of Mn 3+ / Mn 4+ It is related to redox, which corresponds to the release of more sodium ions. At the same time, by limiting the discharge voltage, the subsequent Mn is kept at tetravalent, so that this part of the released sodium ions can be retained in the negative electrode to supplement the sodium ions lost in the negative electrode due to the formation of SEI film. At the same time, due to the replacement of tetravalent manganese by low-valent elements, the sodium content of the material is further increased, so that during the sodium ion deintercalation process of the positive electrode material, more sodium is retained in the bulk phase, thereby stabilizing the structure of the positive electrode material and improving the cycle performance of the whole battery.
[0130] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A sodium ion battery layered oxide positive electrode material, characterized in that: Its chemical formula is Na X Ni A Mn 3+ B Mn 4+ C TM D O2; Wherein, 0.6≤X≤0.8, 0≤A≤0.5, 0≤B≤0.3, 0≤C≤0.7, 0≤D≤0.3, and A+B+C+D=1; TM is selected from at least one of Li, K, Mg, Ca, Zn, Cu, Sr, Fe, Al, Co, Y, La and Bi.
2. A method for preparing the layered oxide positive electrode material for sodium ion batteries according to claim 1, characterized in that: include: The sodium source, the nickel source, the trivalent manganese source, the tetravalent manganese source and the TM source are mixed according to a stoichiometric ratio and then sintered at a high temperature.
3. The preparation method according to claim 2, characterized in that: First, mix the raw materials evenly, press them into tablets, and then sinter them at high temperature; The high temperature sintering process includes: firstly performing a sintering at 300°C-700°C, controlling the holding time to be 2h-16h, and then performing a secondary sintering at 700°C-1150°C, controlling the holding time to be 8h-24h; Preferably, the atmosphere during the high temperature sintering process is selected from at least one of an air atmosphere, an oxygen atmosphere, an argon atmosphere and a nitrogen atmosphere; Preferably, during the high temperature sintering process, the heating rate is controlled to be 1° C. / min-10° C. / min.
4. The preparation method according to claim 3, characterized in that: After sintering at high temperature, the material is ground into powder; Preferably, after the high-temperature sintering, the temperature is lowered to 120° C.-280° C., and then ground into powder in an environment with a relative humidity of less than 1%, and the grinding time is controlled to be 15 min-30 min.
5. The preparation method according to claim 4, characterized in that: The raw materials are mixed evenly by grinding, and then tabletted under a pressure of 40MPa-120MPa for 15min-35min; Preferably, during the grinding of the raw material, an organic solvent is added to wet the powder in the mortar, and the grinding time is controlled to be 0.5h-2.0h; More preferably, the organic solvent is selected from at least one of anhydrous ethanol and acetone.
6. The preparation method according to claim 3, characterized in that: The nickel and manganese elements are added according to the theoretical amounts by adjusting the amounts of the nickel source, the trivalent manganese source and the tetravalent manganese source, and the sodium element is added in an excess of 1% to 15% compared to the theoretical amount by adjusting the amount of the sodium source; Preferably, the sodium source is selected from at least one of Na2CO3, Na2CO3·H2O, NaHCO3, NaOH, CH3COONa, NaNO3, Na2O2, NaO2 and Na2C2O4; Preferably, the nickel source is selected from at least one of NiO and Ni(OH)2; Preferably, the manganese source is selected from at least one of MnO, Mn2O3, MnO2, MnCO3 and Mn3O4; Preferably, the TM source is selected from at least one of oxides, hydroxides and carbonates containing TM elements.
7. A positive electrode sheet, characterized in that: It comprises the sodium ion battery layered oxide positive electrode material according to claim 1 or the sodium ion battery layered oxide positive electrode material prepared by the preparation method according to any one of claims 2-6.
8. A sodium ion battery, characterized in that: Including the positive electrode sheet as described in claim 7.
9. An electrical device, characterized in that: Including the sodium ion battery as described in claim 8.