Mobile phone rear cover with magnetic texture and optical texture and manufacturing method thereof

By using spherical magnetic powder and UV light curing technology, combined with magnetic field induction and multi-layer structural coating, the problems of high cost and appearance defects in the production process of magnetic pattern mobile phone back cover in the prior art are solved, and low-cost and efficient Magnetic texture and optical texture formation significantly improve the quality and stability of the product.

CN119052360APending Publication Date: 2024-11-29DONGGUAN JULONG HIGH-TECH ELECTRONIC TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411173975.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing mobile phone back cover with magnetic patterns has high cost and appearance defects during the production process, such as black dots, dark lines and particles, and the two-dimensional sheet magnetic powder is prone to being not arranged correctly during the directional arrangement. , leading to visual problems.

Method used

Spherical magnetic powder is combined with UV light curing glue, and the spherical magnetic powder is induced to be arranged in a directional manner through magnetic field, and a hardened layer is formed during the UV light curing process, reducing curing time and energy consumption. At the same time, glass micro-structured with multi-layer structure is adopted. Bead and iron nanolayers are coated to improve mechanical stability and magnetic properties and reduce production costs.

Benefits of technology

It significantly reduces the dark lines and black spot problems caused by poor particle arrangement, reduces production costs, and improves the mechanical stability and appearance aesthetics of the product, reducing the occurrence of particle problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119052360A_ABST
    Figure CN119052360A_ABST
Patent Text Reader

Abstract

The invention discloses a mobile phone rear cover with magnetic textures and optical textures and a manufacturing method of the mobile phone rear cover. The manufacturing method comprises the following steps that (1) spherical magnetic powder and UV photocuring glue are mixed to obtain UV photocuring magnetic glue; (2) coating the UV photocuring magnetic glue between the composite board and the optical texture mold; (3) applying a magnetic field to induce directional arrangement of the spherical magnetic powder; (4) performing UV photocuring after the step (3) to enable the UV photocuring magnetic glue to form a hardened layer, wherein the hardened layer is provided with optical textures and magnetic textures; (5) the optical texture mold is removed, and a PVD layer and a bottom covering layer are sequentially formed on the surface of the hardened layer; (6) performing high-pressure forming after the step (5) to form a semi-finished product; (7) spraying hardening liquid on the surface of the semi-finished product; and (8) cutting after the step (7). The manufacturing method is low in production cost, and the probability of appearance flaws such as black spots, dark lines and particles generated on the rear cover of the mobile phone is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mobile phone back cover manufacturing, and in particular relates to a mobile phone back cover with magnetic texture and optical texture and a manufacturing method thereof. Background Art

[0002] With the development of 5G technology, the use of metal back covers of mobile phones has gradually decreased. This is because metal materials will have a shielding effect on 5G signals and affect the quality of communication. In contrast, PMMA / PC composite boards have become increasingly popular in the new generation of smartphones due to their good signal penetration and lightweight characteristics. PMMA / PC composite boards achieve a high-hardness surface, i.e., a glass-like effect, through surface treatment technology (such as spray coating). PMMA / PC composite boards can also achieve various colorful decorative effects on the inner layer of the composite board through processes such as UV transfer, physical vapor deposition (PVD), and silk screen printing, which enhances the visual appeal of the back cover of the mobile phone; these advantages make PMMA / PC composite boards an ideal choice for the back cover of smartphones in the 5G era.

[0003] In order to achieve the innovation of CMF effect on the back cover of mobile phones, in recent years, researchers have developed a technology for applying magnetic patterns on the back cover of mobile phones. For example, Chinese patent CN118200423 A discloses that magnetic ink containing magnetic powder is screen-printed on the surface of the pre-hardened layer, and the magnetic field formed by the magnetic mold is used to orient the magnetic powder to form a specific pattern (texture). Because the magnetic powder itself has color, coupled with the spatial distribution of the magnetic field, the texture formed has texture (color) on the one hand, and gives the texture depth of field or agile effect on the other hand, which is completely different from the CMF effect formed by the traditional texture plus coating process. However, this kind of mobile phone back cover with magnetic pattern effect also encountered some challenges in the production process. On the one hand, it is necessary to maintain the ink curing at a temperature of 80-85℃ for 120-130min, and the magnetic mold must be used continuously to maintain the magnetic field during the period, which means that a large number of magnetic molds are required in mass production, and the production cost is high; on the other hand, the back cover of the mobile phone made by this method will have some appearance defects, such as black spots, dark lines, particles and other problems.

[0004] Therefore, there is an urgent need for a mobile phone back cover with magnetic texture and optical texture and a manufacturing method thereof to solve the deficiencies of the prior art problems. Summary of the invention

[0005] In view of the above problems, the purpose of the present invention is to provide a mobile phone back cover with magnetic texture and optical texture and a method for manufacturing the same. The production method has low production cost and effectively reduces the probability of appearance defects such as black spots, dark lines, particles, etc. on the mobile phone back cover.

[0006] To achieve the above objectives, the first aspect of the present invention provides a method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture, comprising the following steps:

[0007] (1) mixing spherical magnetic powder and UV light-curing glue to obtain UV light-curing magnetic glue;

[0008] (2) applying UV light-curing magnetic glue between the composite board and the optical texture mold;

[0009] (3) applying a magnetic field to induce spherical magnetic powder to align;

[0010] (4) performing UV light curing after step (3) to form a hardened layer of the UV light-cured magnetic glue, wherein the hardened layer has an optical texture and a magnetic texture;

[0011] (5) removing the optical texture mold and sequentially forming a PVD layer and a capping layer on the surface of the hardened layer;

[0012] (6) performing high pressure forming after step (5) to form a semi-finished product;

[0013] (7) Sprinkling hardening liquid on the surface of the semi-finished product;

[0014] (8) Cutting is performed after step (7).

[0015] The inventor of the present invention found in the process of invention that the magnetic powder used in the prior art is a nano powder material with a two-dimensional flaky structure. This type of flaky particles has a significant aspect ratio and a specific directionality in space. This characteristic requires a certain amount of time to arrange to form a magnetic pattern and is more likely to be incorrectly arranged during the arrangement process. If the particles are not correctly arranged, the flaky particles may be locally aggregated to form visual black spots, and the magnetic strength of certain areas may decrease due to incorrect arrangement of the particles, thereby producing visual dark lines. In addition, a long baking environment will increase the probability of dust falling on the surface of the product, thereby producing visual particles. Based on this, the magnetic powder of the present invention uses spherical magnetic powder. Unlike flaky particles, spherical particles do not have a significant aspect ratio. This characteristic enables the spherical magnetic powder to have the same physical properties in all directions. Therefore, these spherical magnetic powders can be quickly arranged under the action of a magnetic field, and then quickly fixed under UV to form a clear magnetic pattern, which effectively reduces the particle problem caused by dust falling on the surface during a long arrangement process, and significantly reduces the problems of dark lines and black spots caused by poor particle arrangement. In addition, the present invention adopts UV curing to replace traditional thermal curing, which can greatly shorten the curing time and reduce energy consumption. At the same time, the number of molds can be greatly reduced, thereby significantly reducing production costs.

[0016] Furthermore, the spherical magnetic powder of the present invention includes spherical glass microbeads and a shell layer sequentially coated on the surface of the glass microbeads, and the shell layer sequentially includes a three-layer structure of a SiO2 layer, a TiO2 layer, and an iron nanolayer, or sequentially includes a five-layer structure of a SiO2 layer, a TiO2 layer, an iron nanolayer, SiO2, and TiO2. The iron nanolayer is the part that exerts a magnetic effect. By uniformly coating the iron nanoparticles on the spherical glass microbeads, the appearance problems such as dark lines and black spots caused by the poor arrangement of two-dimensional flaky particles can be reduced; in addition, the glass microbeads have high hardness and wear resistance, which can improve the mechanical stability of the entire magnetic powder; and the SiO2 layer can enhance the adhesion between the TiO2 layer and the glass microbeads, and the TiO2 layer can provide a smooth surface, which is conducive to the uniform coating of the iron nanolayer. Therefore, by using the SiO2 layer and the TiO2 layer, it can be ensured that the iron nanolayer can be uniformly and stably coated on the surface of the glass microbeads.

[0017] Furthermore, the particle size of the glass microspheres of the present invention is 20 μm or less, and the thickness of the shell layer is 200 to 500 nm. Specifically, the density of the glass microspheres is <0.6 g / cm 3 ; The oil absorption value of glass microspheres is 0.2-0.6g oil / cm 3 More specifically, a SiO2 layer, a TiO2 layer and an iron nanolayer are sequentially deposited on the surface of the spherical glass microbeads by physical vapor deposition (PVD). The PVD method preferably adopts an electron gun coating method, and the particle size of the glass microbeads is preferably less than 5 μm.

[0018] Furthermore, the shell layer of the present invention also includes an indium tin layer. Indium tin (ITO) is a transparent conductive oxide with good conductive properties. Depositing the ITO layer outside the shell layer can provide conductivity, which is very important for applications requiring conductive properties and helps to achieve electromagnetic shielding or conductive functions in certain applications.

[0019] Further, the UV light-curing glue of the present invention comprises UV resin, UV monomer, photoinitiator and auxiliary agent. Specifically, the UV resin can be at least one of polyurethane acrylate, polyester acrylate and pure acrylate resin. The UV monomer can be at least one of monofunctional isobornyl acrylate (IBOA), ethyl vinyl acetate acrylate (VEEA), NVP (N-vinyl pyrrolidone) and tetrahydrofuran acrylate (THFA); it can also be at least one of difunctional hexanediol diacrylate (HDDA), tripropylene glycol diacrylate (TPGDA) and neopentyl glycol diacrylate (NPGDA); of course, it can also be at least one of trimethylolpropane triacrylate (TMPTA) and dipentaerythritol pentaacrylate (DPHA) with a functionality of 3 or more. The photoinitiator can be at least one of 1173, 184, TPO, TPO-L, 369 and 819. The auxiliary agent includes at least one of a dispersant, a wetting agent and a leveling agent. Specifically, the dispersant may be a polyester multi-chain polymer dispersant DISUPERS24, the wetting agent may be a polyether-modified polydimethylsiloxane, and the leveling agent may be a polyether-modified silicone resin or a silicone-modified acrylic resin. Of course, the types of dispersants, wetting agents, and leveling agents are not limited thereto, and those skilled in the art may select other types of dispersants, wetting agents, and leveling agents according to actual needs.

[0020] Furthermore, the UV light-curable magnetic glue of the present invention comprises 3 to 5 parts of spherical magnetic powder, 40 to 65 parts of UV resin, 15 to 25 parts of UV monomer, 2 to 4 parts of photoinitiator and 0.5 to 2 parts of auxiliary agent in terms of mass fraction. Specifically, the spherical magnetic powder can be but not limited to 3 parts, 4 parts, 5 parts; the UV resin can be but not limited to 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts; the UV monomer can be but not limited to 15 parts, 18 parts, 22 parts, 25 parts; the photoinitiator can be but not limited to 2 parts, 3 parts, 4 parts; the auxiliary agent can be but not limited to 0.5 parts, 1 part, 1.5 parts, 2 parts.

[0021] Furthermore, in step (2) of the present invention, the thickness of the UV light-cured magnetic glue after coating is 15 to 25 μm. Specifically, the thickness of the UV light-cured magnetic glue after coating can be, but is not limited to, 15 μm, 18 μm, 20 μm, 22 μm, or 25 μm.

[0022] Furthermore, in step (3) of the present invention, the magnetic field is formed by a magnetic mold. The magnetism of the magnetic mold attracts the spherical magnetic powders and makes them oriented according to the arrangement of the magnetic poles of the mold.

[0023] Furthermore, in step (4) of the present invention, the UV curing time is 1 to 2 seconds; the intensity of the UV light source is 80 to 120 W / cm 2Using ultraviolet rays, the UV resin and UV monomer in the UV light-curing magnetic glue undergo a cross-linking reaction and solidify to form a hardened layer. In this process, the magnetic texture formed by the spherical magnetic powder is fixed, and the pattern on the optical texture mold is also transferred to the hardened layer to form the required optical texture.

[0024] Furthermore, step (7) of the present invention further includes printing the outer texture on the hardening liquid and curing the semi-finished product after printing the outer texture. In order to improve the appearance of the product, the required outer texture can be printed on the surface after high pressure molding, which can ensure that the outer texture does not crack even for the back cover of the mobile phone with a curvature or a special shape.

[0025] Further, the thickness of the composite board of the present invention is 0.3-0.5 mm. Specifically, the thickness of the composite board may be, but is not limited to, 0.3 mm, 0.4 mm, or 0.5 mm. More specifically, the composite board is a PMMA / PC composite board.

[0026] Furthermore, the thickness of the PVD layer of the present invention is 30 to 250 nm. Specifically, the PVD layer can be formed by a physical vapor deposition method. The structure of the PVD layer can be ZrO / SiO / NbO / SiO / NbO to achieve a brightening and gorgeous effect; the structure of the PVD layer can also be ZrO / SiO / NbO / In / SiO / NbO to achieve a bright silver effect.

[0027] Furthermore, the thickness of the cover bottom layer of the present invention is 30-50 μm. The cover bottom layer can be realized by silk-screen printing of white ink, black ink, gray ink, etc. The thickness of the cover bottom layer can be specifically but not limited to 30 μm, 32 μm, 35 μm, 38 μm, 40 μm, 45 μm, 50 μm.

[0028] Correspondingly, the second aspect of the present invention provides a mobile phone back cover having a magnetic texture and an optical texture, which is manufactured by the above-mentioned method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a SEM image of the spherical magnetic powder used in Example 1 of the present invention.

[0030] Figure 2 This is a SEM image of the two-dimensional flaky magnetic powder used in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0031] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.

[0032] Example 1

[0033] This embodiment provides a method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture, comprising the following steps:

[0034] (1) 4 parts of spherical magnetic powder, 45 parts of polyurethane acrylate, 20 parts of difunctional hexanediol diacrylate, 1.5 parts of 1173, 1 part of 184, 0.5 parts of polyether-modified polydimethylsiloxane, 0.7 parts of DISUPER S24, and 0.3 parts of BYK333 were stirred and mixed to obtain UV light-curing magnetic glue;

[0035] (2) coating a UV light-curing magnetic glue between the PC surface of the PMMA / PC composite sheet and the optical texture mold, wherein the thickness of the UV light-curing magnetic glue after coating is 20 μm, and the thickness of the PMMA / PC composite sheet is 0.5 mm;

[0036] (3) applying a magnetic field to induce the spherical magnetic powder to align, the magnetic field being formed by a magnetic mold;

[0037] (4) After step (3), UV light curing is performed to form a hardened layer of the UV light-cured magnetic glue, and the hardened layer has an optical texture and a magnetic texture. The UV light curing time is 1.5 seconds; the intensity of the ultraviolet light source is 100W / cm 2 ;

[0038] (5) removing the optical texture mold and sequentially forming a PVD layer with a thickness of 200 nm and a white ink cover layer with a thickness of 40 μm on the surface of the hardened layer;

[0039] (6) performing high pressure forming after step (5) to form a semi-finished product;

[0040] (7) coating the surface of the semi-finished product with a curing liquid (PPG ECP600), then printing an outer texture on the curing liquid and curing the semi-finished product after printing the outer texture;

[0041] (8) performing cutting after step (7);

[0042] The preparation of spherical magnetic powder includes: depositing SiO2 layer, TiO2 layer and iron nanolayer on the surface of spherical glass microbeads (particle size is less than 10μm) in sequence by physical vapor deposition, wherein the sum of the thickness of SiO2, TiO2 and iron nanolayers is 300nm.

[0043] Example 2

[0044] This embodiment provides a method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture, comprising the following steps:

[0045] (1) 3 parts of spherical magnetic powder, 50 parts of polyurethane acrylate, 12 parts of hexanediol diacrylate with 2 functionalities, 10 parts of trimethylolpropane triacrylate with 3 functionalities, 1.7 parts of 1173, 0.3 parts of polyether-modified polydimethylsiloxane, 1 part of DISUPER S24, and 0.2 parts of BYK333 were stirred and mixed to obtain UV light-curing magnetic glue;

[0046] (2) coating a UV light-curing magnetic glue between the PC surface of the PMMA / PC composite sheet and the optical texture mold, wherein the thickness of the UV light-curing magnetic glue after coating is 15 μm, and the thickness of the PMMA / PC composite sheet is 0.5 mm;

[0047] (3) applying a magnetic field to induce the spherical magnetic powder to align, the magnetic field being formed by a magnetic mold;

[0048] (4) After step (3), UV light curing is performed to form a hardened layer of the UV light-cured magnetic glue, and the hardened layer has an optical texture and a magnetic texture. The UV light curing time is 2 seconds; the intensity of the ultraviolet light source is 80W / cm 2 ;

[0049] (5) removing the optical texture mold and sequentially forming a PVD layer with a thickness of 250 nm and a white ink cover layer with a thickness of 30 μm on the surface of the hardened layer;

[0050] (6) performing high pressure forming after step (5) to form a semi-finished product;

[0051] (7) coating the surface of the semi-finished product with a curing liquid (PPG ECP600), then printing an outer texture on the curing liquid and curing the semi-finished product after printing the outer texture;

[0052] (8) performing cutting after step (7);

[0053] The preparation of spherical magnetic powder includes: using physical vapor deposition to deposit SiO2 layer, TiO2 layer, iron nanolayer and indium tin layer on the surface of spherical glass beads (particle size is less than 10μm), wherein the sum of the thickness of SiO2, TiO2, iron nanolayer and indium tin layer is 400nm.

[0054] Example 3

[0055] This embodiment provides a method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture, comprising the following steps:

[0056] (1) 5 parts of spherical magnetic powder, 60 parts of pure acrylate resin, 15 parts of monofunctional isobornyl acrylate, 8 parts of trifunctional trimethylolpropane triacrylate, 2 parts of 1173, 0.7 parts of polyether-modified polydimethylsiloxane, 0.7 parts of DISUPER S24, and 0.5 parts of BYK333 were stirred and mixed to obtain UV light-curing magnetic glue;

[0057] (2) coating a UV light-curing magnetic glue between the PC surface of the PMMA / PC composite sheet and the optical texture mold, wherein the thickness of the UV light-curing magnetic glue after coating is 25 μm, and the thickness of the PMMA / PC composite sheet is 0.5 mm;

[0058] (3) applying a magnetic field to induce the spherical magnetic powder to align, the magnetic field being formed by a magnetic mold;

[0059] (4) After step (3), UV light curing is performed to form a hardened layer of the UV light-cured magnetic glue, and the hardened layer has an optical texture and a magnetic texture. The UV light curing time is 1 second; the intensity of the ultraviolet light source is 120 W / cm 2 ;

[0060] (5) removing the optical texture mold and sequentially forming a PVD layer with a thickness of 150 nm and a white ink cover layer with a thickness of 50 μm on the surface of the hardened layer;

[0061] (6) performing high pressure forming after step (5) to form a semi-finished product;

[0062] (7) coating the surface of the semi-finished product with a curing liquid (PPG ECP600), then printing an outer texture on the curing liquid and curing the semi-finished product after printing the outer texture;

[0063] (8) performing cutting after step (7);

[0064] The preparation of spherical magnetic powder includes: using physical vapor deposition to deposit SiO2 layer, TiO2 layer, iron nanolayer, SiO2 layer, and TiO2 layer in sequence on the surface of spherical glass beads (particle size is less than 10μm), wherein the sum of the thickness of SiO2, TiO2, iron nanolayer, SiO2 layer, and TiO2 layer is 500nm.

[0065] Comparative Example 1

[0066] This comparative example provides a method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture, comprising the following steps:

[0067] (1) Magnetic ink (magnetic white JM-10182) containing two-dimensional flaky magnetic powder (particle size of less than 10 μm) was screen-printed on the PC surface of the PMMA / PC composite sheet (screen mesh number was 200 meshes), the thickness of the magnetic ink was 20 μm, and the thickness of the PMMA / PC composite sheet was 0.5 mm;

[0068] (2) applying a magnetic field to induce the magnetic powder to align, the magnetic field being formed by a magnetic mold;

[0069] (3) baking at 80° C. for 120 minutes after step (3) to form a magnetic ink layer;

[0070] (4) forming an optical texture layer with a thickness of 20 μm on the magnetic ink layer by UV transfer;

[0071] (5) forming a PVD layer with a thickness of 200 nm and a white ink cover layer with a thickness of 40 μm on the surface of the optical texture layer in sequence;

[0072] (6) performing high pressure forming after step (5) to form a semi-finished product;

[0073] (7) coating the surface of the semi-finished product with a curing liquid (PPG ECP600), then printing an outer texture on the curing liquid and curing the semi-finished product after printing the outer texture;

[0074] (8) Cutting is performed after step (7).

[0075] Comparative Example 2

[0076] This comparative example provides a method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture, comprising the following steps:

[0077] (1) 4 parts of two-dimensional flaky magnetic powder (with a particle size of less than 10 μm), 45 parts of polyurethane acrylate, 20 parts of difunctional hexanediol diacrylate, 1.5 parts of 1173, 1 part of 184, 0.5 parts of polyether-modified polydimethylsiloxane, 0.7 parts of DISUPER S24, and 0.3 parts of BYK333 were stirred and mixed to obtain a UV light-curing magnetic glue;

[0078] (2) coating a UV light-curing magnetic glue between the PC surface of the PMMA / PC composite sheet and the optical texture mold, wherein the thickness of the UV light-curing magnetic glue after coating is 20 μm, and the thickness of the PMMA / PC composite sheet is 0.5 mm;

[0079] (3) applying a magnetic field to induce the magnetic powder to align, the magnetic field being formed by a magnetic mold;

[0080] (4) After step (3), UV light curing is performed to form a hardened layer of the UV light-cured magnetic glue, and the hardened layer has an optical texture and a magnetic texture. The UV light curing time is 1.5 seconds; the intensity of the ultraviolet light source is 100W / cm 2 ;

[0081] (5) removing the optical texture mold and sequentially forming a PVD layer with a thickness of 200 nm and a white ink cover layer with a thickness of 40 μm on the surface of the hardened layer;

[0082] (6) performing high pressure forming after step (5) to form a semi-finished product;

[0083] (7) coating the surface of the semi-finished product with a curing liquid (PPG ECP600), then printing an outer texture on the curing liquid and curing the semi-finished product after printing the outer texture;

[0084] (8) Cutting is performed after step (7).

[0085] According to the preparation methods of Examples 1 to 3 and Comparative Examples 1 to 2, 100 mobile phone back covers were produced respectively, and then the number of black spots, dark lines and particles in the 100 mobile phone back covers was counted. The results are shown in Table 1.

[0086] Table 1

[0087]

[0088] Comparing Example 1 with Comparative Example 1, it can be seen that the mobile phone back cover prepared by the preparation method of Comparative Example 1 has more appearance problems caused by particles. This is because long-term thermal curing will greatly increase the probability of dust in the environment falling onto the product surface, which in turn causes more appearance problems caused by particles on the mobile phone back cover. At the same time, because the two-dimensional flaky magnetic powder has a significant aspect ratio, the two-dimensional flaky magnetic powder is more likely to be incorrectly arranged during the arrangement process, which will also increase the probability of black spots and black lines.

[0089] By comparing Example 1 with Comparative Example 2, it can be seen that the mobile phone back cover prepared by the preparation method of Comparative Example 2 has more appearance problems caused by black spots and dark lines. This is because the two-dimensional flaky magnetic powder has a significant aspect ratio, and the two-dimensional flaky magnetic powder needs a certain arrangement time to form a magnetic pattern. If the UV method time is too short, more two-dimensional flaky magnetic powder will be fixed without being properly arranged, which will cause more appearance problems caused by black spots and dark lines on the back cover of the mobile phone.

[0090] In addition, in Comparative Example 1, a magnetic ink layer with a magnetic texture is first formed by screen printing and thermal curing, and then an optical texture is formed on the surface of the magnetic ink layer by transfer printing. In Example 1, UV light-cured magnetic glue is applied between the composite board and the optical texture mold, and then the optical texture and the magnetic texture are formed simultaneously by UV curing. It is obvious that the present application combines the two processes of forming the optical texture and the magnetic texture together, which not only shortens the curing time and simplifies the process, but also greatly reduces the number of magnetic molds required, thereby significantly reducing the production cost.

[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture, characterized in that: The following steps are involved: (1) mixing spherical magnetic powder and UV light-curing glue to obtain UV light-curing magnetic glue; (2) applying the UV light-curing magnetic glue between the composite board and the optical texture mold; (3) applying a magnetic field to induce the spherical magnetic powder to be oriented; (4) after step (3), UV light curing is performed to form a hardened layer of the UV light-cured magnetic glue, wherein the hardened layer has an optical texture and a magnetic texture; (5) removing the optical texture mold and sequentially forming a PVD layer and a capping layer on the surface of the hardened layer; (6) performing high pressure forming after step (5) to form a semi-finished product; (7) coating the surface of the semi-finished product with a curing liquid; (8) Cutting is performed after step (7).

2. The method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture as claimed in claim 1, characterized in that: The spherical magnetic powder includes spherical glass beads and a shell layer coated on the surface of the glass beads, and the shell layer includes SiO2 layer, TiO2 layer, iron nanolayer in sequence or includes SiO2 layer, TiO2 layer, iron nanolayer, SiO2, and TiO2 in sequence.

3. The method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture as claimed in claim 2, characterized in that: The particle size of the glass microbeads is 20 μm or less, and the thickness of the shell layer is 200 to 500 nm.

4. The method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture as claimed in claim 1, characterized in that: The UV light curing glue shown includes UV resin, UV monomer, photoinitiator and auxiliary agent.

5. The method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture as claimed in claim 4, characterized in that: In parts by mass, the UV light-curing magnetic glue comprises 3 to 5 parts of the spherical magnetic powder, 40 to 65 parts of the UV resin, 15 to 25 parts of the UV monomer, 2 to 4 parts of the photoinitiator and 0.5 to 2 parts of the auxiliary agent.

6. The method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture as claimed in claim 1, characterized in that: The thickness of the UV light-cured magnetic glue after coating in step (2) is 15 to 25 μm.

7. The method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture as claimed in claim 1, characterized in that: The magnetic field in step (3) is formed by a magnetic mold.

8. The method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture as claimed in claim 1, characterized in that: The UV curing time in step (4) is 1 to 2 seconds; the UV light intensity is 80 to 120 W / cm 2 .

9. The method for manufacturing a mobile phone back cover having a magnetic texture and an optical texture as claimed in claim 1, characterized in that: Step (7) also includes printing an external texture on the hardening liquid and curing the semi-finished product after printing the external texture.

10. A mobile phone back cover with magnetic texture and optical texture, characterized in that: The mobile phone back cover having magnetic texture and optical texture is manufactured by the manufacturing method of any one of claims 1 to 9.

Citation Information

Cited By