Modified bismaleimide resin composition, preparation method thereof and prepreg
By adding specific compounds to the bismaleimide resin to adjust the crosslinking density and viscosity, the problems of poor toughness and insufficient processability of bismaleimide resin are solved, and the heat resistance and process of the modified resin are realized The performance improvement has expanded its application in advanced structural composite materials.
Patent Information
- Application Number
- CN202411282088.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-03
AI Technical Summary
The crosslinking density of bismaleimide resins leads to poor toughness and poor processability, making it difficult to meet the requirements of advanced structural composite materials for resin matrix.
The modified bismaleimide resin composition is prepared by adding allyl compounds, phenol compounds, epoxy modifiers and thermoplastic toughening resins to the bismaleimide resin to adjust the crosslinking density and viscosity to prepare the modified bismaleimide resin composition. , improve toughness and process performance.
The heat resistance, toughness and process performance of the modified resin have been improved, and the application needs of advanced structural composite materials are met.
Smart Images

Figure CN119060536A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of composite material matrix resin synthesis, and in particular to a modified bismaleimide resin composition, a preparation method thereof, and a prepreg. Background Art
[0002] Bismaleimide resin (Bismaleimide, BMI) is a kind of resin system derived from polyimide resin system, which has similar fluidity and moldability as thermosetting resin. BMI resin has been widely used because of its advantages such as low moisture absorption, small thermal expansion coefficient, high temperature resistance and radiation resistance.
[0003] However, due to the high cross-linking density and high molecular chain rigidity of BMI resin, its toughness is poor and cannot meet the toughness requirements of advanced structural composite materials for the resin matrix. At the same time, the processability of BMI resin is relatively poor, and the laying and adhesion of the prepreg composited with carbon fiber at room temperature are difficult to match the epoxy system prepreg, which limits the application of BMI resin in advanced structural composite materials. Summary of the invention
[0004] In order to solve the above technical problems, the present application aims to provide a modified bismaleimide resin composition and a preparation method and a prepreg thereof, wherein the modified bismaleimide resin composition has excellent heat resistance, toughness and process performance.
[0005] According to the first aspect of the present application, a modified bismaleimide resin composition is provided, comprising the following raw materials in parts by weight:
[0006] 20-40 parts by weight of allyl compound;
[0007] 0.2-2.5 parts by weight of phenolic compound;
[0008] 30-65 parts by weight of bismaleimide monomer;
[0009] Epoxy modifier 10-20 parts by weight;
[0010] 5-20 parts by weight of thermoplastic toughening resin.
[0011] In some embodiments of the present application, the weight ratio of the bismaleimide monomer, the allyl compound, and the phenolic compound is 75-116:45-55:1.
[0012] In some embodiments of the present application, the weight ratio of the epoxy modifier to the phenolic compound is 20.0-26.0:1.
[0013] In some embodiments of the present application, the weight ratio of the sum of the weight of the allyl compound, the phenolic compound, the bismaleimide monomer, and the epoxy modifier to the thermoplastic toughening resin is 4.0-19.1:1.
[0014] In some embodiments of the present application, the allyl compound includes a combination of one or more of diallyl bisphenol A, diallyl bisphenol S, bisphenol A bisallyl ether, and diallyl phenol;
[0015] The phenolic compound includes a combination of one or more of phenol, bisphenol A, and allyl phenol;
[0016] The bismaleimide monomer includes a combination of one or more of diphenylmethane bismaleimide and toluenediamine bismaleimide;
[0017] The epoxy modifier includes a combination of one or more of triglycidyl p-aminophenol, resorcinol diglycidyl ether, bisphenol A diglycidyl ether, and tetraglycidyl 4,4-diaminodiphenylmethane;
[0018] The thermoplastic resin includes one or more of polyethersulfone, polyetheretherketone, polyimide, polyaryletherketone, polyphenylene ether, and polyetherimide.
[0019] In some embodiments of the present application, when the bismaleimide monomer includes diphenylmethane bismaleimide and toluenediamine bismaleimide, the weight ratio of the diphenylmethane bismaleimide to the toluenediamine bismaleimide is 1.05-1.80:1.
[0020] In some embodiments of the present application, the raw materials of the composition further include a catalyst, and the amount of the catalyst is 0.1-0.5% of the total weight of the composition.
[0021] In some embodiments of the present application, the catalyst includes triphenylphosphine.
[0022] According to a second aspect of the present application, a method for preparing a modified bismaleimide resin composition is provided. The method for preparing the modified bismaleimide resin composition is used to prepare the modified bismaleimide resin composition as described above. The preparation method comprises:
[0023] mixing the allyl compound and the phenolic compound under a first preset condition to obtain a first premix;
[0024] Mixing the first premix with the thermoplastic toughening resin under second preset conditions to obtain a second premix;
[0025] Mixing the second premix with the bismaleimide monomer under third preset conditions to obtain a third premix;
[0026] The third premix is mixed with the epoxy modifier under fourth preset conditions to obtain the modified bismaleimide resin composition.
[0027] According to a third aspect of the present application, a prepreg is provided, comprising reinforcing fibers and the modified bismaleimide resin as described above or a modified bismaleimide resin prepared by the method for preparing the modified bismaleimide resin as described above.
[0028] The technical solution provided by this application may have the following beneficial effects:
[0029] The present application uses an allyl compound to toughen and modify the bismaleimide resin. The addition of an epoxy modifier can reduce the crosslinking density of the bismaleimide resin, improve the brittleness of the cured resin composition, and improve the toughness of the resin composition by combining with a thermoplastic toughening resin. The combination of an epoxy modifier and a phenolic compound can reduce the viscosity of the synthesized bismaleimide resin, increase the viscosity of the resin composition, and improve the processability of the resin composition.
[0030] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0032] Figure 1 The present invention is a flow chart of a method for preparing a modified bismaleimide resin composition according to an exemplary embodiment. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme of the present application will be clearly and completely described below in combination with the embodiments of the present application and the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be arbitrarily combined with each other.
[0034] In order to solve the problem of poor toughness of BMI resin, in the related technology, thermoplastic toughening resin is added to modify it to improve its toughness, which can improve the fracture toughness of the modified resin without sacrificing the bending properties of the modified resin; however, the addition of thermoplastic resin has a certain upper limit, otherwise it will greatly affect the process performance of BMI resin.
[0035] Based on this, the present application provides a modified bismaleimide resin composition, including the following raw materials in parts by weight: 20-50 parts by weight of allyl compound; 0.2-5 parts by weight of phenolic compound; 30-80 parts by weight of bismaleimide monomer; 8-20 parts by weight of epoxy modifier; 6-20 parts by weight of thermoplastic toughening resin. The present application toughens and modifies the bismaleimide resin by using an allyl compound. The addition of epoxy modifier can reduce the crosslinking density of the bismaleimide resin, improve the brittleness of the cured resin composition, and improve the toughness of the resin composition by combining with thermoplastic toughening resin; the combination of epoxy modifier and phenolic compound can reduce the viscosity of the synthesized bismaleimide resin, improve the viscosity of the resin composition, and improve the processability of the resin composition.
[0036] Some specific implementation modes described below are intended to facilitate those skilled in the art to understand the present embodiment, and the present embodiment is not limited to some specific implementation modes described below.
[0037] In an exemplary embodiment, the present application provides a modified bismaleimide resin composition, comprising the following raw materials in parts by weight:
[0038]
[0039] In this embodiment, the bismaleimide resin is toughened and modified by means of an allyl compound. The crosslinking density of the bismaleimide resin can be reduced by adding an epoxy modifier, thereby improving the brittleness of the cured resin composition. Furthermore, the toughness of the resin composition can be improved by combining with a thermoplastic toughening resin. The viscosity of the synthesized bismaleimide resin can be reduced by combining with an epoxy modifier and a phenolic compound, thereby improving the processability of the resin composition.
[0040] Exemplarily, in one embodiment, the modified bismaleimide resin composition includes the following raw materials in parts by weight:
[0041]
[0042] In another embodiment, the modified bismaleimide resin composition comprises the following raw materials in parts by weight:
[0043]
[0044] In another embodiment, the modified bismaleimide resin composition comprises the following raw materials in parts by weight:
[0045]
[0046] 20 parts by weight of thermoplastic toughening resin.
[0047] In an exemplary embodiment, the weight ratio of the bismaleimide monomer, the allyl compound, and the phenolic compound is 86-116:45-55:1.
[0048] In this embodiment, the allyl compound can be introduced into the molecular chain of the bismaleimide resin to adjust the crosslinking density of the bismaleimide resin and improve the toughness of the bismaleimide resin; however, the softening point of the bismaleimide resin modified by the allyl compound is high, which makes its paving property at room temperature poor; therefore, by introducing a phenolic compound, the viscosity of the bismaleimide resin modified by the allyl compound can be improved, its fluidity can be improved, and the process performance can be improved. By controlling the weight ratio of the bismaleimide monomer, the allyl compound, and the phenolic compound to 86-116:45-55:1, the toughness and process performance of the bismaleimide resin can be improved at the same time. Exemplarily, the bismaleimide monomer, the allyl compound, and the phenolic compound are 86:45:1, 100:50:1, or 116:55:1.
[0049] In an exemplary embodiment, the weight ratio of the epoxy modifier to the phenolic compound is 22.0-24.0:1.
[0050] In this embodiment, the addition of the phenolic compound can reduce the viscosity of the resin composition system to improve the processability of the resin composition; wherein the hydroxyl group contained in the phenolic compound opens the epoxy group in the epoxy modifier to generate an ether bond and form a three-dimensional network structure, thereby improving the processability of the resin composition while improving the thermal stability and toughness of the resin composition. Exemplarily, the weight ratio of the epoxy modifier to the phenolic compound is 20.0:1, 22.0:1 or 24.0:1.
[0051] In an exemplary embodiment, the weight ratio of the sum of the weight of the allyl compound, the phenolic compound, the bismaleimide monomer, and the epoxy modifier to the thermoplastic toughening resin is 4.0-19.1:1.
[0052] In this embodiment, the addition of thermoplastic toughening resin can play a role in toughening and modifying the modified bismaleimide resin; by controlling the weight ratio of the sum of the weight of the allyl compound, the phenolic compound, the bismaleimide monomer, and the epoxy modifier to the thermoplastic toughening resin to 4.0-19.1:1, the modified bismaleimide resin composition prepared thereby can have the advantages of heat resistance, toughness, and processability. Exemplarily, the weight ratio of the sum of the weight of the allyl compound, the phenolic compound, the bismaleimide monomer, and the epoxy modifier to the thermoplastic toughening resin is 4.0:1, 5.7:1, 7.5:1, or 19.1:1.
[0053] In an exemplary embodiment, the allyl compound includes a combination of one or more of diallyl bisphenol A, diallyl bisphenol S, bisphenol A bisallyl ether, and diallyl phenol.
[0054] In this embodiment, diallyl bisphenol A, diallyl bisphenol S, bisphenol A diallyl ether, and diallyl phenol contain two allyl groups, which can provide more reaction sites, so that they can be introduced into the molecular chain of the bismaleimide resin, adjust the crosslinking density of the bismaleimide resin, and improve the toughness of the bismaleimide resin.
[0055] In an exemplary embodiment, the phenolic compound includes a combination of one or more of phenol, bisphenol A, and allylphenol.
[0056] In this embodiment, the phenolic compound can be phenol, bisphenol A, allyl phenol, etc. For example, the epoxy group in the epoxy modifier is opened by the hydroxyl group of phenol to generate an ether bond and form a three-dimensional network structure, thereby improving the processability of the resin composition while improving the thermal stability and toughness of the resin composition.
[0057] In an exemplary embodiment, the bismaleimide monomer includes a combination of one or more of diphenylmethane-type bismaleimide and toluenediamine-type bismaleimide.
[0058] Bismaleimide (BMI) of diphenylmethane type has the characteristics of good heat resistance, high mechanical properties and high crosslinking density. Toluenediamine bismaleimide (TDI) has good bonding properties and flexibility. In this embodiment, the bismaleimide monomer can be one of BMI and TDI, or the two can be used in combination.
[0059] Wherein, when the bismaleimide monomer includes diphenylmethane bismaleimide and toluenediamine bismaleimide, the weight of the diphenylmethane bismaleimide and toluenediamine bismaleimide is controlled at 1.05-1.32:1 by compounding the two. The synthesized modified bismaleimide resin can have both heat resistance and toughness. Exemplarily, the weight of diphenylmethane bismaleimide and toluenediamine bismaleimide is controlled at 1.05:1, 1.21:1 or 1.32:1.
[0060] In an exemplary embodiment, the epoxy modifier includes a combination of one or more of triglycidyl p-aminophenol, resorcinol diglycidyl ether, bisphenol A diglycidyl ether, and tetraglycidyl 4,4-diaminodiphenylmethane.
[0061] In this embodiment, the addition of epoxy modifiers containing epoxy groups such as triglycidyl p-aminophenol, resorcinol diglycidyl ether, bisphenol A diglycidyl ether, and tetraglycidyl 4,4-diaminodiphenylmethane can reduce the crosslinking density of the bismaleimide resin, improve the brittleness of the cured resin composition, and improve the toughness of the resin composition; and the addition of the above-mentioned epoxy modifiers can reduce the viscosity of the synthesized bismaleimide resin, increase the viscosity of the resin composition, and improve the processability of the resin composition.
[0062] In an exemplary embodiment, the thermoplastic resin includes a combination of one or more of polyethersulfone, polyetheretherketone, polyimide, polyaryletherketone, polyphenylene ether, and polyetherimide.
[0063] In this embodiment, polyethersulfone (PES), polyetheretherketone (PEEK), polyimide (PI), polyaryletherketone (PAEK), polyphenylene ether (PPO) and polyetherimide (PEI) are a class of high-performance engineering plastics, which generally have excellent thermal stability, strength and rigidity, and can absorb more energy when subjected to impact loads to improve the toughness of bismaleimide resin.
[0064] The particle size of the thermoplastic toughening resin can be 10-50 μm, and can be screened by a sieving machine; using micron-grade thermoplastic toughening resin is conducive to its dissolution and dispersion in the system. For example, the average particle size of the thermoplastic toughening resin is 10 μm, 20 μm, and 50 μm.
[0065] In an exemplary embodiment, the raw materials of the composition further include a catalyst, and the amount of the catalyst used is 0.1-0.5% of the total weight of the composition.
[0066] In this embodiment, by adding a catalyst, the reaction process of the modified bismaleimide resin during the curing process can be catalyzed, the reaction temperature of the phenolic compound and the epoxy group can be reduced, and the reaction temperature of the bismaleimide resin can be reduced. Exemplarily, the amount of the catalyst is 0.1%, 0.3% or 0.5% of the total weight of the composition.
[0067] In an exemplary embodiment, the catalyst includes triphenylphosphine.
[0068] In this embodiment, the catalyst can be triphenylphosphine (PPh3 or (C6H5)3P for short), which can not only promote the reaction progress of the curing process and reduce the reaction temperature of the system, but also react with the epoxy groups in the modified bismaleimide resin to increase the crosslinking density and heat resistance of the epoxy resin, thereby improving the heat resistance and thermal stability of the resin composition.
[0069] like Figure 1 As shown, an exemplary embodiment of the present application provides a method for preparing a modified bismaleimide resin composition, comprising:
[0070] S110, mixing the allyl compound and the phenolic compound under first preset conditions to obtain a first premix.
[0071] In step S110, the first preset condition may be: a temperature of 120-130°C and a mixing and stirring time of 20-40 minutes.
[0072] Exemplarily, in one embodiment, the first preset condition is: the temperature is 120° C. and the mixing time is 40 min.
[0073] In another embodiment, the first preset condition is: the temperature is 125° C. and the mixing time is 30 minutes.
[0074] In another embodiment, the first preset condition is: the temperature is 130° C. and the mixing time is 20 min.
[0075] S120, mixing the first premix with the thermoplastic toughening resin under second preset conditions to obtain a second premix.
[0076] In step S120, the second preset condition may be: firstly cooling to 80-90°C and dispersing for 20-30 minutes to ensure that there is no agglomeration of the thermoplastic toughening resin; then heating to 140-150°C and continuously mechanically stirring for 20-30 minutes until a transparent and uniform second mixture is obtained.
[0077] Exemplarily, in one embodiment, step S120 includes:
[0078] The first premix was cooled to 80°C, and the thermoplastic toughening resin was added and dispersed for 30 minutes to ensure that there was no agglomeration of the thermoplastic toughening resin; then the temperature was raised to 140°C and mechanically stirred continuously for 30 minutes until a transparent and uniform second mixture was obtained.
[0079] In another embodiment, step S120 includes:
[0080] The first premix was cooled to 85°C, and the thermoplastic toughening resin was added and dispersed for 25 minutes to ensure that there was no agglomeration of the thermoplastic toughening resin; then the temperature was raised to 145°C and mechanically stirred continuously for 25 minutes until a transparent and uniform second mixture was obtained.
[0081] In another embodiment, step S120 includes:
[0082] The first premix is cooled to 90° C., and the thermoplastic toughening resin is added and dispersed for 20 minutes to ensure that there is no agglomeration of the thermoplastic toughening resin; then the temperature is raised to 150° C. and mechanically stirred continuously for 20 minutes until a transparent and uniform second mixture is obtained.
[0083] S130, mixing the second premix with the bismaleimide monomer under a third preset condition to obtain a third premix.
[0084] In step S130, the third preset condition may be: temperature of 120-130°C and mixing time of 20-40 minutes.
[0085] Exemplarily, in one embodiment, the third preset condition is: the temperature is 120° C. and the mixing time is 40 min.
[0086] In another embodiment, the first preset condition is: the temperature is 125° C. and the mixing time is 30 minutes.
[0087] In another embodiment, the first preset condition is: the temperature is 140° C. and the mixing time is 30 minutes.
[0088] S140, mixing the third premix with the epoxy modifier under fourth preset conditions to obtain a modified bismaleimide resin composition.
[0089] In step S140, the fourth preset condition may be: temperature of 80-100°C, mixing and stirring time of 20-40 minutes. For example, the fourth preset condition is: temperature of 80°C, mixing and stirring time of 40 minutes; the fourth preset condition is: temperature of 90°C, mixing and stirring time of 30 minutes.
[0090] Wherein, when the raw materials further include a catalyst, after the third premix is mixed with the epoxy modifier under the fourth preset condition, the temperature is lowered to 70-80° C., the catalyst is added, and stirred for 20-40 minutes to obtain a modified maleimide resin composition.
[0091] Illustratively, in one embodiment, the mixing temperature for adding the catalyst is 70° C. and the stirring time is 40 min.
[0092] In another embodiment, the mixing temperature for adding the catalyst is 75° C. and the stirring time is 30 min.
[0093] In another embodiment, the mixing temperature for adding the catalyst is 70° C. and the stirring time is 20 min.
[0094] An exemplary embodiment of the present application provides a prepreg, comprising reinforcing fibers and the modified bismaleimide resin as described above or a modified bismaleimide resin prepared by the method for preparing the modified bismaleimide resin as described above.
[0095] The modified bismaleimide resin prepared by the formula or method of the above embodiment has excellent heat resistance, toughness and process performance, and can meet the requirements of the paving and adhesion of prepreg at room temperature, thereby expanding its application in advanced structural composite materials.
[0096] The specific implementation methods of the present application are further described below in conjunction with preferred embodiments, and examples of preferred value ranges of each component in the modified bismaleimide resin provided in the present application are explained in detail.
[0097] Preferred Example 1
[0098] A modified bismaleimide resin composition comprises the following raw materials in parts by weight:
[0099] 20-40 parts by weight of allyl compound;
[0100] 0.2-2.5 parts by weight of phenolic compound;
[0101] 30-65 parts by weight of bismaleimide monomer;
[0102] Epoxy modifier 10-20 parts by weight;
[0103] 5-20 parts by weight of thermoplastic toughening resin;
[0104] Wherein, the weight ratio of the bismaleimide monomer, the allyl compound and the phenolic compound is 75-116:45-55:1.
[0105] Preferred Example 2
[0106] A modified bismaleimide resin composition comprises the following raw materials in parts by weight:
[0107] 20-40 parts by weight of allyl compound;
[0108] 0.2-2.5 parts by weight of phenolic compound;
[0109] 30-65 parts by weight of bismaleimide monomer;
[0110] Epoxy modifier 10-20 parts by weight;
[0111] 5-20 parts by weight of thermoplastic toughening resin;
[0112] Wherein, the weight ratio of bismaleimide monomer, allyl compound and phenolic compound is 75-116:45-55:1;
[0113] The weight ratio of the epoxy modifier to the phenolic compound is 20.0-24.0:1;
[0114] The weight ratio of the sum of the weights of the allyl compound, the phenolic compound, the bismaleimide monomer and the epoxy modifier to the thermoplastic toughening resin is 4.0-19.1:1.
[0115] Preferred Example 3
[0116] A modified bismaleimide resin composition comprises the following raw materials in parts by weight:
[0117] 20-40 parts by weight of allyl compound;
[0118] 0.2-2.5 parts by weight of phenolic compound;
[0119] 30-65 parts by weight of bismaleimide monomer;
[0120] Epoxy modifier 10-20 parts by weight;
[0121] 5-20 parts by weight of thermoplastic toughening resin;
[0122] Wherein, the weight ratio of bismaleimide monomer, allyl compound and phenolic compound is 75-116:45-55:1;
[0123] The weight ratio of the epoxy modifier to the phenolic compound is 20.0-24.0:1;
[0124] The weight ratio of the sum of the weight of the allyl compound, the phenolic compound, the bismaleimide monomer, and the epoxy modifier to the thermoplastic toughening resin is 4.0-19.1:1;
[0125] The allyl compound includes a combination of one or more of diallyl bisphenol A, diallyl bisphenol S, bisphenol A bisallyl ether, and diallyl phenol;
[0126] The phenolic compound includes a combination of one or more of phenol and bisphenol A;
[0127] The bismaleimide monomer includes a combination of one or more of diphenylmethane bismaleimide and toluenediamine bismaleimide;
[0128] The epoxy modifier includes a combination of one or more of triglycidyl p-aminophenol, resorcinol diglycidyl ether, bisphenol A diglycidyl ether, and tetraglycidyl 4,4-diaminodiphenylmethane;
[0129] The thermoplastic resin includes a combination of one or more of polyethersulfone, polyetheretherketone, polyimide, polyaryletherketone, polyphenylene ether, and polyetherimide.
[0130] Preferred Example 4
[0131] A modified bismaleimide resin composition comprises the following raw materials in parts by weight:
[0132] 20-40 parts by weight of allyl compound;
[0133] 0.2-2.5 parts by weight of phenolic compound;
[0134] 30-65 parts by weight of bismaleimide monomer;
[0135] Epoxy modifier 10-20 parts by weight;
[0136] 5-20 parts by weight of thermoplastic toughening resin;
[0137] Wherein, the weight ratio of bismaleimide monomer, allyl compound and phenolic compound is 75-116:45-55:1;
[0138] The weight ratio of the epoxy modifier to the phenolic compound is 20.0-24.0:1;
[0139] The weight ratio of the sum of the weight of the allyl compound, the phenolic compound, the bismaleimide monomer, and the epoxy modifier to the thermoplastic toughening resin is 4.0-19.1:1;
[0140] The allyl compound includes a combination of one or more of diallyl bisphenol A, diallyl bisphenol S, bisphenol A bisallyl ether, and diallyl phenol;
[0141] The phenolic compound includes a combination of one or more of phenol and bisphenol A;
[0142] The bismaleimide monomer includes diphenylmethane bismaleimide and toluenediamine bismaleimide, and the weight ratio of diphenylmethane bismaleimide to toluenediamine bismaleimide is 1.05-1.32:1;
[0143] The epoxy modifier includes a combination of one or more of triglycidyl p-aminophenol, resorcinol diglycidyl ether, bisphenol A diglycidyl ether, and tetraglycidyl 4,4-diaminodiphenylmethane;
[0144] The thermoplastic resin includes a combination of one or more of polyethersulfone, polyetheretherketone, polyimide, polyaryletherketone, polyphenylene ether, and polyetherimide.
[0145] Preferred Example 5
[0146] A modified bismaleimide resin composition comprises the following raw materials in parts by weight:
[0147] 25-36 parts by weight of allyl compound;
[0148] 0.5-0.8 parts by weight of phenolic compound;
[0149] 48-60 parts by weight of bismaleimide monomer;
[0150] Epoxy modifier 12-18 parts by weight;
[0151] 15-18 parts by weight of thermoplastic toughening resin;
[0152] The raw materials also include a catalyst, and the amount of the catalyst is 0.2-0.4% of the total mass of the composition;
[0153] The weight ratio of the bismaleimide monomer, the allyl compound, and the phenolic compound is 75-96:45-55:1;
[0154] The weight ratio of epoxy modifier to phenolic compound is 22.5-24.0:1;
[0155] The weight ratio of the sum of the weight of the allyl compound, the phenolic compound, the bismaleimide monomer, and the epoxy modifier to the thermoplastic toughening resin is 5.5-6.4:1;
[0156] The allyl compound includes a combination of one or more of diallyl bisphenol A, diallyl bisphenol S, bisphenol A bisallyl ether, and diallyl phenol;
[0157] The phenolic compound includes a combination of one or more of phenol and bisphenol A;
[0158] The bismaleimide monomer includes diphenylmethane bismaleimide and toluenediamine bismaleimide, and the weight ratio of diphenylmethane bismaleimide to toluenediamine bismaleimide is 1.09-1.14:1;
[0159] The epoxy modifier includes a combination of one or more of triglycidyl p-aminophenol, resorcinol diglycidyl ether, bisphenol A diglycidyl ether, and tetraglycidyl 4,4-diaminodiphenylmethane;
[0160] The thermoplastic resin includes one or more of polyethersulfone, polyetheretherketone, polyimide, polyaryletherketone, polyphenylene ether, and polyetherimide;
[0161] The catalyst includes triphenylphosphine.
[0162] In order to more clearly explain the technical solution of the present application, the present application lists a specific embodiment of the preparation method of the modified bismaleimide resin composition, and the beneficial effects of selecting the above range of the content of each component will be explained by giving specific experimental data through specific embodiments. The raw material components and contents of the modified bismaleimide resin in the embodiments of the present application do not limit the protection scope of the present application.
[0163] Example
[0164] Unless otherwise specified, the raw materials in the following examples are all commercially available.
[0165] Embodiment 1: A method for preparing a modified maleimide resin, comprising the following steps:
[0166] Take 25g of diallyl bisphenol A and 0.5g of phenol and place them in a three-necked flask, adjust the temperature of the oil bath to 125°C, mix and stir for 30min to obtain the first premix. Cool the first premix to 85°C, add 5g of polyethersulfone toughening particles, and disperse for 25min; then heat to 145°C, continuously mechanically stir for 25min to dissolve the polyethersulfone to obtain the second premix. Add 30g of toluene diamine type bismaleimide resin monomer and 28g of diphenylmethane type bismaleimide resin monomer to the second premix, stir at 125°C for 25min to obtain the third premix. Add 12g of bisphenol F diglycidyl ether to the third premix, mix it with bismaleimide resin monomer, diallyl bisphenol A, phenol and polyethersulfone, and control the temperature to 90°C, mix and stir for 30min; then cool to 75°C, add triphenylphosphine, stir for 30min to obtain a modified maleimide resin composition.
[0167] In order to more clearly explain the technical solution of the present application, the present application also lists Examples 2-12 of the preparation method of the modified bismaleimide resin composition, wherein the formulas of Examples 2-12 are shown in Table 1.
[0168] Table 1 shows a specific example of the modified bismaleimide resin composition in the present application. It should be noted that, except for the parameters listed in Table 1, other parameters of Examples 2-12 are substantially the same as those of Example 1.
[0169] Wherein, the ratio C1 is the weight ratio of the bismaleimide monomer, the allyl compound, and the phenolic compound;
[0170] The ratio C2 is the weight ratio of the epoxy modifier to the phenolic compound;
[0171] The ratio C3 is the weight ratio of the sum of the weights of the allyl compound, the phenolic compound, the bismaleimide monomer, and the epoxy modifier to the weight ratio of the thermoplastic toughening resin;
[0172] The ratio C4 is the weight ratio of diphenylmethane type bismaleimide to toluenediamine type bismaleimide.
[0173] Table 1 Raw material formula table of embodiment (unit: g)
[0174]
[0175] Table 1 (Continued) Raw material formula table of the embodiment (unit: g)
[0176]
[0177] Performance Testing
[0178] The properties of the modified bismaleimide resin composition prepared in the example were tested according to the following method, and the test results are recorded in Table 2.
[0179] 1. Viscosity value: Pour the resin composition into a glass vial of a rotational rheometer and test its viscosity value at 85-130°C; wherein the heating rate is 1.5°C / min, the GAP is 500-1000μm, and the test range is 25°C-230°C. The lower the viscosity value, the better the fluidity of the resin composition, that is, the better the process performance.
[0180] 2. Fracture toughness: According to the change of viscosity value of the resin composition, pour the resin composition into K IC The mold is then placed in a vacuum oven for vacuum degassing at low viscosity temperature for 60-90 minutes to obtain a prefabricated specimen; a universal testing machine (MTS5KN) is used to perform a three-point bending test on the prefabricated specimen at a rate of 1 mm / min. The higher the fracture toughness value, the better the toughness of the resin composition.
[0181] 3. Heat resistance: The glass transition temperature of the resin composition is tested by differential scanning calorimetry (DSC). The higher the glass transition temperature, the better the heat resistance of the resin composition.
[0182] Table 2 Performance test table of the modified bismaleimide resin composition of the embodiment
[0183]
[0184] Table 2 (Continued) Performance test table of the modified bismaleimide resin composition of the embodiment
[0185]
[0186] Combining Table 1, Table 2 and Examples 1-4, it can be seen that the resin composition in Example 1-3 has the lowest viscosity value at about 115°C, while the viscosity value of the resin composition in Example 4 is always significantly higher than that in Example 1-3, indicating that the processability of Example 4 is relatively poor. Compared with Example 4, the glass transition temperature of the resin composition of Example 1-3 is ≥220°C, indicating that the resin composition of Example 1-3 has better heat resistance. Compared with Example 1-2, the resin composition of Example 3-4 has better fracture toughness. It can be shown that with the increase in the amount of thermoplastic toughening resin, the toughness of the resin composition will gradually increase, but the thermoplastic toughening resin will reduce the crosslinking density of the bismaleimide resin, affect its heat resistance, and also cause the viscosity of the resin composition to increase. Therefore, it is necessary to control the amount of thermoplastic toughening resin.
[0187] In the present application, the raw materials for preparing the modified bismaleimide resin composition also have a synergistic effect. In addition to toughening and modifying the bismaleimide resin by adding a thermoplastic toughening resin, the reaction between the epoxy modifier, the phenolic compound and the bismaleimide resin monomer is also used to improve the toughness of the resin composition while maintaining good heat resistance and processability. Among them, Example 3, Example 8 and Example 10 can simultaneously maintain good heat resistance, toughness and processability, and have better comprehensive performance. It can be seen that by adjusting the amount and proportion of each raw material, when the allyl compound is 25-36 parts by weight; the phenolic compound is 0.5-0.8 parts by weight; the bismaleimide monomer is 48-60 parts by weight; the epoxy modifier is 12-18 parts by weight; the thermoplastic toughening resin is 15-18 parts by weight; wherein the raw materials also include a catalyst, and the amount of the catalyst is 0.2-0.4% of the total mass of the composition; the bismaleimide monomer The weight ratio of the epoxy modifier to the phenolic compound is 75-96:45-55:1; the weight ratio of the epoxy modifier to the phenolic compound is 22.5-24.0:1; the weight ratio of the sum of the weights of the allyl compound, the phenolic compound, the bismaleimide monomer and the epoxy modifier to the thermoplastic toughening resin is 5.5-6.4:1; when the weight ratio of diphenylmethane type bismaleimide and toluenediamine type bismaleimide is 1.09-1.14:1, the modified bismaleimide resin composition obtained thereby has excellent heat resistance, toughness and process performance.
[0188] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0189] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application is described in detail with reference to the above embodiments, a person skilled in the art should understand that the technical solutions described in the above embodiments can still be modified, or some of the technical features can be replaced by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present application.
Claims
1. A modified bismaleimide resin composition, characterized in that: The invention comprises the following raw materials in parts by weight: 20-40 parts by weight of allyl compound; 0.2-2.5 parts by weight of phenolic compound; 30-65 parts by weight of bismaleimide monomer; Epoxy modifier 10-20 parts by weight; 5-20 parts by weight of thermoplastic toughening resin.
2. The modified bismaleimide resin composition according to claim 1, characterized in that The weight ratio of the bismaleimide monomer, the allyl compound and the phenolic compound is 75-116:45-55:
1.
3. The modified bismaleimide resin composition according to claim 1, characterized in that: The weight ratio of the epoxy modifier to the phenolic compound is 20.0-24.0:
1.
4. The modified bismaleimide resin composition according to claim 1, characterized in that: The weight ratio of the sum of the weights of the allyl compound, the phenolic compound, the bismaleimide monomer, and the epoxy modifier to the thermoplastic toughening resin is 4.0-19.1:
1.
5. The modified bismaleimide resin composition according to any one of claims 1 to 4, characterized in that: The allyl compound includes a combination of one or more of diallyl bisphenol A, diallyl bisphenol S, bisphenol A bisallyl ether, and diallyl phenol; The phenolic compound includes a combination of one or more of phenol, bisphenol A, and allyl phenol; The bismaleimide monomer includes a combination of one or more of diphenylmethane bismaleimide and toluenediamine bismaleimide; The epoxy modifier includes a combination of one or more of triglycidyl p-aminophenol, resorcinol diglycidyl ether, bisphenol A diglycidyl ether, and tetraglycidyl 4,4-diaminodiphenylmethane; The thermoplastic resin includes one or more of polyethersulfone, polyetheretherketone, polyimide, polyaryletherketone, polyphenylene ether, and polyetherimide.
6. The modified bismaleimide resin composition according to claim 5, characterized in that: When the bismaleimide monomer comprises diphenylmethane bismaleimide and toluenediamine bismaleimide, the weight ratio of the diphenylmethane bismaleimide to the toluenediamine bismaleimide is 1.05-1.32:
1.
7. The modified bismaleimide resin composition according to claim 1, characterized in that: The raw materials of the composition also include a catalyst, and the amount of the catalyst used is 0.1-0.5% of the total weight of the composition.
8. The modified bismaleimide resin composition according to claim 7, characterized in that: The catalyst includes triphenylphosphine.
9. A method for preparing a modified bismaleimide resin composition, characterized in that: The preparation method of the modified bismaleimide resin composition is used to prepare the modified bismaleimide resin composition according to any one of claims 1 to 8, and the preparation method comprises: mixing the allyl compound and the phenolic compound under a first preset condition to obtain a first premix; Mixing the first premix with the thermoplastic toughening resin under second preset conditions to obtain a second premix; Mixing the second premix with the bismaleimide monomer under third preset conditions to obtain a third premix; The third premix is mixed with the epoxy modifier under fourth preset conditions to obtain the modified bismaleimide resin composition.
10. A prepreg, characterized in that: The invention comprises reinforcing fibers and the modified bismaleimide resin according to any one of claims 1 to 8 or a modified bismaleimide resin prepared by the preparation method of the modified bismaleimide resin according to claim 9.
Citation Information
Cited By
Bismaleimide resin for high-modulus carbon fiber prepreg and preparation method of bismaleimide resin
CN120737605A
Toughened bismaleimide resin, preparation method thereof and prepreg
CN121086525A
Low-viscosity toughened bismaleimide resin composition and preparation method thereof
CN122587474A
A bismaleimide resin composition toughened by a solubilizer, a prepreg, a composite material, and a method for producing the same
CN123026913A