Preparation method of high-uniformity medium carbon steel large round billet
By using tundra induction heating and electromagnetic cyclone water port combined with stirring technology during continuous casting of medium carbon steel, the problem of uniformity control of large-scale round blanks is solved, and the extreme difference control of carbon, manganese and chromium elements in wind power bearings is achieved and the good condition of low-power tissue improves the performance stability of the product.
Patent Information
- Application Number
- CN202411182999.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to effectively control the uniformity of large round billets of carbon steel in large specifications, resulting in inconsistent performance of wind power bearings and prone to fatigue life problems.
The stirring method is adopted that combines tundish induction heating, electromagnetic cyclone outlet and crystallizer electromagnetic stirring, combined with end electromagnetic stirring, controls the temperature and pulling speed during continuous casting of medium carbon steel to ensure the macroscopic uniformity and low-speed of casting billets organize.
The good macroscopic uniformity and low-magnitude structure of large-scale medium-carbon steel large round billets are achieved, ensuring stable hardenability of the products after forging. The hardenability bandwidth of the same batch is ≤3HRC, meeting the requirements of high uniformity.
Smart Images

Figure BDA0005012745450000031 
Figure BDA0005012745450000041 
Figure BDA0005012745450000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a method for preparing a large round billet of medium carbon steel with high uniformity. Background Art
[0002] Facing the national "dual carbon" strategy, wind power equipment is developing rapidly towards higher power, which also puts forward higher technical requirements for large-scale, long life, high reliability, intelligence and efficient operation of different types and series of rolling bearings in high-power wind power equipment. Wind power bearings are the core components of wind turbines, mainly including large and heavy-duty bearings such as yaw bearings, pitch bearings, and main shaft bearings. The uniformity and cleanliness of their steel determine the service life of the bearings, which seriously affects the normal operation of wind turbines.
[0003] During the continuous casting solidification process, due to the existence of temperature gradient in the solidification direction of the ingot, three solidification structures are usually formed: edge fine equiaxed crystal area, columnar crystal area and central equiaxed crystal area. Due to the influence of selective crystallization, component segregation and inclusion aggregation are prone to occur at the junction of the columnar crystal area and the central equiaxed crystal area, forming a segregation zone.
[0004] The uniformity of the entire cross-section of medium-carbon steel round billets used to produce wind turbine bearings has a significant impact on the performance of the bearings. Severe segregation can easily lead to inconsistent bearing performance and fatigue life at weak points that cannot meet requirements. However, there are few patents and papers reporting on the control technology for uniformity of large-size round billets. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a method for preparing a medium carbon steel round billet with high uniformity, wherein the main element composition range of the Φ500mm medium carbon steel round billet prepared by the method is ≤0.035%, the hardenability bandwidth of the same batch is ≤3HRC, and has good macrostructure.
[0006] The present invention provides a method for preparing a large round billet of medium carbon steel with high uniformity, comprising the following steps:
[0007] The medium carbon steel is continuously cast and induction heated in the tundish; electromagnetic swirl water inlet is used, and a stirring method combining electromagnetic stirring of the crystallizer and electromagnetic stirring of the end is used to obtain the ingot;
[0008] After the ingot is rolled off the production line, it is slowly cooled in a pit to obtain a round ingot of Φ500 mm;
[0009] The medium carbon steel comprises the following components by mass fraction:
[0010] C0.39~0.44%, Mn0.65~0.80%, Cr1.00~1.20%.
[0011] The temperature of the continuous casting steel in the present invention is 1520-1535°C;
[0012] The temperature of the intermediate package is 1510±2℃.
[0013] The current used in the electromagnetic vortex in the present invention is 300-400A, which is opposite to the stirring direction of the crystallizer;
[0014] The continuous casting speed is 0.33~0.37m / min.
[0015] The current used for electromagnetic stirring of the crystallizer is 100-200A and the frequency is 1.0-1.5HZ;
[0016] The current used for the terminal electromagnetic stirring is 150-300A and the frequency is 4.0-6.0HZ.
[0017] The medium carbon steel described in the present invention also includes: Si0.17-0.35%, Mo0.20-0.25%, Al0.015-0.040%, P≤0.015%, S≤0.015%, Ti≤0.005%, Ca≤0.0015%, As+Sn+Pb+Sb+Bi≤0.035%, [O]≤20ppm, [H]≤2ppm, [N]≤70ppm, and the rest is Fe and unavoidable impurities.
[0018] In the present invention, for a Φ500 mm round billet, the specific water content is 0.10 to 0.12 L / kg.
[0019] The invention reasonably designs the continuous casting process of the large-size continuous casting round billet, and the content difference of C, Mn and Cr elements in the full cross section of the round billet is ≤0.035%, thereby obtaining good macroscopic uniformity.
[0020] The invention provides a method for preparing a large round billet of medium carbon steel with high uniformity, comprising the following steps: continuously casting medium carbon steel, heating by induction in a tundish; adopting an electromagnetic swirl water inlet, adopting a stirring method combining electromagnetic stirring of a crystallizer and electromagnetic stirring at the end to obtain a billet; after the billet is off the production line, it is slowly cooled in a pit to obtain a round billet of Φ500mm; in terms of mass fraction, the medium carbon steel comprises the following components: C0.39-0.44%, Mn0.65-0.80%, Cr1.00-1.20%. The large-scale continuous casting round billet prepared by the method has a carbon, manganese and chromium element content range of ≤0.035% in the whole cross section, and a hardenability bandwidth of ≤3HRC in the same batch, achieving good macroscopic uniformity; the round billet has a uniform as-cast structure, a central looseness of ≤1.0 level, and no low-magnification structural defects such as shrinkage cavities and cracks. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a low-magnification structure diagram of a Φ500 mm round billet prepared in an embodiment of the present invention;
[0022] Figure 2 This is a low-magnification microstructure diagram of a Φ500mm round billet prepared as a comparative example. DETAILED DESCRIPTION
[0023] In order to further illustrate the present invention, a method for preparing a large round billet of medium carbon steel with high uniformity provided by the present invention is described in detail below in combination with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0024] Example 1
[0025] The chemical composition by mass percentage is: C: 0.42%, Si: 0.22%, Mn: 0.74%, Cr: 1.13%, P: 0.012%, S: 0.003%, Mo: 0.22%, Ti: 0.003%, Ca: 0.0008%, Al: 0.027%, As+Sn+Pb+Sb+Bi: 0.008%, [O]: 9.2ppm, [H]: 1.3ppm, [N]: 56ppm, and the rest is Fe and unavoidable impurities. The upper steel temperature is 1532℃, the continuous casting adopts induction heating of the tundish, and the tundish temperature is 1510℃; the electromagnetic swirl water nozzle is adopted, the current is 350A, and the stirring direction is opposite to the crystallizer; the continuous casting speed is 0.34m / min, and the specific water volume is 0.11L / kg; the crystallizer electromagnetic stirring current is 150A, and the frequency is 1.2HZ; the end electromagnetic stirring current is 200A, and the frequency is 5.0HZ; the billet is slowly cooled in the pit after it comes off the line. The extreme difference of the content of the main components in the whole cross section, the level of low-multiple organization, the hardenability of different branches after forging, and the hardenability bandwidth of the same batch are shown in Table 1.
[0026] Table 1
[0027]
[0028] Embodiment 2:
[0029] The chemical composition by mass percentage is: C: 0.43%, Si: 0.25%, Mn: 0.76%, Cr: 1.12%, P: 0.010%, S: 0.002%, Mo: 0.23%, Ti: 0.0025%, Ca: 0.0009%, Al: 0.029%, As+Sn+Pb+Sb+Bi: 0.009%, [O]: 8.5ppm, [H]: 1.1ppm, [N]: 49.5ppm, and the rest is Fe and unavoidable impurities. The upper steel temperature is 1523℃, the continuous casting adopts induction heating of the tundish, and the tundish temperature is 1509℃; the electromagnetic swirl water nozzle is adopted, the current is 400A, and the stirring direction is opposite to the crystallizer; the continuous casting speed is 0.35m / min, the specific water volume is 0.11L / kg; the crystallizer electromagnetic stirring current is 150A, the frequency is 1.0HZ; the end electromagnetic stirring current is 250A, the frequency is 4.5HZ; the billet is slowly cooled in the pit after it comes off the line. The extreme difference of the content of the main components in the full cross section and the low-magnification structure level are shown in Table 2.
[0030] Table 2
[0031]
[0032] Embodiment 3:
[0033] The chemical composition mass percentage is: C: 0.42%, Si: 0.23%, Mn: 0.77%, Cr: 1.15%, P: 0.010%, S: 0.002%, Mo: 0.224%, Ti: 0.0028%, Ca: 0.0010%, Al: 0.032%, As+Sn+Pb+Sb+Bi: 0.011%, [O]: 10.3ppm, [H]: 1.1ppm, [N]: 58.2ppm, and the rest is Fe and unavoidable impurities. The upper steel temperature is 1530℃, the continuous casting adopts induction heating of the tundish, and the tundish temperature is 1511℃; the electromagnetic swirl water nozzle is adopted, the current is 300A, and the stirring direction is opposite to the crystallizer; the continuous casting speed is 0.36m / min, the specific water volume is 0.10L / kg; the crystallizer electromagnetic stirring current is 200A, the frequency is 1.0HZ; the end electromagnetic stirring current is 300A, the frequency is 4.0HZ; the billet is slowly cooled in the pit after it comes off the line. The extreme difference of the content of the main components in the full cross section and the low-magnification structure level are shown in Table 3.
[0034] Table 3
[0035]
[0036] It can be seen from the above embodiments that the medium carbon steel large-size round billet produced by the present invention has good macrostructure, the center looseness of the largest size is ≤1.0 level, and there are no other macrostructure defects; and the extreme differences in the contents of the main elements C, Mn, and Cr are all ≤0.035%, the hardenability of the forged product is stably controlled, and the hardenability bandwidth of the same batch is ≤3HRC, which well meets the uniformity requirements of the product.
[0037] Comparative Example
[0038] The chemical composition by mass percentage is: C: 0.40%, Si: 0.25%, Mn: 0.78%, Cr: 1.15%, P: 0.013%, S: 0.002%, Mo: 0.20%, Ti: 0.001%, Ca: 0.0008%, Al: 0.033%, As+Sn+Pb+Sb+Bi: 0.009%, [O]: 10.1ppm, [H]: 1.5ppm, [N]: 47ppm, and the rest is Fe and unavoidable impurities. The steel temperature is 1545℃, the tundish induction heating is not used in the continuous casting process, and the tundish temperature is 1523℃; the electromagnetic swirl water nozzle is used, the current is 450A, and the stirring direction is opposite to the crystallizer; the continuous casting speed is 0.42m / min, the specific water volume is 0.15L / kg; the crystallizer electromagnetic stirring current is 220A, the frequency is 2HZ; the end electromagnetic stirring current is 200A, the frequency is 7.0HZ; the billet is slowly cooled in the pit after it comes off the line. The extreme difference of the content of the main components in the full cross section and the low-magnification structure level are shown in Table 1.
[0039] Table 1
[0040]
[0041] It can be seen from the comparative examples that the composition range of the comparative examples is large, shrinkage defects appear in the low-magnification structure, the hardenability of the forged products fluctuates greatly, and the hardenability bandwidth of the same batch is about 5HRC, which can easily cause risks such as product deformation.
[0042] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a large round billet of medium carbon steel with high uniformity, comprising the following steps: The medium carbon steel is continuously cast and induction heated in the tundish; electromagnetic swirl water inlet is used, and a stirring method combining electromagnetic stirring of the crystallizer and electromagnetic stirring of the end is used to obtain the ingot; After the ingot is rolled off the production line, it is slowly cooled in a pit to obtain a round ingot of Φ500 mm; The medium carbon steel comprises the following components by mass fraction: C0.39~0.44%, Mn0.65~0.80%, Cr1.00~1.20%.
2. The preparation method according to claim 1, characterized in that: The temperature of the continuous casting steel is 1520-1535°C; The temperature of the intermediate package is 1510±2℃.
3. The preparation method according to claim 1, characterized in that: The current used in electromagnetic swirl is 300-400A; The continuous casting speed is 0.33~0.37m / min.
4. The preparation method according to claim 1, wherein the current used for electromagnetic stirring of the crystallizer is 100-200A and the frequency is 1.0-1.5HZ; The current used for the end electromagnetic stirring is 150-300A and the frequency is 4.0-6.0HZ.
5. The preparation method according to claim 1, characterized in that: The medium carbon steel also includes: Si0.17-0.35%, Mo0.20-0.25%, Al0.015-0.040%, P≤0.015%, S≤0.015%, Ti≤0.005%, Ca≤0.0015%, As+Sn+Pb+Sb+Bi≤0.035%, [O]≤20ppm, [H]≤2ppm, [N]≤70ppm, and the rest is Fe.
6. The preparation method according to claim 1, characterized in that: The water content of Φ500mm round billet is 0.10~0.12L / kg.
7. The preparation method according to claim 1, characterized in that: The maximum content of C, Mn and Cr elements is ≤0.035%.