Sodium manganate positive electrode material and preparation method and application thereof
By adopting sodium manganate positive electrode material with the chemical formula NaxTikWzMn1-z-kO2, including O'3 phase sodium manganate and externally doped with element M, the problem of low performance of the positive electrode material of sodium ion battery is solved and high specific capacity is achieved , improvements in rate performance and cycle performance.
Patent Information
- Application Number
- CN202411144958.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-12-03
AI Technical Summary
The existing sodium ion battery positive electrode materials are relatively low in specific capacity, rate performance and cycle performance, and cannot compete with lithium ion battery positive electrodes.
The sodium manganate positive electrode material with the chemical formula NaxTikWzMn1-z-kO2 includes sodium manganate O'3 phase, and optionally contains external doping element M. It is prepared by a specific calcining process to form high specific capacity and magnification performance. and cycling properties of materials.
The high specific capacity, high rate performance and high cycle performance of sodium manganate positive electrode material are achieved, and the cost-effectiveness of sodium ion batteries is improved.
Smart Images

Figure CN119069686A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion batteries, and in particular relates to a sodium manganate positive electrode material and a preparation method and application thereof. Background Art
[0002] Lithium-ion battery technology is mature, but the relative lack of lithium resources and uneven distribution have affected the continued development and utilization of lithium-ion batteries. Sodium-ion batteries have received widespread attention and research due to their abundant and widely distributed sodium resources, and have the greatest potential to replace lithium-ion batteries. The positive electrode material in the battery plays a decisive role in the performance of the battery. Due to its own performance, the existing sodium-ion battery positive electrode cannot compete with the lithium-ion battery positive electrode in terms of capacity (the capacity of mature sodium-ion battery positive electrodes on the market is generally 150mAh / g, while the capacity of mature lithium-ion battery positive electrodes is above 200mAh / g). Due to the large amount of nickel oxide used as raw materials, the specific capacity, rate performance and cycle performance of sodium-ion battery positive electrode materials are low, and they cannot show their cost-effective advantages. Summary of the invention
[0003] Therefore, the technical problem to be solved by the present invention is to overcome the defects of low specific capacity, rate performance and cycle performance of existing sodium ion battery positive electrode materials, thereby providing a sodium manganate positive electrode material and a preparation method and application thereof.
[0004] The present invention provides a sodium manganate positive electrode material, the chemical general formula of the sodium manganate positive electrode material is Na x Ti k W z Mn 1-z-k O2, where 0.9≤x≤1, 0 <z≤0.03,0.01<k≤0.05;
[0005] The sodium manganate positive electrode material includes O'3 phase sodium manganate.
[0006] Optionally, the content of O'3 phase sodium manganate in the sodium manganate positive electrode material is 60%-90%.
[0007] Optionally, the sodium manganate positive electrode material also includes P2 phase sodium manganate.
[0008] Preferably, the sodium manganate positive electrode material further includes an external doping element M;
[0009] The chemical formula of the sodium manganate positive electrode material is Na x Ti k M y W z Mn 1-z-y-k O2, where 0.9≤x≤1, 0 <z≤0.03,0<y≤0.05,0.01<k≤0.05;
[0010] The external doping element M is selected from at least one of Al, Ca, Sn, Sb, Mo, Li, Cu, K, Zn, and Mg.
[0011] The present invention provides a method for preparing the above-mentioned sodium manganate positive electrode material, comprising the following steps:
[0012] The sodium source, titanium source, tungsten source and manganese source are weighed and mixed according to a stoichiometric ratio, and the mixture is subjected to a first calcination and a second calcination to obtain the sodium manganate positive electrode material.
[0013] Preferably, the sodium source is selected from at least one of sodium oxalate, sodium hydroxide and sodium carbonate;
[0014] The titanium source is selected from at least one of titanium dioxide, titanium sulfate and titanium oxalate;
[0015] The manganese source is selected from at least one of manganese acetate, manganese oxide, manganese dioxide, manganese nitrate, manganese sulfate, and manganese trioxide;
[0016] The tungsten source is selected from at least one of ammonium paratungstate, ammonium tungstate, ammonium metatungstate and tungsten trioxide.
[0017] Preferably, when the sodium source, titanium source, tungsten source and manganese source are weighed and mixed according to the stoichiometric ratio, the step of adding an external doping element compound is also included;
[0018] The external doping element compound is selected from at least one of CaO, CaCO3, Ca(OH)2, K2CO3, KOH, Li2CO3, KOH, MgO, MgSO4, SnO2, Sb2O5, MoO3, (NH4)2MoO4, CuO, CuSO4, Cu(NO3)2, ZnO, Zn(NO3)2, Al2O3, and AlOOH.
[0019] Preferably, the first calcination temperature is 600-800°C, and the first calcination time is 2-5h;
[0020] Optionally, the first calcination is performed in air or oxygen atmosphere.
[0021] Optionally, the first calcination temperature is 800° C., and the first calcination time is 4 hours.
[0022] Preferably, the second calcination temperature is 900-1100°C, and the second calcination time is 9-12h;
[0023] Optionally, the second calcination is performed in air or oxygen atmosphere.
[0024] Optionally, the second calcination temperature is 1000° C., and the second calcination time is 10 h.
[0025] Preferably, the mixing time is 5 - 20 min;
[0026] After the second calcination, a cooling step is further included.
[0027] Preferably, the heating rate of the first calcination is 1 - 10 °C;
[0028] The heating rate of the second calcination is 1 - 10 °C.
[0029] The present invention also provides an application of the sodium manganese oxide cathode material described above or the sodium manganese oxide cathode material prepared by the above - described preparation method in a sodium - ion battery.
[0030] The technical solution of the present invention has the following advantages:
[0031] 1. For the sodium manganese oxide cathode material provided by the present invention, the chemical general formula of the sodium manganese oxide cathode material is Na x Ti k W z Mn 1-z-k O2, where 0.9 ≤ x ≤ 1, 0 < z ≤ 0.01, 0.01 < k ≤ 0.04. The sodium manganese oxide cathode material includes O'3 - phase sodium manganese oxide. In the sodium manganese oxide cathode material of the present invention, specific contents of Ti, W cooperate with Na and Mn to form stable O'3 - phase sodium manganese oxide, which is beneficial to the capacity performance of the cathode material. The specific sodium manganese oxide cathode material of the present invention has the advantages of high specific capacity, high rate performance, and high cycle performance.
[0032] 2. For the sodium manganese oxide cathode material provided by the present invention, the sodium manganese oxide cathode material further includes an externally doped element M; the chemical general formula of the sodium manganese oxide cathode material is Na x Ti k M y W z Mn 1-z-y-k O2, where 0.9 ≤ x ≤ 1, 0 < z ≤ 0.03, 0 < y ≤ 0.05, 0.01 < k ≤ 0.05; the externally doped element M is selected from at least one of Al, Ca, Sn, Sb, Mo, Li, Cu, K, Zn, Mg. By adding an external metal element, the present invention helps to further improve the specific capacity and cycle performance of the cathode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following will briefly introduce the drawings required for the description of the specific embodiments or the prior art. Obviously, the following drawings are some embodiments of the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative efforts.
[0034] Figure 1 XRD test pattern of the sodium manganate positive electrode material of Example 1 of the present invention;
[0035] Figure 2 The voltage-specific capacity corresponding curve of the first cycle of charge and discharge of the sodium manganate positive electrode material of Example 1 of the present invention. DETAILED DESCRIPTION
[0036] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0037] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0038] Example 1
[0039] This embodiment provides a method for preparing a sodium manganate positive electrode material, comprising the following steps:
[0040] Sodium carbonate, titanium dioxide, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, titanium element, tungsten element and manganese element of 1.0:0.02:0.01:0.97, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the sodium manganate positive electrode material (NaTi 0.02 W 0.01 Mn 0.97 O2).
[0041] The sodium manganate positive electrode material obtained in this embodiment is subjected to XRD scanning, and the results show that the obtained sodium manganate positive electrode material is mainly O'3 phase sodium manganate, and its content is 85.6%. In addition, it contains a small amount of P2 phase sodium manganate. The mixed phase sodium manganate mainly composed of O'3 phase prepared by the present invention can have high capacity and high rate performance. The XRD detection diagram is as follows Figure 1 As shown, Figure 1 Also included are the XRD standard PDF card of O'3 phase sodium manganate (No. 73-0156) and the XRD standard PDF card of P2 phase sodium manganate (No. 54-0894) for comparison.
[0042] Example 2
[0043] This embodiment provides a method for preparing a sodium manganate positive electrode material, comprising the following steps:
[0044] Sodium carbonate, titanium dioxide, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, titanium element, tungsten element and manganese element of 0.95:0.02:0.02:0.96, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the sodium manganate positive electrode material (Na 0.95 Ti 0.02 W 0.02 Mn 0.96 O2).
[0045] Example 3
[0046] This embodiment provides a method for preparing a sodium manganate positive electrode material, comprising the following steps:
[0047] Sodium carbonate, titanium dioxide, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, titanium element, tungsten element and manganese element of 1:0.02:0.01:0.97, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 5°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 5°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the sodium manganate positive electrode material (NaTi 0.02 W 0.01 Mn 0.97 O2).
[0048] Example 4
[0049] This embodiment provides a method for preparing a sodium manganate positive electrode material, comprising the following steps:
[0050] Sodium carbonate, titanium dioxide, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, titanium element, tungsten element and manganese element of 1:0.02:0.01:0.97, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 950°C at a heating rate of 2°C / min in an air atmosphere, calcined at 950°C for 10 hours, and naturally cooled to room temperature to obtain the sodium manganate positive electrode material (NaTi0.02 W 0.01 Mn 0.97 O2).
[0051] Example 5
[0052] This embodiment provides a method for preparing a sodium manganate positive electrode material, comprising the following steps:
[0053] Sodium carbonate, titanium dioxide, calcium carbonate, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, titanium element, calcium element, tungsten element and manganese element of 0.9:0.05:0.02:0.01:0.92, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the sodium manganate positive electrode material (Na 0.9 Ti 0.05 Ca 0.02 W 0.01 Mn 0.92 O2).
[0054] Comparative Example 1
[0055] This comparative example provides a method for preparing a sodium manganate positive electrode material, comprising the following steps:
[0056] Sodium carbonate, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, tungsten element and manganese element of 1.0:0.01:0.99, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the sodium manganate positive electrode material (NaW 0.01 Mn 0.99 O2).
[0057] Comparative Example 2
[0058] This comparative example provides a method for preparing a sodium manganate positive electrode material, comprising the following steps:
[0059] Sodium carbonate, titanium dioxide, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, titanium element, tungsten element and manganese element of 1.0:0.005:0.01:0.985, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the sodium manganate positive electrode material (NaTi 0.005 W 0.01 Mn 0.985 O2).
[0060] Comparative Example 3
[0061] This comparative example provides a method for preparing a sodium manganate positive electrode material, comprising the following steps:
[0062] Sodium carbonate, titanium dioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, titanium element and manganese element of 1.0:0.02:0.98, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the sodium manganate positive electrode material (NaTi 0.02 Mn 0.98 O2).
[0063] Comparative Example 4
[0064] This comparative example provides a method for preparing a sodium manganate positive electrode material, comprising the following steps:
[0065] Sodium carbonate, titanium dioxide, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, titanium element, tungsten element and manganese element of 0.8:0.02:0.01:0.97, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the sodium manganate positive electrode material (Na 0.8 Ti 0.02 W 0.01 Mn 0.97 O2).
[0066] Test Case
[0067] The sodium manganate positive electrode materials prepared in Examples 1-5 and Comparative Examples 1-4 were used as the positive electrode main materials to prepare positive electrode sheets, N-methylpyrrolidone was used as a dispersant, and the positive electrode main material: carbon black: PVDF (polyvinylidene fluoride): dispersant were mixed in a mass ratio of 95:2.5:2.5:120 to prepare a positive electrode slurry, and the same mass of the positive electrode slurry was evenly coated on an aluminum foil, compacted for the same time under the same pressure conditions, and then dried in an oven at 80°C for 2h to obtain a positive electrode sheet; metallic sodium was used as a negative electrode sheet, glass fiber was used as a diaphragm, and 1 mol / L NaPF6 ethylene carbonate (EC) / dimethyl carbonate (DMC) solution was used as an electrolyte (the volume ratio of EC and DMC was 1:1), and in an argon atmosphere of a glove box, the positive electrode sheet, the negative electrode sheet, the electrolyte, the diaphragm, the gasket and the spring were placed in a button battery shell to assemble a CR2032 button battery.
[0068] The button cell was placed in the Blue Electric test system for electrical performance testing. The electrical performance test parameters were set as follows: voltage range 2.0V-4.0V, the first cycle was charged and discharged at 0.1C / 0.1C for charge and discharge specific capacity test, and then charged and discharged at 0.2C / 0.2C and 0.5C / 0.5C to test the charge and discharge specific capacity at different rates, and then charged and discharged at 1C / 1C for 50 cycles, and the discharge rate performance was evaluated by the value of the lower discharge specific capacity of the first cycle of 1C rate cycle / the discharge specific capacity of the first cycle at 0.1C rate*100%; and the cycle performance was evaluated based on the discharge specific capacity retention rate of 50 cycles of 1C / 1C charge and discharge, and the cycle discharge specific capacity retention rate = the lower discharge specific capacity of the 50th cycle of 1C rate cycle / the discharge specific capacity of the first cycle of 1C rate cycle*100%. The test results of the discharge specific capacity, discharge rate performance and 1C / 1C cycle 50 cycle capacity retention rate of the first cycle of 0.1C / 0.1C charge and discharge are shown in Table 1. Among them, the voltage-specific capacity corresponding curve of the first cycle of charge and discharge cycle of the positive electrode material of Example 1 of the present invention is shown in Table 1. Figure 2 shown.
[0069] Table 1
[0070]
[0071] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A sodium manganate positive electrode material, characterized in that: The chemical formula of the sodium manganate positive electrode material is Na x Ti k W z Mn 1-z-k O2, where 0.9≤x≤1, 0 <z≤0.03,0.01<k≤0.05; The sodium manganate positive electrode material includes O'3 phase sodium manganate.
2. The sodium manganate positive electrode material according to claim 1, characterized in that: The sodium manganate positive electrode material also includes an external doping element M; The chemical formula of the sodium manganate positive electrode material is Na x Ti k M y W z Mn 1-z-y-k O2, where 0.9≤x≤1, 0 <z≤0.03,0<y≤0.05,0.01<k≤0.05; The external doping element M is selected from at least one of Al, Ca, Sn, Sb, Mo, Li, Cu, K, Zn, and Mg.
3. A method for preparing the sodium manganate positive electrode material according to claim 1 or 2, characterized in that: The steps include: The sodium source, titanium source, tungsten source and manganese source are weighed and mixed according to a stoichiometric ratio, and the mixture is subjected to a first calcination and a second calcination to obtain the sodium manganate positive electrode material.
4. The method for preparing the sodium manganate positive electrode material according to claim 3, characterized in that: The sodium source is selected from at least one of sodium oxalate, sodium hydroxide and sodium carbonate; The titanium source is selected from at least one of titanium dioxide, titanium sulfate and titanium oxalate; The manganese source is selected from at least one of manganese acetate, manganese oxide, manganese dioxide, manganese nitrate, manganese sulfate, and manganese trioxide; The tungsten source is selected from at least one of ammonium paratungstate, ammonium tungstate, ammonium metatungstate and tungsten trioxide.
5. The method for preparing the sodium manganate positive electrode material according to claim 3 or 4, characterized in that: When the sodium source, titanium source, tungsten source and manganese source are weighed and mixed according to the stoichiometric ratio, the step of adding an external doping element compound is also included; The external doping element compound is selected from at least one of CaO, CaCO3, Ca(OH)2, K2CO3, KOH, Li2CO3, KOH, MgO, MgSO4, SnO2, Sb2O5, MoO3, (NH4)2MoO4, CuO, CuSO4, Cu(NO3)2, ZnO, Zn(NO3)2, Al2O3, and AlOOH.
6. The method for preparing the sodium manganate positive electrode material according to any one of claims 3 to 5, characterized in that: The first calcination temperature is 600-800°C, and the first calcination time is 2-5h; Optionally, the first calcination is performed in air or oxygen atmosphere.
7. The method for preparing the sodium manganate positive electrode material according to any one of claims 3 to 6, characterized in that: The second calcination temperature is 900-1100°C, and the second calcination time is 8-15h; Optionally, the second calcination is performed in air or oxygen atmosphere.
8. The method for preparing the sodium manganate positive electrode material according to any one of claims 3 to 7, characterized in that: The mixing time is 5-20min; The second calcination further includes a cooling step after completion.
9. The method for preparing the sodium manganate positive electrode material according to any one of claims 3 to 8, characterized in that: The heating rate of the first calcination is 1-10°C; The heating rate of the second calcination is 1-10°C.
10. Use of the sodium manganate positive electrode material according to claim 1 or 2 or the sodium manganate positive electrode material prepared by the preparation method according to any one of claims 3 to 9 in a sodium ion battery.