Hydrogenation catalyst as well as preparation method and application thereof
By using an organic treatment agent with a hydrocarbon group and a -C(=O)-O group coordination group and an active metal complex, an oil-soluble catalyst dispersed in the organic treatment agent is formed, and the insufficient hydrogenation activity of the oil-soluble catalyst is solved. The problem of easy oxidation achieves higher hydrogenation activity and storage stability.
Patent Information
- Application Number
- CN202310637673.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
The existing oil-soluble catalysts have insufficient hydrogenation activity during hydrotreatment and are prone to oxidation and deterioration, affecting storage and transportation.
The organic treatment agent with hydrocarbon moiety and -C(=O)-O group coordination group is mixed with the active metal complex to remove part of the organic ligand to form an oil-soluble catalyst dispersed in the organic treatment agent to increase the catalyst Thermal stability and hydrogenation activity.
It improves the thermal stability and hydrogenation activity of the catalyst, enhances the residual cracking rate and distillate yield, reduces the condensation rate, and is suitable for storage and transportation.
Smart Images

Figure CN119056494A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of petrochemical industry, and in particular, relates to a hydrogenation catalyst and a preparation method and application thereof. Background Art
[0002] With the decline in the yield of light oil products and the growing demand for light oil products, efficient processing of petroleum, especially the efficient conversion of high-sulfur, high-nitrogen inferior heavy oil into light oil and gas, is an effective way to solve the current problems of tight domestic energy supply and demand and high dependence on foreign crude oil.
[0003] The oil-soluble non-supported catalyst used in the slurry bed residual oil processing technology has the characteristics of high dispersibility, nano-size and high hydrogenation activity, can overcome steric hindrance, efficiently convert asphaltene, and avoid the problems of short operation cycle caused by coking and scaling, so it is regarded as an effective way to hydrogenate and upgrade the raw oil products. However, the current preparation of synthetic oil-soluble catalysts also contains a certain amount of organic ligand compounds. For example, when preparing synthetic oil-soluble highly dispersed Mo-based catalyst products, in order to ensure that more metals can be converted into catalyst products (metal conversion rate>95%), excessive organic coordination agents are usually used in the preparation process. Therefore, the catalyst product usually contains a large amount of organic ligand compounds. At the same time, the catalyst product is in liquid form and is easily oxidized and deteriorated by air, which is not conducive to storage and transportation. Therefore, how to deal with the solvent in the recovered oil-soluble catalyst to obtain an ideal treated product is a problem that needs to be solved.
[0004] Chinese patent application 201810186262.X discloses a method for treating an oil-soluble catalyst, which is to react an oil-soluble catalyst with an aniline compound at 30-300°C for 0.5-5h until the reaction is complete; vacuum dry completely at 30-80°C, and cool to room temperature to obtain an oil-soluble hydrogenation catalyst. Chinese patent ZL201911047233.6 provides a preparation method and application of a heavy oil hydrocracking molybdenum nickel catalyst, which dissolves and disperses a hexavalent molybdenum source compound with a solvent, adds an inorganic acid catalyst, reacts with a small molecule organic acid, then adds a macromolecular organic acid or ester, separates the reaction product to remove the solvent phase, washes the oil phase with water, and obtains an organic molybdenum salt after vacuum distillation to remove the light component, and then uses a similar method to prepare an organic nickel salt; the organic molybdenum salt and the organic nickel salt are mixed in proportion to obtain a heavy oil hydrocracking molybdenum nickel catalyst.
[0005] Chinese patent application 202210674912.1 discloses a method for preparing an organic acid molybdenum oil-soluble catalyst for slurry bed hydrogenation, using a long-chain organic acid as an organic ligand and a molybdenum source as its catalytically active metal. The method allows the prepared product to stand for a preset length of time and then cools it to room temperature, then adds a preset volume ratio of toluene or xylene to the cooled oil phase for washing, and then evaporates the solvent, and then dries to obtain the organic acid molybdenum oil-soluble catalyst.
[0006] However, the hydrogenation activity of existing oil-soluble catalysts when used in hydroprocessing still needs to be improved. Summary of the invention
[0007] The object of the present invention is to improve the hydrogenation activity of an oil-soluble catalyst.
[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides a hydrogenation catalyst, comprising an organic treatment agent and an oil-soluble catalyst dispersed in the organic treatment agent; wherein the oil-soluble catalyst comprises an active metal central atom or central ion and an organic ligand coordinated with the active metal central atom or central ion; the active metal is selected from one or more of VB group metals, VIB group metals, VIII group metals and IB group metals having hydrogenation performance; the organic ligand comprises a hydrocarbon group part and a coordination group part, wherein the coordination group is a -C(=O)-O group, and forms a coordination bond with the metal central atom or central ion through an oxygen atom; in the hydrogenation catalyst, the molar ratio between the active metal and the organic ligand is 1:(0.5-3.5), and the mass ratio between the active metal and the organic treatment agent is 1:(0.1-10); the initial distillation point of the organic treatment agent is higher than the boiling point of the organic ligand.
[0009] Optionally, preferably, in the hydrogenation catalyst, the molar ratio between the active metal and the organic ligand is 1:(1.5-2.5), and the mass ratio between the active metal and the organic treatment agent is 1:(0.5-5).
[0010] Optionally, the oil-soluble catalyst has a schematic composition shown in general formula (I):
[0011] MO a [R(COO) x ] b (I)
[0012] Where M represents metal, R(COO) xrepresents an organic ligand, R represents a hydrocarbon group in the organic ligand, COO represents a coordinating group in the organic ligand, x represents the number of coordinating groups in the organic ligand, a represents the molar ratio of the non-coordinating oxygen atoms connected to the metal M to the metal M, and b represents the molar ratio of the organic ligand to the metal M, wherein: R is a C3-C19 hydrocarbon group, preferably selected from a C5-C11 normal or isomeric alkyl group, a C5-C12 cycloalkyl group and a C6-C12 aryl group; x is 1, 2 or 3, preferably 1 or 2; a is a positive number of 0-5, preferably a positive number of 1-3; wherein the infrared spectrum of the oil-soluble catalyst is 700-1000cm -1 1350-1450cm -1 and 1500-1610cm -1 There is a characteristic peak at the position.
[0013] Optionally, the VB group metal, VIB group metal, VIII group metal and IB group metal with hydrogenation performance are selected from V, Cr, Mo, W, Fe, Co, Ru, Ni, Cu and Zn, preferably selected from V, Mo, W, Fe, Co, Ni, Cu and Zn, and further preferably selected from Mo, Ni and Co; the organic ligand is derived from C4-C20 organic carboxylic acid and / or C4-C20 organic carboxylic acid anhydride, and the organic carboxylic acid is preferably selected from one or more of C4-C20 normal or isomeric alkyl carboxylic acid, C6-C20 cycloalkane carboxylic acid containing saturated carbon ring and C7-C20 aromatic carboxylic acid containing aromatic ring, preferably selected from one or more of C4-C12 normal or isomeric alkyl carboxylic acid, C6-C13 cycloalkane carboxylic acid containing saturated carbon ring and C7-C13 aromatic carboxylic acid containing aromatic ring.
[0014] Optionally, the initial distillation point of the organic treatment agent is 10-150°C higher than the boiling point of the organic ligand; the organic treatment agent is selected from one or more of alkanes with C>17, monocyclic aromatic hydrocarbons with side chains C>14, aromatic hydrocarbons with an aromatic ring number of not less than 2, dodecylbenzenesulfonic acid, oleic acid, oleylamine, stearic acid, hexadecyltrimethylammonium bromide, ethylenediaminetetraacetic acid, diesel, paraffin, ozokerite, slurry oil, residual oil, asphalt and coal tar.
[0015] The second aspect of the present invention provides a method for preparing a hydrogenation catalyst, which comprises: mixing a metal organic acid complex and an organic treatment agent to obtain a mixture; heating the mixture to remove part of the organic ligands in the metal organic acid complex and retain the organic treatment agent to obtain a residual material; the metal organic acid complex comprises an active metal central atom or central ion and an organic ligand coordinated with the active metal central atom or central ion; the active metal is selected from one or more of VB group metals, VIB group metals, VIII group metals and IB group metals with hydrogenation performance; the organic ligand comprises a hydrocarbon group part and a coordination group part, wherein the coordination group is a -C(=O)-O group, and forms a coordination bond with the metal central atom or central ion through an oxygen atom; in the metal organic acid complex, the molar ratio between the active metal and the organic ligand is 1:(1-10).
[0016] Optionally, the mass ratio between the active metal in the metal organic acid complex and the organic treatment agent is 1:(0.1-10), preferably 1:(0.5-5).
[0017] Optionally, the heating treatment is performed at a temperature of 200-450° C. and for a time of 0.5-8 h.
[0018] Optionally, the metal organic acid complex has a schematic composition shown in general formula (I):
[0019] MO a [R(COO) x ] b (I)
[0020] Where M represents metal, R(COO) x represents an organic ligand, R represents a hydrocarbon group in the organic ligand, COO represents a coordinating group in the organic ligand, x represents the number of coordinating groups in the organic ligand, a represents the molar ratio of the non-coordinating oxygen atoms connected to the metal M to the metal M, and b represents the molar ratio of the organic ligand to the metal M, wherein: R is a C3-C19 hydrocarbon group, preferably selected from a C5-C11 normal or isomeric alkyl group, a C5-C12 cycloalkyl group and a C6-C12 aryl group; x is 1, 2 or 3, preferably 1 or 2; a is a positive number of 0-5, preferably a positive number of 1-3; the infrared spectrum of the metal organic acid complex is 700-1000cm -1 1350-1450cm -1 and 1500-1610cm -1 There is a characteristic peak at the position.
[0021] Optionally, the VB group metal, VIB group metal, VIII group metal and IB group metal having hydrogenation performance are selected from V, Cr, Mo, W, Fe, Co, Ru, Ni, Cu and Zn, preferably selected from V, Mo, W, Fe, Co, Ni, Cu and Zn, and further preferably selected from Mo, Ni and Co; the organic ligand is derived from a C4-C20 organic carboxylic acid and / or an anhydride of a C4-C20 organic carboxylic acid, and the organic carboxylic acid is preferably selected from one of a C4-C20 normal or isomeric alkyl carboxylic acid, a C6-C20 cycloalkane carboxylic acid containing a saturated carbon ring and a C7-C20 aromatic carboxylic acid containing an aromatic ring. or several thereof, preferably one or more selected from normal or isomeric alkyl carboxylic acids of C4-C12, cycloalkane carboxylic acids containing saturated carbon rings of C6-C13, and aromatic carboxylic acids containing aromatic rings of C7-C13; the organic treatment agent is selected from one or more selected from alkanes with C>17, monocyclic aromatic hydrocarbons with side chains C>14, aromatic hydrocarbons with aromatic rings not less than 2, dodecylbenzenesulfonic acid, oleic acid, oleylamine, stearic acid, hexadecyltrimethylammonium bromide, ethylenediaminetetraacetic acid, diesel, paraffin, ozokerite, slurry, residual oil, asphalt and coal tar; in the metal organic acid complex, the molar ratio between the active metal and the organic ligand is 1:(1-10).
[0022] The third aspect of the present invention provides an oil hydrogenation method, which comprises: under hydrogenation reaction conditions, contacting an oil raw material with the hydrogenation catalyst described in the first aspect or the second aspect of the present invention; wherein the oil raw material is selected from at least one of benzene, alkylbenzene, naphthalene, alkylnaphthalene, anthracene, alkylanthracene, crude oil, gasoline, diesel, wax oil, slurry oil, residual oil, coal tar and biomass oil.
[0023] Optionally, the conditions of the hydrogenation reaction include: based on the weight of the oil feedstock and calculated as metal, the amount of the hydrogenation catalyst is 50-10000 μg / g, preferably 50-3000 μg / g; the initial hydrogen pressure is 1-20 MPa, preferably 3-15 MPa; the reaction temperature is 300-500°C, preferably 350-450°C; the liquid hourly space velocity is 0.05-5.0h -1 , preferably 0.05-1.0h -1 ; The volume ratio of hydrogen to oil is 100-3000, preferably 200-2000.
[0024] Through the above technical scheme, the present invention improves the hydrogenation activity of the oil-soluble catalyst. When the hydrogenation catalyst of the present invention is used for oil hydrogenation, the hydrogenation catalyst is fully dispersed in the raw material, and a higher residual oil cracking rate, a lower condensation rate and a higher distillate oil yield can be obtained.
[0025] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:
[0027] Figure 1 This is the thermogravimetric TGA diagram of the raw material molybdenum organic acid complex used in Example 1 of the present invention.
[0028] Figure 2 This is the thermogravimetric TGA diagram of the product obtained in Example 1 of the present invention.
[0029] Figure 3 It is the infrared spectrum of the product obtained in Example 1 of the present invention.
[0030] Figure 4 It is the infrared spectrum of the product obtained in Example 2 of the present invention. DETAILED DESCRIPTION
[0031] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0032] The inventors found that the existing oil-soluble catalysts have low hydrogenation activity. The possible reason is that the oil-soluble catalysts are prone to agglomeration under heating conditions and have low thermal stability. After using an organic treatment agent to replace a part of the organic ligand in the oil-soluble catalyst, the agglomeration phenomenon of the oil-soluble catalyst under heating conditions is reduced, and the thermal stability and hydrogenation activity are improved.
[0033] The first aspect of the present invention provides a hydrogenation catalyst, comprising an organic treatment agent and an oil-soluble catalyst dispersed in the organic treatment agent; wherein the oil-soluble catalyst comprises an active metal central atom or central ion and an organic ligand coordinated with the active metal central atom or central ion; the active metal is selected from one or more of VB group metals, VIB group metals, VIII group metals and IB group metals having hydrogenation performance; the organic ligand comprises a hydrocarbon group part and a coordination group part, wherein the coordination group is a -C(=O)-O group, and forms a coordination bond with the metal central atom or central ion through an oxygen atom; in the hydrogenation catalyst, the molar ratio between the active metal and the organic ligand is 1:(0.5-3.5), and the mass ratio between the active metal and the organic treatment agent is 1:(0.1-10); the initial distillation point of the organic treatment agent is higher than the boiling point of the organic ligand.
[0034] Through the above technical scheme, the oil-soluble catalyst in the hydrogenation catalyst of the present invention is dispersed in the organic treatment agent, the initial distillation point of the organic treatment agent is higher than the boiling point of the organic ligand, and the oxidation resistance of the hydrogenation catalyst is improved; at the same time, the agglomeration phenomenon of the hydrogenation catalyst of the present invention is reduced under heating conditions, thereby improving the thermal stability of the hydrogenation catalyst.
[0035] Among them, preferably, in the hydrogenation catalyst, the molar ratio between the active metal and the organic ligand is 1:(1.5-2.5), and the mass ratio between the active metal and the organic treatment agent is 1:(0.5-5).
[0036] Wherein, the oil-soluble catalyst has a schematic composition shown in general formula (I):
[0037] MO a [R(COO) x ] b (I)
[0038] Where M represents metal, R(COO) x represents an organic ligand, R represents a hydrocarbon group in the organic ligand, COO represents a coordinating group in the organic ligand, x represents the number of coordinating groups in the organic ligand, a represents the molar ratio of the non-coordinating oxygen atoms connected to the metal M to the metal M, and b represents the molar ratio of the organic ligand to the metal M, wherein: R is a C3-C19 hydrocarbon group, preferably selected from a C5-C11 normal or isomeric alkyl group, a C5-C12 cycloalkyl group and a C6-C12 aryl group; x is 1, 2 or 3, preferably 1 or 2; a is a positive number of 0-5, preferably a positive number of 1-3; wherein the infrared spectrum of the oil-soluble catalyst is 700-1000cm -1 1350-1450cm -1 and 1500-1610cm -1 There is a characteristic peak at the position.
[0039] In the present invention, "C3-C19 hydrocarbon group" refers to a hydrocarbon group having 3-19 carbon atoms, which may be a saturated or unsaturated straight chain, branched chain or carbon ring hydrocarbon group, including but not limited to C3-C19 normal alkyl, C3-C19 isomeric alkyl, C5-C19 cycloalkyl and C6-C19 aromatic group.
[0040] In the present invention, "C5-C11 normal alkyl" refers to a straight-chain alkyl group having 5 to 11 carbon atoms, such as n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, and n-undecyl.
[0041] In the present invention, "C5-C11 isomeric alkyl" refers to a branched alkyl group having 5 to 11 carbon atoms, such as isopentyl, isohexyl, isoheptyl, isooctyl, isononyl, isodecyl, and isoundecyl.
[0042] In the present invention, "C5-C12 cycloalkyl group" refers to a saturated hydrocarbon group containing a saturated carbon ring having 5-12 carbon atoms, such as cyclopentyl, cyclohexyl, methylcyclohexyl, decahydronaphthyl, methyldecahydronaphthyl, ethyldecahydronaphthyl and the like.
[0043] In the present invention, "C6-C12 aryl group" refers to a group containing an aromatic ring having 6 to 12 carbon atoms, for example, phenyl, naphthyl, anthracenyl, p-tolyl, benzyl, methylnaphthyl and the like.
[0044] According to the present invention, the C3-C19 hydrocarbon group, C5-C11 normal alkyl group, C5-C11 isomeric alkyl group, C5-C12 cycloalkyl group and C6-C12 aryl group may be optionally substituted, for example, may be unsubstituted, or may be substituted by one or more groups selected from halogen, nitro, sulfonic acid group and the like.
[0045] Wherein, the VB group metal, VIB group metal, VIII group metal and IB group metal with hydrogenation performance are selected from V, Cr, Mo, W, Fe, Co, Ru, Ni, Cu and Zn, preferably selected from V, Mo, W, Fe, Co, Ni, Cu and Zn, and further preferably selected from Mo, Ni and Co; the organic ligand is derived from C4-C20 organic carboxylic acid and / or C4-C20 organic carboxylic acid anhydride, and the organic carboxylic acid is preferably selected from one or more of C4-C20 normal or isomeric alkyl carboxylic acid, C6-C20 cycloalkane carboxylic acid containing saturated carbon ring and C7-C20 aromatic carboxylic acid containing aromatic ring, preferably selected from one or more of C4-C12 normal or isomeric alkyl carboxylic acid, C6-C13 cycloalkane carboxylic acid containing saturated carbon ring and C7-C13 aromatic carboxylic acid containing aromatic ring.
[0046] According to the present invention, C4-C20 organic carboxylic acid refers to a monocarboxylic acid having 4-20 carbon atoms, and the organic carboxylic acid may be a saturated or unsaturated straight chain, branched chain or monocarboxylic acid having a carbon ring, including but not limited to C4-C20 normal alkyl carboxylic acids, C4-C20 isomeric alkyl carboxylic acids, C6-C20 cycloalkane carboxylic acids containing saturated carbon rings, and C7-C20 aromatic carboxylic acids containing aromatic rings.
[0047] According to the present invention, the organic carboxylic acid is further preferably one or more of succinic acid, caproic acid, adipic acid, heptanoic acid, octanoic acid, nonanoic acid, ethylhexanoic acid, oleic acid, petroleum acid, salicylic acid, benzoic acid and phenylacetic acid.
[0048] In a specific embodiment of the present invention, the oil-soluble catalyst is a catalyst currently used in oil hydrogenation, which can be highly dispersed in the oil phase, such as an oil-soluble molybdenum catalyst, an oil-soluble molybdenum-cobalt catalyst, an oil-soluble molybdenum-nickel catalyst, etc. In a specific embodiment of the present invention, the oil-soluble catalyst can be an oil-soluble catalyst such as nickel cyclohexaneate, molybdenum carboxylate, acyl ketone cobalt, etc.
[0049] The initial distillation point of the organic treatment agent is 10-150°C higher than the boiling point of the organic ligand; the organic treatment agent is selected from one or more of alkanes with C>17, monocyclic aromatic hydrocarbons with side chains C>14, aromatic hydrocarbons with an aromatic ring number of not less than 2, dodecylbenzenesulfonic acid, oleic acid, oleylamine, stearic acid, hexadecyltrimethylammonium bromide, ethylenediaminetetraacetic acid, diesel, paraffin, ozokerite, slurry oil, residual oil, asphalt and coal tar.
[0050] In the present invention, when the organic treatment agent is a pure substance, the initial distillation point of the organic treatment agent is the boiling point of the organic treatment agent. When the organic treatment agent is a mixture, the initial distillation point of the organic treatment agent is the temperature recorded when the first drop of condensate falls from the end of the condenser during distillation.
[0051] According to the present invention, the alkane with C>17 refers to a normal alkane or an isoalkane having more than 17 carbon atoms.
[0052] According to the present invention, the monocyclic aromatic hydrocarbon with a side chain C>14 refers to an aromatic hydrocarbon compound containing one benzene ring and having more than 14 carbon atoms on the side chain.
[0053] According to the present invention, the aromatic hydrocarbon with an aromatic ring number of not less than 2 refers to an aromatic hydrocarbon compound containing at least 2 aromatic rings, for example, biphenyl, terphenyl, tetraphenyl, diphenylmethane, triphenylmethane, and the like.
[0054] The second aspect of the present invention provides a method for preparing a hydrogenation catalyst, which comprises: mixing a metal organic acid complex and an organic treatment agent to obtain a mixture; heating the mixture to remove part of the organic ligands in the metal organic acid complex and retain the organic treatment agent to obtain a residual material; the metal organic acid complex comprises an active metal central atom or central ion and an organic ligand coordinated with the active metal central atom or central ion; the active metal is selected from one or more of VB group metals, VIB group metals, VIII group metals and IB group metals with hydrogenation performance; the organic ligand comprises a hydrocarbon group part and a coordination group part, wherein the coordination group is a -C(=O)-O group, and forms a coordination bond with the metal central atom or central ion through an oxygen atom; in the metal organic acid complex, the molar ratio between the active metal and the organic ligand is 1:(1-10).
[0055] According to the present invention, since the initial boiling point of the organic treatment agent is higher than the boiling point of the organic ligand in the metal organic acid complex, the metal organic acid complex rich in organic ligand is heated to remove part of the organic ligand in the metal organic acid complex and retain the organic treatment agent, and the metal organic acid complex is then dispersed in the organic treatment, so it has higher thermal stability, is not only convenient for storage and transportation, but also can maintain efficient catalytic activity. The remaining material obtained by the reaction is generally solid at room temperature, and can be made liquid by heating or solvent dissolution.
[0056] The raw materials of the method for preparing the hydrogenation catalyst of the present invention are only metal organic acid complex and organic treatment agent, less raw materials are needed, the processing technology is simple, and the energy consumption is low. In addition, part of the organic ligand removed by the reaction can be recycled to prepare the metal organic acid complex, thereby reducing the cost of preparing the catalyst.
[0057] The method for preparing the hydrogenation catalyst of the present invention has no strict requirements on the reaction pressure and reaction atmosphere. For example, the reaction pressure can be normal pressure, and the reaction atmosphere can be air or an inert gas atmosphere. The method for removing part of the organic ligand of the present invention is a conventional choice in the art and is not specifically required herein. For example, it can be distillation.
[0058] Wherein, the mass ratio between the active metal in the metal organic acid complex and the organic treatment agent is 1:(0.1-10), preferably 1:(0.5-5).
[0059] The heating treatment is carried out at a temperature of 200-450°C for 0.5-8 hours. Preferably, the heating treatment is carried out at a temperature of 230-400°C for 1-5 hours.
[0060] Wherein, the metal organic acid complex has a schematic composition shown in general formula (I):
[0061] MO a [R(COO) x ] b (I)
[0062] Where M represents metal, R(COO) xrepresents an organic ligand, R represents a hydrocarbon group in the organic ligand, COO represents a coordinating group in the organic ligand, x represents the number of coordinating groups in the organic ligand, a represents the molar ratio of the non-coordinating oxygen atoms connected to the metal M to the metal M, and b represents the molar ratio of the organic ligand to the metal M, wherein: R is a C3-C19 hydrocarbon group, preferably selected from a C5-C11 normal or isomeric alkyl group, a C5-C12 cycloalkyl group and a C6-C12 aryl group; x is 1, 2 or 3, preferably 1 or 2; a is a positive number of 0-5, preferably a positive number of 1-3; wherein the infrared spectrum of the metal organic acid complex is 700-1000cm -1 1350-1450cm -1 and 1500-1610cm -1 The VB group metal, VIB group metal, VIII group metal and IB group metal having hydrogenation performance are selected from V, Cr, Mo, W, Fe, Co, Ru, Ni, Cu and Zn, preferably selected from V, Mo, W, Fe, Co, Ni, Cu and Zn, and further preferably selected from Mo, Ni and Co; the organic ligand is derived from C4-C20 organic carboxylic acid and / or C4-C20 organic carboxylic acid anhydride, and the organic carboxylic acid is preferably selected from C4-C20 normal or isomeric alkyl carboxylic acid, C6-C20 cycloalkane carboxylic acid containing saturated carbon ring and C7-C20 aromatic carboxylic acid containing aromatic ring. One or more of, preferably selected from one or more of C4-C12 normal or isomeric alkyl carboxylic acids, C6-C13 cycloalkane carboxylic acids containing saturated carbon rings and C7-C13 aromatic carboxylic acids containing aromatic rings; the organic treatment agent is selected from one or more of C>17 alkanes, monocyclic aromatic hydrocarbons with side chains C>14, aromatic hydrocarbons with aromatic rings not less than 2, dodecylbenzenesulfonic acid, oleic acid, oleylamine, stearic acid, hexadecyltrimethylammonium bromide, ethylenediaminetetraacetic acid, diesel, paraffin, ozokerite, slurry, residual oil, asphalt and coal tar; in the metal organic acid complex, the molar ratio between the active metal and the organic ligand is 1:(1-10).
[0063] In a specific embodiment of the present invention, the method for preparing a hydrogenation catalyst comprises: adding a metal organic acid complex and an organic treatment agent into a reactor to obtain a mixture, wherein the mass ratio between the active metal in the metal organic acid complex and the organic treatment agent is 1:(0.1-10). The mixture is stirred and heated to 200-450°C, kept for 0.5-8h, and the gas generated by the reaction is separated by distillation. After the reaction is completed, the residual material in the reactor is poured out to obtain the hydrogenation catalyst.
[0064] The third aspect of the present invention provides an oil hydrogenation method, which comprises: under hydrogenation reaction conditions, contacting an oil raw material with the hydrogenation catalyst described in the first aspect or the second aspect of the present invention; wherein the oil raw material is selected from at least one of benzene, alkylbenzene, naphthalene, alkylnaphthalene, anthracene, alkylanthracene, crude oil, gasoline, diesel, wax oil, slurry oil, residual oil, coal tar and biomass oil.
[0065] The conditions of the hydrogenation reaction include: based on the weight of the oil product raw material and calculated as metal, the amount of the hydrogenation catalyst is 50-10000 μg / g, preferably 50-3000 μg / g; the initial hydrogen pressure is 1-20 MPa, preferably 3-15 MPa; the reaction temperature is 300-500°C, preferably 350-450°C; the liquid hourly space velocity is 0.05-5.0 h -1 , preferably 0.05-1.0h -1 ; The volume ratio of hydrogen to oil is 100-3000, preferably 200-2000.
[0066] The present invention is further described in detail below by way of examples, but the present invention is not limited thereto.
[0067] Unless otherwise specified, the raw materials used in the examples can be obtained through commercial sources.
[0068] Examples 1-4
[0069] Examples 1-4 prepare hydrogenation catalysts C1-C4.
[0070] The raw materials, reaction conditions and test results used in Examples 1-4 are shown in Table 1. According to Table 1, the corresponding weights of the metal organic acid complex and the organic treatment agent are weighed and added to a three-necked flask, and then the reaction is carried out under the conditions shown in Table 1, and the gas generated during the reaction is separated. After the reaction is completed, the liquid product in the flask is poured out to obtain a hydrogenation catalyst. The obtained liquid product is generally solid at room temperature after cooling. The metal content and infrared spectrum of the obtained product are measured, and the composition of the obtained product is determined based on the measured results.
[0071] The preparation method of the metal organic acid complex used in Examples 1-4 includes: adding a metal-containing compound into a three-necked flask, adding an organic carboxylic acid in a molar ratio of 1 to 10 times that of the metal and mixing, reacting at 160-260° C. for 5 hours to obtain an oily metal organic acid complex.
[0072] Method for determining the metal content in the hydrogenation catalysts C1-C4 obtained in Examples 1-4 and the raw metal organic acid complexes used: After the test sample is diluted 200 times with an organic solvent, it is determined using a SPECTRO ARCOS SOP plasma emission spectrometer using inductively coupled plasma optical emission spectrometry (ICP-OES). The measurement conditions are a closed optical chamber filled with argon, vertical observation, and a wavelength range of 130-770nm.
[0073] Infrared spectra of the hydrogenation catalysts C1-C4 obtained in Example 1-4 were measured by using a NICOLET IS50 spectrometer from Thermo Fisher Scientific, Inc., under the following conditions: the infrared spectra of the solid catalyst products were measured at a scanning wavelength of 400-4000 cm -1 The number of scans is 16. ZnSe crystal and HgCdTe infrared detector are used together to measure the attenuated total reflectance (ATR) of the sample with a resolution of 4cm -1 .
[0074] Thermal analysis of the raw metal organic acid complexes used in Examples 1-4 and the hydrogenation catalysts C1-C4 obtained in Examples 1-4: The solid catalyst products obtained were measured using a STA 499C thermal analyzer (NETZSCH, Germany) under a N2 atmosphere with a test range of 50-600°C and a heating rate of 10°C / min.
[0075] Table 1
[0076]
[0077] Figure 1 This is the thermogravimetric analysis diagram of the hydrogenation catalyst C1 obtained in Example 1. Figure 2 This is the thermogravimetric analysis diagram of the raw material metal organic acid complex used in Example 1. Figure 1 and Figure 2 It can be seen that the metal organic acid complex will experience severe weight loss at 160°C and more than 60% at 200°C, while the weight loss of hydrogenation catalyst C1 is less than 20% at 300°C. This shows that the thermal stability of the metal organic acid complex will be greatly improved after being treated with an organic treatment agent, which has a favorable effect on the storage stability and in-situ activation of the hydrogenation catalyst.
[0078] Figure 3 is the infrared spectrum of the hydrogenation catalyst C1 obtained in Example 1, Figure 4 This is the infrared spectrum of the hydrogenation catalyst C2 obtained in Example 2. Figure 3 and Figure 4 It can be seen that the infrared spectra of hydrogenation catalysts C1 and C2 have a peak at 1350 cm -1 -1450cm-1 With 1500cm -1 -1610cm -1 There are obvious characteristic peaks, indicating that the binding mode between metal and organic ligand does not change after the metal organic acid complex is treated with organic treatment agent.
[0079] Embodiment 5-8
[0080] Raw material A is vacuum residue oil, which has an asphaltene content of 12.7%, a carbon residue value of 19.8%, and a heavy metal (Ni+V) content of 371 μg / g.
[0081] A was used as raw material and mixed with hydrogenation catalysts C1-C4 in an intermittent high-pressure reactor, and contacted with hydrogen under hydrogenation conditions to conduct a residual oil catalytic hydrogenation thermal conversion test, and the reaction products were analyzed and tested. The hydrogenation reaction conditions and experimental results are shown in Table 2.
[0082] Comparative Example 1
[0083] Comparative Example 1 was tested with reference to Example 5, except that the catalyst used in Comparative Example 1 was the raw material oil-soluble molybdenum organic acid complex used in Example 1, and other test conditions were the same. The experimental results are shown in Table 2.
[0084] Comparative Example 2
[0085] Comparative Example 2 was tested with reference to Example 6, except that the catalyst used in Comparative Example 2 was the raw material oil-soluble molybdenum-nickel organic acid complex used in Example 2, and other test conditions were the same. The experimental results are shown in Table 2.
[0086] Table 2
[0087]
[0088] By comparing the data of Examples 5-8 and Comparative Examples 1-2 in Table 2, it can be seen that the hydrogenation catalyst obtained after the metal organic acid complex is treated with an organic treatment agent has a higher hydrogenation activity, and when applied to oil hydrogenation, a higher residue oil cracking rate, a lower condensation rate and a higher distillate oil yield can be obtained.
[0089] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0090] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0091] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A hydrogenation catalyst, characterized in that It includes an organic treatment agent and an oil-soluble catalyst dispersed in the organic treatment agent; The oil-soluble catalyst comprises an active metal central atom or central ion and an organic ligand coordinated with the active metal central atom or central ion; the active metal is selected from one or more of VB group metals, VIB group metals, VIII group metals and IB group metals having hydrogenation performance; the organic ligand comprises a hydrocarbon group part and a coordination group part, wherein the coordination group is a -C(=O)-O group, and forms a coordination bond with the metal central atom or central ion through an oxygen atom; in the hydrogenation catalyst, the molar ratio between the active metal and the organic ligand is 1:(0.5-3.5), and the mass ratio between the active metal and the organic treatment agent is 1:(0.1-10); The initial boiling point of the organic treatment agent is higher than the boiling point of the organic ligand.
2. The hydrogenation catalyst according to claim 1, wherein Preferably, in the hydrogenation catalyst, the molar ratio between the active metal and the organic ligand is 1:(1.5-2.5), and the mass ratio between the active metal and the organic treatment agent is 1:(0.5-5).
3. The hydrogenation catalyst according to claim 1 or 2, wherein The oil-soluble catalyst has a schematic composition shown in general formula (I): MO a [R(COO) x ] b (I), Where M represents metal, R(COO) x represents the organic ligand, R represents the hydrocarbon group in the organic ligand, COO represents the coordination group in the organic ligand, x represents the number of coordination groups in the organic ligand, a represents the molar ratio of the non-coordinating oxygen atoms connected to the metal M to the metal M, and b represents the molar ratio of the organic ligand to the metal M, wherein: R is a C3-C19 hydrocarbon group, preferably selected from a C5-C11 normal or isomeric alkyl group, a C5-C12 cycloalkyl group and a C6-C12 aryl group; x is 1, 2 or 3, preferably 1 or 2; a is a positive number between 0 and 5, preferably a positive number between 1 and 3; The infrared spectrum of the oil-soluble catalyst is between 700 and 1000 cm -1 1350-1450cm -1 and 1500-1610cm -1 The VB group metal, VIB group metal, VIII group metal and IB group metal having hydrogenation performance are selected from V, Cr, Mo, W, Fe, Co, Ru, Ni, Cu and Zn, preferably selected from V, Mo, W, Fe, Co, Ni, Cu and Zn, and further preferably selected from Mo, Ni and Co; The organic ligand is derived from a C4-C20 organic carboxylic acid and / or an anhydride of a C4-C20 organic carboxylic acid, and the organic carboxylic acid is preferably selected from one or more of a C4-C20 normal or isomeric alkyl carboxylic acid, a C6-C20 cycloalkane carboxylic acid containing a saturated carbon ring, and a C7-C20 aromatic carboxylic acid containing an aromatic ring, and is preferably selected from one or more of a C4-C12 normal or isomeric alkyl carboxylic acid, a C6-C13 cycloalkane carboxylic acid containing a saturated carbon ring, and a C7-C13 aromatic carboxylic acid containing an aromatic ring.
4. The hydrogenation catalyst according to claim 1 or 2, wherein The initial boiling point of the organic treatment agent is 10-150°C higher than the boiling point of the organic ligand; The organic treatment agent is selected from one or more of alkanes with C>17, monocyclic aromatic hydrocarbons with side chains with C>14, aromatic hydrocarbons with an aromatic ring number of not less than 2, dodecylbenzenesulfonic acid, oleic acid, oleylamine, stearic acid, hexadecyltrimethylammonium bromide, ethylenediaminetetraacetic acid, diesel, paraffin, ozokerite, slurry oil, residual oil, asphalt and coal tar.
5. A method for preparing a hydrogenation catalyst, characterized in that: The method comprises: mixing a metal organic acid complex and an organic treatment agent to obtain a mixture; heating the mixture to remove part of the organic ligands in the metal organic acid complex and retain the organic treatment agent to obtain a residual material; The metal organic acid complex comprises an active metal central atom or central ion and an organic ligand coordinated with the active metal central atom or central ion; the active metal is selected from one or more of VB group metals, VIB group metals, VIII group metals and IB group metals having hydrogenation performance; the organic ligand comprises a hydrocarbon group part and a coordination group part, wherein the coordination group is a -C(=O)-O group, and forms a coordination bond with the metal central atom or central ion through an oxygen atom; In the metal organic acid complex, the molar ratio between the active metal and the organic ligand is 1:(1-10).
6. The method according to claim 5, wherein: The mass ratio between the active metal in the metal organic acid complex and the organic treatment agent is 1:(0.1-10), preferably 1:(0.5-5).
7. The method according to claim 5, wherein: The heating treatment is carried out at a temperature of 200-450° C. and for a time of 0.5-8 h.
8. The method according to claim 5, wherein: The metal organic acid complex has a schematic composition shown in general formula (I): MO a [R(COO) x ] b (I), Where M represents metal, R(COO) x represents the organic ligand, R represents the hydrocarbon group in the organic ligand, COO represents the coordination group in the organic ligand, x represents the number of coordination groups in the organic ligand, a represents the molar ratio of the non-coordinating oxygen atoms connected to the metal M to the metal M, and b represents the molar ratio of the organic ligand to the metal M, wherein: R is a C3-C19 hydrocarbon group, preferably selected from a C5-C11 normal or isomeric alkyl group, a C5-C12 cycloalkyl group and a C6-C12 aryl group; x is 1, 2 or 3, preferably 1 or 2; a is a positive number between 0 and 5, preferably a positive number between 1 and 3; The infrared spectrum of the metal organic acid complex is between 700-1000 cm -1 1350-1450cm -1 and 1500-1610cm -1 The VB group metal, VIB group metal, VIII group metal and IB group metal having hydrogenation performance are selected from V, Cr, Mo, W, Fe, Co, Ru, Ni, Cu and Zn, preferably selected from V, Mo, W, Fe, Co, Ni, Cu and Zn, and further preferably selected from Mo, Ni and Co; The organic ligand is derived from a C4-C20 organic carboxylic acid and / or an anhydride of a C4-C20 organic carboxylic acid, wherein the organic carboxylic acid is preferably selected from one or more of a C4-C20 normal or isomeric alkyl carboxylic acid, a C6-C20 cycloalkane carboxylic acid containing a saturated carbocyclic ring, and a C7-C20 aromatic carboxylic acid containing an aromatic ring, and preferably selected from one or more of a C4-C12 normal or isomeric alkyl carboxylic acid, a C6-C13 cycloalkane carboxylic acid containing a saturated carbocyclic ring, and a C7-C13 aromatic carboxylic acid containing an aromatic ring; The organic treatment agent is selected from one or more of alkanes with C>17, monocyclic aromatic hydrocarbons with side chains with C>14, aromatic hydrocarbons with an aromatic ring number of not less than 2, dodecylbenzenesulfonic acid, oleic acid, oleylamine, stearic acid, hexadecyltrimethylammonium bromide, ethylenediaminetetraacetic acid, diesel, paraffin, ozokerite, slurry oil, residual oil, asphalt and coal tar; In the metal organic acid complex, the molar ratio between the active metal and the organic ligand is 1:(1-10).
9. A method for hydrogenating oil, characterized in that: The method includes: Under hydrogenation reaction conditions, contacting the oil product raw material with the hydrogenation catalyst according to any one of claims 1 to 4; The oil raw material is selected from at least one of benzene, alkylbenzene, naphthalene, alkylnaphthalene, anthracene, alkylanthracene, crude oil, gasoline, diesel, wax oil, slurry oil, residual oil, coal tar and biomass oil.
10. The method according to claim 9, wherein: The conditions of the hydrogenation reaction include: Based on the weight of the oil raw material and calculated as metal, the amount of the hydrogenation catalyst is 50-10000 μg / g, preferably 50-3000 μg / g; the initial hydrogen pressure is 1-20 MPa, preferably 3-15 MPa; the reaction temperature is 300-500°C, preferably 350-450°C; the liquid hourly space velocity is 0.05-5.0 h -1 , preferably 0.05-1.0h -1 ; The volume ratio of hydrogen to oil is 100-3000, preferably 200-2000.
Citation Information
Patent Citations
Preparation method of an oil-soluble catalyst
CN110240930A
A method for preparing a hydrogenation catalyst, the hydrogenation catalyst and its application
CN112742478B
Preparation method of organic acid molybdenum oil-soluble catalyst for slurry reactor hydrogenation
CN114870902A
Multi-tooth bionic ligand for improving biocompatibility and stability of nano particles as well as preparation method of multi-tooth bionic ligand
CN104672462A
Non-supported bimetallic hydrogenation catalyst, and composition and application thereof
CN116020565A