Preparation method of nutshell-derived porous carbon material and its application in lithium-ion batteries

Nut shell porous carbon materials prepared by hydrothermal pre-carbonization and high-temperature activation pyrolysis methods solve the non-renewable and contaminant problems of hard carbon materials in the prior art, and achieve high capacity and good cycle stability of the negative electrode materials of lithium-ion batteries improves the electrochemical performance of lithium-ion batteries.

CN116477623BActive Publication Date: 2024-12-03HARBIN INST OF TECH +1
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202310469632.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-12-03
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

The existing industrial preparation of hard carbon materials using bitumen or organic polymers has problems of non-renewability and pollution. Nut shell-derived carbon anode materials have low reversible capacity and short cycle life in lithium-ion batteries, which limit their application.

Method used

Porous carbon materials are prepared by hydrothermal pre-carbonization and high-temperature activation pyrolysis methods by waste biomass nut shells. They are used as the negative electrode material of lithium-ion batteries to achieve high-value conversion using biomass resources, and through appropriate hydrothermal pretreatment and activator Regulate and improve the structural order and electrochemical properties of materials.

Benefits of technology

The high specific capacity and good cycle stability of biomass-derived carbon materials were achieved. The first reversible capacity reached 706mAh/g, and the capacity retention rate after 2000 cycles under 1000mA/g current density was 74.7%, which significantly improved the dynamic performance of the material. and cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116477623B_ABST
    Figure CN116477623B_ABST
Patent Text Reader

Abstract

A method for preparing a porous carbon material derived from nutshells and its application in lithium-ion batteries, it relates to a method for preparing a porous carbon material and its application in lithium-ion batteries. The purpose of the invention is to solve the problems that the hard carbon materials currently prepared in industry mostly use asphalt or organic polymers as raw materials, which are non-renewable and polluting in the reaction process, and the nutshell-derived carbon negative electrode materials have low reversible capacity and short cycle life at higher current density. Method: 1. Mix the nutshell raw material with an acid solution; 2. Hydrothermal reaction; 3. Mix the pre-carbonized material with an activator and carbonize. The carbon material prepared by the present invention has a high reversible capacity of 50mAg ‑1 The first reversible capacity at a current density of 706 mAh g ‑1 , at 1000mAg ‑1 After 2000 cycles at a current density of ‑1 , the capacity retention rate is 74.7%, showing high reversible specific capacity and good cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method of a porous carbon material and application of the porous carbon material in a lithium ion battery. Background Art

[0002] Nowadays, climate change has become a common problem for the world, and we need to pay more attention to environmental and energy issues. As fossil energy is continuously consumed, people are increasingly in need of clean energy, such as wind and solar energy, and at the same time, the demand for energy storage is also increasing. Since lithium has the lowest reduction potential among all elements and is also the metal element with the smallest ion radius, lithium-ion batteries have higher voltage and energy density. It is precisely because of these advantages that lithium-ion batteries have undoubtedly become the most popular energy storage device in the past half century.

[0003] The electrochemical performance of lithium-ion batteries is closely related to the electrode active material, which directly affects the energy density and power density of the battery. The main source of negative electrode materials is modified natural graphite or asphalt-based artificial graphite, which has serious production pollution and is limited to 372mAhg -1 Theoretical capacity. Therefore, the research on new high-capacity negative electrode materials has attracted much attention in recent years. Hard carbon-type negative electrode materials are very ideal negative electrode materials because they contain rich graphite microcrystalline structures and large cavity volume, thus having the characteristics of high capacity and good rate performance. At present, asphalt or organic polymers are mostly used as raw materials in the industry to prepare hard carbon materials, which have the disadvantages of being non-renewable and polluting in the reaction process. As a renewable energy source, nutshell biomass has attracted widespread attention in the preparation of carbonaceous materials due to its advantages such as abundant output, non-toxicity and low cost. Nutshell biomass has a unique microstructure and itself has a self-doping effect (such as oxygen, nitrogen and phosphorus). These advantages make nutshells a promising precursor for high-performance negative electrodes after certain treatments, but nutshell-derived carbon negative electrode materials have problems such as low reversible capacity and short cycle life at higher current density, which limits their practical application in lithium-ion batteries. Summary of the invention

[0004] The purpose of the present invention is to solve the problems that the hard carbon materials currently prepared in industry mostly use asphalt or organic polymers as raw materials, which have the disadvantages of being non-renewable and having pollution in the reaction process, and the nutshell-derived carbon negative electrode materials have low reversible capacity and short cycle life at high current density, and to provide a method for preparing nutshell-derived porous carbon materials and their application in lithium-ion batteries.

[0005] The present invention provides a preparation method and application of nutshell-derived porous carbon materials. The method adopts waste biomass nutshells as a biomass source, prepares the porous carbon material by hydrothermal precarbonization and high-temperature activation pyrolysis, and uses the prepared porous carbon as a negative electrode material for lithium-ion batteries, thereby realizing high-value conversion of waste biomass materials. When used as a negative electrode material for lithium-ion batteries, the porous carbon exhibits higher specific capacity and good cycle performance.

[0006] A method for preparing a nutshell-derived porous carbon material is specifically completed by the following steps:

[0007] 1. At room temperature, the nut shell raw material is mixed with the acid solution to obtain a mixed solution; the mixed solution is heated and stirred, then washed with water until neutral, and finally placed in an oven to dry to obtain a reaction product I;

[0008] 2. Transfer the reaction product I to a high-temperature reactor, then add deionized water, and then put it into an oven for hydrothermal reaction, and finally cool it to room temperature to obtain a pre-carbonized material;

[0009] 3. Grind the pre-carbonized material and the activator thoroughly, then heat up under the protection of an inert gas for high-temperature carbonization, and then cool to room temperature to obtain a reaction product II; wash and dry the reaction product II to obtain a nutshell-derived porous carbon material.

[0010] Beneficial effects of the present invention:

[0011] 1. A biomass-derived carbon material of the present invention uses waste biomass nut shells as a precursor, which is low-cost, easy to mass-produce, and self-doped with rich and uniform oxygen atoms, which can provide additional capacity;

[0012] 2. The present invention can reduce some irreversible defects through appropriate hydrothermal pretreatment, effectively improve the structural order of carbon materials, and enhance their electrochemical properties;

[0013] 3. The present invention uses alkali as an activator, which reduces the cost of the activator, and can adjust its specific surface area and pore ratio according to the proportion of the activator; the porous structure can provide a fast channel for ions while also improving conductivity and enhancing its kinetic performance; at 50mAg -1 The first reversible capacity at a current density of 706 mAh g -1 , at 1000mAg -1 After 2000 cycles at a current density of -1 , the capacity retention rate is 74.7%, showing high reversible specific capacity and good cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1This is a SEM image of the nutshell-derived porous carbon prepared in Example 1 of the present invention;

[0015] Figure 2 XRD patterns of nutshell-derived porous carbon prepared in Example 1 of the present invention and Comparative Example 1;

[0016] Figure 3 The XPS graphs of the nutshell-derived porous carbon prepared in Example 1 of the present invention and Comparative Example 1;

[0017] Figure 4 The Raman images of the nutshell-derived porous carbon prepared in Example 1 of the present invention and Comparative Example 1;

[0018] Figure 5 This is a nitrogen adsorption / desorption isotherm diagram of the nutshell-derived porous carbon prepared in Example 1 of the present invention;

[0019] Figure 6 This is a graph showing the rate performance of nutshell-derived porous carbon prepared in Example 1 of the present invention at different current densities;

[0020] Figure 7 This is a cycle performance diagram of the nutshell-derived porous carbon prepared in Example 1 of the present invention;

[0021] Figure 8 The nutshell-derived porous carbon prepared in Example 1 of the present invention was subjected to 1000 mA g -1 Long cycle performance diagram at current density

[0022] Fig. 9 This is a cycle performance diagram of the nutshell-derived porous carbon prepared in Example 2 of the present invention;

[0023] Fig.10 This is a cycle performance diagram of the nutshell-derived porous carbon prepared in Example 3 of the present invention;

[0024] Fig.11 This is a rate performance diagram of nutshell-derived porous carbon prepared in Comparative Example 1 of the present invention at different current densities;

[0025] Fig.12 This is a cycle performance diagram of the nutshell-derived porous carbon prepared in Comparative Example 1 of the present invention;

[0026] Fig.13 This is a cycling performance diagram of the nutshell-derived porous carbon prepared in Control Example 2 of the present invention. DETAILED DESCRIPTION

[0027] Specific implementation method 1: This implementation method is a method for preparing a nutshell-derived porous carbon material, which is specifically completed by the following steps:

[0028] 1. At room temperature, the nut shell raw material is mixed with the acid solution to obtain a mixed solution; the mixed solution is heated and stirred, then washed with water until neutral, and finally placed in an oven to dry to obtain a reaction product I;

[0029] 2. Transfer the reaction product I to a high-temperature reactor, then add deionized water, and then put it into an oven for hydrothermal reaction, and finally cool it to room temperature to obtain a pre-carbonized material;

[0030] 3. Grind the pre-carbonized material and the activator thoroughly, then heat up under the protection of an inert gas for high-temperature carbonization, and then cool to room temperature to obtain a reaction product II; wash and dry the reaction product II to obtain a nutshell-derived porous carbon material.

[0031] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: the nut shell raw material described in step 1 is one or a mixture of almond shell, walnut shell, hazelnut shell and macadamia shell; the acid solution described in step 1 is hydrochloric acid with a concentration of 1 to 3 mol / L or sulfuric acid with a concentration of 1 to 3 mol / L. The other steps are the same as those in specific embodiment 1.

[0032] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the volume ratio of the mass of the nut shell raw material to the acid solution in step 1 is (3.0 g to 6.0 g): (30 mL to 60 mL). The other steps are the same as those in specific embodiment 1 or 2.

[0033] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: the temperature of the heating and stirring in step 1 is 60°C to 90°C, the time of the heating and stirring is 6h to 12h, and the speed of the heating and stirring is 700r / min to 900r / min; the temperature of the drying in step 1 is 60°C to 120°C, and the time of the drying is 8h to 16h. The other steps are the same as those in specific embodiments 1 to 3.

[0034] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: the mass ratio of the reaction product I described in step 2 to the volume of deionized water is (0.5 g to 2 g): (10 mL to 40 mL); the temperature of the hydrothermal reaction described in step 2 is 140° C. to 200° C., and the time of the hydrothermal reaction is 4 h to 8 h. The other steps are the same as those of specific embodiments 1 to 4.

[0035] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the grinding time in step 3 is 30 min to 90 min; the activator in step 3 is sodium hydroxide or potassium hydroxide; the mass ratio of the pre-carbonized material to the activator in step 3 is 1:(0.5 to 3). The other steps are the same as those in specific embodiments 1 to 5.

[0036] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the inert gas in step 3 is nitrogen or argon; the heating rate in step 3 is 3°C / min to 6°C / min; the carbonization temperature in step 3 is 600°C to 1000°C, and the carbonization time is 80min to 140min. The other steps are the same as those in specific embodiments 1 to 6.

[0037] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that: the specific method of washing described in step three is: using deionized water as a cleaning agent, using a suction filtration device to filter and wash 3 to 5 times; the drying temperature described in step three is 60°C to 120°C, and the drying time is 8h to 16h. The other steps are the same as specific embodiments one to seven.

[0038] Specific embodiment 9: This embodiment is a nutshell-derived porous carbon material used as a negative electrode material for a lithium-ion battery.

[0039] Specific embodiment ten: The difference between this embodiment and specific embodiment nine is that the preparation method of the lithium-ion battery is as follows: nutshell-derived porous carbon material, acetylene black and polyvinylidene fluoride solution dissolved in N-methylpyrrolidone are mixed in a mass ratio of 8:1:1 to form a slurry, and then evenly coated on the surface of copper foil, and finally dried under vacuum conditions of 80°C to 100°C for 10h to 12h to obtain a negative electrode sheet; a lithium sheet is used as a counter electrode, polypropylene PP is used as a diaphragm, and LiPF6 / EC+DMC+FEC is used as an electrode. The electrolyte is packaged into a lithium ion battery in a high-purity argon glove box; the mass ratio of polyvinylidene fluoride to N-methylpyrrolidone in the polyvinylidene fluoride solution dissolved in N-methylpyrrolidone is (3-5): (97-95); the preparation method of the LiPF6 / EC+DMC+FEC electrolyte is: dissolving LiPF6 into a mixed solution of EC and DMC, adding FEC additive, wherein the volume ratio of EC to DMC in the mixed solution of EC and DMC is 1:1, and the concentration of LiPF6 is 1 mol L -1 , the mass fraction of FEC is 5%. The other steps are the same as those in the ninth embodiment.

[0040] The following examples are used to verify the beneficial effects of the present invention:

[0041] Embodiment 1:

[0042] 1. Separate the almond core from the shell, grind and crush the shell, stir it with 1 mol / L sulfuric acid solution in a 60°C water bath for 6 hours at a stirring speed of 800 r / min, then repeatedly wash the acid-washed sample with deionized water until the pH value reaches neutral, and then dry it at 80°C for 12 hours to obtain the almond shell;

[0043] 2. Weigh 1.2 g of the almond shell obtained in step 1 and put it into 50 mL of polytetrafluoroethylene liner, then add 25 mL of deionized water, put it into a high-temperature reactor and seal it, then react it in an oven at 180°C for 5 hours, and after the hydrothermal reaction, filter and wash it with deionized water and anhydrous ethanol three times respectively, and then put it into an oven at 80°C for 12 hours to obtain a pre-carbonized material;

[0044] 3. Weigh 0.64g of pre-carbonized material and grind it with potassium hydroxide. Put the ground sample into a porcelain boat and put it into a tube furnace. Heat it to 700℃ at a rate of 5℃ / min under argon atmosphere and keep it warm for 2h. The argon flow rate is 200sccm. After the pyrolysis is completed, cool it to room temperature and take out the material. Filter and wash it with deionized water three times, and dry it in an oven at 80℃ for 12h to obtain a nutshell-derived porous carbon material.

[0045] The mass ratio of the pre-carbonized material to potassium hydroxide described in step three is 1:0.5.

[0046] Comparative Example 1:

[0047] 1) Separating the almond core from the shell, grinding and crushing the shell, stirring it with 1 mol / L sulfuric acid solution in a 60°C water bath for 6 hours at a stirring speed of 800 r / min, then repeatedly washing the acid-washed sample with deionized water until the pH value reaches neutral, and then drying it at 80°C for 12 hours to obtain the almond shell;

[0048] 2) Weigh 1.2g of the almond shell obtained in step 1 and put it into 50mL of polytetrafluoroethylene liner, add 25mL of deionized water, put it into a high-temperature reactor and seal it, and react it in an oven at 180°C for 5h. After the hydrothermal reaction, filter and wash it with deionized water and anhydrous ethanol three times respectively, then put it into an oven at 80°C and dry it for 12h to obtain a pre-carbonized material;

[0049] 3) Weigh 0.8 g of the pre-carbonized material and grind it thoroughly with potassium hydroxide. Put the ground sample into a porcelain boat and put it into a tube furnace. Heat it to 800°C at a rate of 5°C / min in an argon atmosphere and keep it warm for 2 hours. The argon flow rate is 200 sccm. After the pyrolysis is completed, cool it to room temperature and take out the material. Repeatedly filter and wash it with deionized water three times, and dry it in an oven at 80°C for 12 hours to obtain a nutshell-derived porous carbon material.

[0050] The mass ratio of the pre-carbonized material to potassium hydroxide described in step three is 1:0.5.

[0051] Figure 1 This is a scanning electron micrograph of the nutshell-derived porous carbon prepared in Example 1 of the present invention;

[0052] from Figure 1 It can be clearly seen that the nutshell-derived porous carbon material prepared in Example 1 of the present invention presents a highly interconnected sheet-like honeycomb structure, forming a large number of pores, which is conducive to lithium ion transmission.

[0053] The X-ray diffraction (XRD) patterns of the nutshell-derived porous carbon materials prepared in Example 1 and Comparative Example 1 are as follows: Figure 2 As shown;

[0054] Figure 2 X-ray diffraction patterns of nutshell-derived porous carbon materials prepared in Example 1 and Comparative Example 1 of the present invention;

[0055] from Figure 2 It can be seen that the nutshell-derived porous carbon materials prepared in Example 1 and Comparative Example 1 have two main diffraction peaks at 23° and 44°, corresponding to the (002) and (101) crystal planes of amorphous carbon, respectively. It is also observed that the (002) peak shifts to a larger angle with increasing pyrolysis temperature, indicating that the average spacing between graphite layers decreases and the carbon structure becomes more ordered.

[0056] Figure 3 X-ray photoelectron spectra of nutshell-derived porous carbon materials prepared in Example 1 and Comparative Example 1 of the present invention;

[0057] from Figure 3 It can be seen that the material mainly contains two elements, carbon and oxygen, and with the increase of carbonization temperature, the oxygen content continues to decrease, which verifies the self-doped oxygen characteristics of the material.

[0058] Figure 4 The Raman images of the nutshell-derived porous carbon materials prepared in Example 1 and Comparative Example 1 of the present invention;

[0059] from Figure 4 It can be seen that I D / I G >1, there are a large number of defects in the carbon skeleton, and the abundant surface defects can provide more active sites for ions.

[0060] Figure 5 This is a nitrogen adsorption / desorption isotherm diagram of the nutshell-derived porous carbon material prepared in Example 1 of the present invention;

[0061] from Figure 5 It can be seen that the specific surface area of ​​Example 1 is 912m 2 ·g-1 The rich specific surface area is conducive to the full contact between the material and the electrolyte, accelerating the electron transmission speed, thereby improving the electrochemical performance of the material.

[0062] The nutshell-derived porous carbon material prepared in Example 1, acetylene black and a polyvinylidene fluoride solution dissolved in N-methylpyrrolidone were mixed in a mass ratio of 8:1:1 to form a slurry, which was then evenly coated on the surface of a copper foil and finally dried at 80°C under vacuum for 12 h to obtain a negative electrode sheet; the active material loading per unit area was 1 mg cm -2 ; A lithium sheet is used as a counter electrode, polypropylene PP is used as a diaphragm, and LiPF6 / EC+DMC+FEC is used as an electrolyte, and a lithium-ion battery is packaged in a high-purity argon glove box; the mass ratio of polyvinylidene fluoride to N-methylpyrrolidone in the polyvinylidene fluoride solution dissolved in N-methylpyrrolidone is 3:97; the preparation method of the LiPF6 / EC+DMC+FEC electrolyte is: dissolving LiPF6 in a mixed solution of EC and DMC, adding FEC additive, wherein the volume ratio of EC to DMC in the mixed solution of EC and DMC is 1:1, and the concentration of LiPF6 is 1 mol L -1 , the mass fraction of FEC is 5%. The electrochemical performance of lithium-ion batteries was tested; the test voltage range was 0.01V~3.00V (vs.Li + / Li), the current density is 50mA g -1 ~5000mA g -1 .

[0063] The rate performance of the nutshell-derived porous carbon material prepared in Example 1 at different current densities is as follows: Figure 6 As shown;

[0064] Figure 6 This is a rate performance diagram of the nutshell-derived porous carbon material prepared in Example 1 of the present invention at different current densities;

[0065] from Figure 6 It can be seen that at 50mA g -1 The reversible capacity at the current density is 606.3 mAh g -1 , at 5000mA g -1 The discharge capacity at high current density is still 50.0 mAh g -1 , showing good rate performance at 50mA g -1 After 50 cycles, the current density is still 378 mAh g -1 The reversible capacity is as follows: Figure 7 , and at 1000mAg -1After 2000 cycles at the current density, the capacity retention rate is still 74.7%, which has good cycle stability. Figure 8 .

[0066] Figure 7 This is a cycle performance diagram of the nutshell-derived porous carbon material prepared in Example 1 of the present invention;

[0067] Figure 8 The nutshell-derived porous carbon material prepared in Example 1 of the present invention is subjected to 1000 mA g -1 Long cycle performance diagram at current density of ;

[0068] Example 2: The difference between this example and Example 1 is that in step 3, the pre-carbonized material is loaded into a porcelain boat and placed in a tube furnace, and the temperature is raised to 600°C at a rate of 5°C / min in an argon atmosphere and then kept for 2 hours, and the argon flow rate is 200 sccm. After the pyrolysis is completed, the material is cooled to room temperature and taken out, and repeatedly filtered and washed with deionized water for three times, and placed in an oven at 80°C for 12 hours to obtain a nutshell-derived porous carbon material. The other steps and parameters are the same as those in Example 1.

[0069] The nutshell-derived porous carbon material prepared in Example 2, acetylene black, and a polyvinylidene fluoride solution dissolved in N-methylpyrrolidone were mixed in a mass ratio of 8:1:1 to form a slurry, which was then evenly coated on the surface of the copper foil and finally dried at 80°C under vacuum for 12 hours to obtain a negative electrode sheet; the active material loading per unit area was 1 mg cm -2 ; A lithium sheet is used as a counter electrode, polypropylene PP is used as a diaphragm, and LiPF6 / EC+DMC+FEC is used as an electrolyte, and a lithium-ion battery is packaged in a high-purity argon glove box; the mass ratio of polyvinylidene fluoride to N-methylpyrrolidone in the polyvinylidene fluoride solution dissolved in N-methylpyrrolidone is 3:97; the preparation method of the LiPF6 / EC+DMC+FEC electrolyte is: dissolving LiPF6 in a mixed solution of EC and DMC, adding FEC additive, wherein the volume ratio of EC to DMC in the mixed solution of EC and DMC is 1:1, and the concentration of LiPF6 is 1 mol L -1 , the mass fraction of FEC is 5%. The electrochemical performance of lithium-ion batteries was tested; the test voltage range was 0.01V~3.00V (vs.Li + / Li), the current density is 50mA g -1 .

[0070] The cyclic performance of the nutshell-derived porous carbon material prepared in Example 2 is as follows: Fig. 9 As shown;

[0071] Fig. 9This is a cycle performance diagram of the nutshell-derived porous carbon material prepared in Example 2 of the present invention;

[0072] from Fig. 9 It can be seen that at 50mA g -1 After 50 cycles at the current density, the reversible capacity is 244.2 mAh g -1 .

[0073] Example 3: The difference between this example and Example 1 is that in step 3, the pre-carbonized material is loaded into a porcelain boat and placed in a tube furnace, and the temperature is raised to 900°C at a rate of 5°C / min in an argon atmosphere and then kept for 2 hours, and the argon flow rate is 200 sccm. After the pyrolysis is completed, the material is cooled to room temperature and taken out, and repeatedly filtered and washed with deionized water for three times, and placed in an oven at 80°C for 12 hours to obtain a nutshell-derived porous carbon material. The other steps and parameters are the same as those in Example 1.

[0074] The nutshell-derived porous carbon material prepared in Example 3, acetylene black, and a polyvinylidene fluoride solution dissolved in N-methylpyrrolidone were mixed in a mass ratio of 8:1:1 to form a slurry, which was then evenly coated on the surface of the copper foil and finally dried at 80°C under vacuum for 12 h to obtain a negative electrode sheet; the active material loading per unit area was 1 mg cm -2 ; A lithium sheet is used as a counter electrode, polypropylene PP is used as a diaphragm, and LiPF6 / EC+DMC+FEC is used as an electrolyte, and a lithium-ion battery is packaged in a high-purity argon glove box; the mass ratio of polyvinylidene fluoride to N-methylpyrrolidone in the polyvinylidene fluoride solution dissolved in N-methylpyrrolidone is 3:97; the preparation method of the LiPF6 / EC+DMC+FEC electrolyte is: dissolving LiPF6 in a mixed solution of EC and DMC, adding FEC additive, wherein the volume ratio of EC to DMC in the mixed solution of EC and DMC is 1:1, and the concentration of LiPF6 is 1 mol L -1 , the mass fraction of FEC is 5%. The electrochemical performance of lithium-ion batteries was tested; the test voltage range was 0.01V~3.00V (vs.Li + / Li), the current density is 50mA g -1 .

[0075] The cyclic performance of the prepared nutshell-derived porous carbon material is as follows: Fig.10 As shown;

[0076] Fig.10 This is a cycle performance diagram of the nutshell-derived porous carbon material prepared in Example 3 of the present invention;

[0077] from Fig.10 It can be seen that at 50mA g -1After 50 cycles at the current density, the reversible capacity is 229.1 mAh g -1 .

[0078] The nutshell-derived porous carbon material prepared in Control Example 1, acetylene black, and polyvinylidene fluoride solution dissolved in N-methylpyrrolidone were mixed in a mass ratio of 8:1:1 to form a slurry, which was then evenly coated on the surface of the copper foil and finally dried at 80°C under vacuum for 12 h to obtain a negative electrode sheet; the active material loading per unit area was 1 mg cm -2 ; A lithium sheet is used as a counter electrode, polypropylene PP is used as a diaphragm, and LiPF6 / EC+DMC+FEC is used as an electrolyte, and a lithium-ion battery is packaged in a high-purity argon glove box; the mass ratio of polyvinylidene fluoride to N-methylpyrrolidone in the polyvinylidene fluoride solution dissolved in N-methylpyrrolidone is 3:97; the preparation method of the LiPF6 / EC+DMC+FEC electrolyte is: dissolving LiPF6 in a mixed solution of EC and DMC, adding FEC additive, wherein the volume ratio of EC to DMC in the mixed solution of EC and DMC is 1:1, and the concentration of LiPF6 is 1 mol L -1 , the mass fraction of FEC is 5%. The electrochemical performance of lithium-ion batteries was tested; the test voltage range was 0.01V~3.00V (vs.Li + / Li), the current density is 50mA g -1 ~5000mA g -1 .

[0079] The rate performance of the nutshell-derived porous carbon material prepared in Comparative Example 1 at different current densities is shown in Fig.11 As shown;

[0080] Fig.11 This is a rate performance diagram of the nutshell-derived porous carbon material prepared in Comparative Example 1 of the present invention at different current densities;

[0081] from Fig.11 It can be seen that: At 50mA g -1 The reversible capacity at the current density is 291.5 mAh g -1 The discharge capacity at a current density of 5000mAg-1 is still 44.2mAh g -1 , and the rate performance of the nutshell-derived porous carbon material prepared in Example 1 is somewhat different. In addition, Fig.12 The nutshell-derived porous carbon material prepared in Comparative Example 1 was subjected to 50 mA g -1 Cyclic performance diagram under current density of Fig.12 It can be seen that after 50 cycles, the reversible capacity is 224.9 mAh g -1, which is significantly lower than the nutshell-derived porous carbon material prepared in Example 1.

[0082] Comparative Example 2:

[0083] 1) Separating the almond core from the shell, grinding and crushing the shell, stirring it with 1 mol / L sulfuric acid solution in a 60°C water bath for 6 hours at a stirring speed of 800 r / min, then repeatedly washing the acid-washed sample with deionized water until the pH value reaches neutral, and then drying it at 80°C for 12 hours to obtain the almond shell;

[0084] 3) Weigh 1.2 g of the above almond shell, put it into a porcelain boat and put it into a tubular furnace. Heat it to 800°C at a rate of 5°C / min under an argon atmosphere, keep it warm for 2 hours, and the argon flow rate is 200 sccm. After the pyrolysis is completed, cool it to room temperature and take out the material. Repeatedly filter and wash it with deionized water three times, and place it in an oven at 80°C to dry for 12 hours to obtain nut shell-derived carbon material.

[0085] The nutshell-derived carbon material prepared in Control Example 2, acetylene black and a polyvinylidene fluoride solution dissolved in N-methylpyrrolidone were mixed in a mass ratio of 8:1:1 to form a slurry, and then evenly coated on the surface of the copper foil, and finally dried at 80°C under vacuum conditions for 12 hours to obtain a negative electrode sheet; the unit area loading of the active material was 1 mg·cm-2; a lithium sheet was used as a counter electrode, polypropylene PP was used as a diaphragm, and LiPF6 / EC+DMC+FEC was used as an electrolyte, and a lithium ion battery was packaged in a high-purity argon glove box; the mass ratio of polyvinylidene fluoride to N-methylpyrrolidone in the polyvinylidene fluoride solution dissolved in N-methylpyrrolidone was 3:97; the preparation method of the LiPF6 / EC+DMC+FEC electrolyte was as follows: LiPF6 was dissolved in a mixed solution of EC and DMC, and a FEC additive was added, wherein the volume ratio of EC to DMC in the mixed solution of EC and DMC was 1:1, and the concentration of LiPF6 was 1 mol L -1 , the mass fraction of FEC is 5%. The electrochemical performance of lithium-ion batteries was tested; the test voltage range was 0.01V~3.00V (vs.Li + / Li), the current density is 50mA g -1 .

[0086] The cyclic performance of the nutshell-derived porous carbon material prepared in Comparative Example 2 is as follows: Fig.13 As shown;

[0087] Fig.13 This is a cycle performance diagram of the nutshell-derived porous carbon material prepared in Comparative Example 2 of the present invention;

[0088] from Fig.13 It can be seen that at 50mA g -1After 50 cycles at the current density, the reversible capacity of control example 2 is 133.1 mAh g -1 , much smaller than the embodiment.

Claims

1. A method for preparing a nutshell-derived porous carbon material, characterized in that The nutshell-derived porous carbon material prepared by the preparation method is used as a negative electrode material for lithium-ion batteries; The preparation method is specifically completed according to the following steps:

1. At room temperature, the nut shell raw material is mixed with the acid solution to obtain a mixed solution; the mixed solution is heated and stirred, then washed with water until neutral, and finally placed in an oven to dry to obtain a reaction product I; The nut shell raw material described in step 1 is one or a mixture of almond shells, walnut shells, hazelnut shells and macadamia shells; The acid solution described in step 1 is hydrochloric acid with a concentration of 1 to 3 mol / L or sulfuric acid with a concentration of 1 to 3 mol / L; 2. Transfer the reaction product I to a high-temperature reactor, then add deionized water, and then put it into an oven for hydrothermal reaction, and finally cool it to room temperature to obtain a pre-carbonized material; The temperature of the hydrothermal reaction in step 2 is 180° C., and the time of the hydrothermal reaction is 4 to 8 hours; 3. Grind the pre-carbonized material and the activator thoroughly, then heat them up under the protection of an inert gas for high-temperature carbonization, and then cool them to room temperature to obtain a reaction product II; washing and drying the reaction product II to obtain a nutshell-derived porous carbon material; The carbonization temperature in step 3 is 700° C., and the carbonization time is 120 min.

2. The method for preparing a nutshell-derived porous carbon material according to claim 1, characterized in that The volume ratio of the mass of the nut shell raw material described in step 1 to the acid solution is (3.0 g to 6.0 g): (30 mL to 60 mL).

3. The method for preparing a nutshell-derived porous carbon material according to claim 1, characterized in that The temperature of the heating and stirring described in step one is 60°C to 90°C, the time of the heating and stirring is 6h to 12h, and the speed of the heating and stirring is 700r / min to 900r / min; the temperature of the drying described in step one is 60°C to 120°C, and the time of the drying is 8h to 16h.

4. The method for preparing a nutshell-derived porous carbon material according to claim 1, characterized in that The mass ratio of the reaction product I described in step 2 to the volume ratio of deionized water is (0.5 g to 2 g): (10 mL to 40 mL).

5. The method for preparing a nutshell-derived porous carbon material according to claim 1, characterized in that The grinding time described in step three is 30min to 90min; the activator described in step three is sodium hydroxide or potassium hydroxide; the mass ratio of the pre-carbonized material to the activator described in step three is 1:(0.5 to 3).

6. The method for preparing a nutshell-derived porous carbon material according to claim 1, characterized in that The inert gas described in step three is nitrogen or argon; the heating rate described in step three is 3°C / min to 6°C / min.

7. The method for preparing a nutshell-derived porous carbon material according to claim 1, characterized in that The specific method of washing described in step three is: using deionized water as a cleaning agent, using a suction filtration device to filter and wash 3 to 5 times; the drying temperature described in step three is 60° C. to 120° C., and the drying time is 8 h to 16 h.

8. The method for preparing a nutshell-derived porous carbon material according to claim 1, characterized in that The preparation method of the lithium-ion battery is as follows: nutshell-derived porous carbon material, acetylene black and polyvinylidene fluoride solution dissolved in N-methylpyrrolidone are mixed in a mass ratio of 8:1:1 to form a slurry, and then evenly coated on the surface of copper foil, and finally dried under vacuum conditions of 80°C to 100°C for 10h to 12h to obtain a negative electrode sheet; a lithium sheet is used as a counter electrode, polypropylene PP is used as a diaphragm, and LiPF6 / EC+DMC+FEC is used as an electrolyte, and encapsulated in a high-purity argon glove box. The lithium-ion battery is formed; the mass ratio of polyvinylidene fluoride to N-methylpyrrolidone in the polyvinylidene fluoride solution dissolved in N-methylpyrrolidone is (3-5): (97-95); the preparation method of the LiPF6 / EC+DMC+FEC electrolyte is: dissolving LiPF6 into a mixed solution of EC and DMC, adding FEC additive, wherein the volume ratio of EC to DMC in the mixed solution of EC and DMC is 1:1, and the concentration of LiPF6 is 1 molL -1 , the mass fraction of FEC is 5%.

Citation Information

Patent Citations

  • Method for preparing activated carbon through walnut shells and application of activated carbon to degradation of substituted ureas herbicides isoproturon through specific adsorption-catalysis

    CN105217628A

  • Preparation method of biomass based activated carbon with high CO2 adsorption efficiency

    CN106517181A

  • Method for synthesizing flaky porous carbon in hydrothermal mode based on biomass

    CN107021483A

  • Activated carbon, hydrochar and processes for making same

    CN107108232A

  • Preparation method of high-capacitive performance hierarchically-porous charcoal based on walnut shells

    CN107697913A