Battery
By adjusting the proportion of linear organic matter mass of C1-C4 in the electrolyte and the coverage of the diaphragm adhesive layer, optimizing lithium ion transmission, combining explosion-proof valves and insulating adhesive paper, the fast charging performance and safety problems of lithium iron phosphate batteries are solved, and the More efficient battery performance and safety.
Patent Information
- Application Number
- CN202411201418.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
AI Technical Summary
Lithium iron phosphate batteries have problems with long charging time and short battery life in the field of power batteries. This is mainly due to the obstruction of lithium ions transmission between the positive and negative electrodes, resulting in large ohmic impedance and serious safety hazards.
By controlling the coverage of S1 and the separator adhesive layer of C1-C4 in the electrolyte, the transmission of lithium ions between the electrodes is optimized, the fast charging and cycling performance of the battery is improved, and the explosion-proof valve and insulation are combined through the battery case Structures such as tapered paper improve safety performance.
It effectively improves the transmission speed of lithium ions between the positive and negative electrodes, improves the fast charging performance and safety of the battery, and reduces the risk of expansion and explosion.
Smart Images

Figure CN119069768A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a battery. Background Art
[0002] Compared with traditional batteries, lithium-ion batteries have advantages such as high specific energy, long cycle life, no pollution, and high operating voltage, so they have been widely used in many fields such as portable electronic devices, energy storage, and automotive power. With the gradual promotion of electric vehicles, the demand for fast charging performance and safety performance of power batteries is increasing.
[0003] Lithium iron phosphate batteries have the advantages of good safety and low cost, which makes them have a large share in the field of power batteries. Compared with oil vehicles, the biggest problem of electric vehicles at present is the long charging time and short endurance, which is attributed to the poor rate performance and low energy density of lithium iron phosphate. On the one hand, the electronic conductivity and ion conductivity of lithium iron phosphate positive electrode particles are low, and the transmission of lithium ions inside the particles is hindered; on the other hand, in order to increase the energy density, the surface density and compaction density of the pole piece are increased, but under this condition, the transmission of lithium ions between the positive and negative electrodes is hindered, so that the lithium iron phosphate battery has a large ohmic impedance, and a large amount of Joule heat will be generated under high-rate charging conditions, resulting in serious safety hazards to the battery. Summary of the invention
[0004] The object of the present invention is to overcome the above-mentioned problems existing in the prior art and provide a battery, wherein the mass proportion S1 of the linear organic matter of C1-C4 and the coverage of the diaphragm glue layer meet the requirements of Improve the rapid transmission of lithium ions between electrodes and enhance the fast charging cycle performance of the battery.
[0005] In order to achieve the above object, the present invention provides a battery, the battery comprising an electrode assembly, the electrode assembly comprising a positive electrode sheet, a separator and a negative electrode sheet arranged in a stacked manner; the positive electrode sheet comprises lithium iron phosphate;
[0006] The battery includes an electrolyte, the electrolyte includes a first solvent, and the first solvent includes a C1-C4 linear organic matter; the mass proportion of the first solvent is recorded as S1 based on the total mass of the electrolyte;
[0007] The diaphragm includes a base film, and a glue layer is provided on at least one side of the base film; the coverage of the glue layer on the base film is denoted as w; S1 and w satisfy:
[0008] The present invention adopts the above technical solution to achieve the following beneficial effects:
[0009] (1) The battery provided by the present invention can solve the problem of slow transmission of lithium ions between the positive and negative electrodes by adjusting the mass ratio of the low-viscosity solvent and the coverage rate of the diaphragm glue layer to meet a specific relationship, thereby improving the fast charging performance of the battery.
[0010] (2) The battery provided by the present invention suppresses the problem of glue layer shedding and pore blocking by controlling the lithium salt content in the electrolyte, the coverage of the glue layer, and the mass ratio of the first solvent and the second solvent, thereby improving the stability of the battery.
[0011] (3) The battery provided by the present invention solves the problem that the diaphragm glue layer and low-viscosity solvent are easy to swell and explode by using a battery shell in combination with an explosion-proof valve, thereby improving the safety performance of the battery.
[0012] (4) The battery provided by the present invention improves the safety performance of the battery by using a diaphragm outer packaging structure, insulating tape and Mylar film.
[0013] The endpoints and any values of the range disclosed in this article are not limited to the precise range or value, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 Shown is a schematic diagram of the structure of a square shell battery.
[0015] Figure 2 Shown are schematic diagrams of the structure of square shell batteries at different angles.
[0016] Figure 3 Shown is a schematic diagram of the cross-sectional structure of the battery shell in a square shell battery.
[0017] Figure 4 Shown is a schematic diagram of the structure of an explosion-proof valve.
[0018] Figure 5 Shown is a schematic diagram of the structure of an explosion-proof valve.
[0019] Figure 6 Shown is a schematic diagram of the interface structure of the electrode assembly.
[0020] Figure 7 Shown is a schematic diagram of the interface structure of the electrode assembly.
[0021] Figure markings: 1-shell; 11-third side, 12-fourth side; 2-top cover; 3-positive electrode column; 4-negative electrode column; 5-liquid injection hole; 6-explosion-proof valve; 61-explosion-proof plate; 62-notched groove; 7-bottom wall; 8-positive electrode sheet; 9-diaphragm; 10-negative electrode sheet; 11-insulating tape; 12-Mylar film. DETAILED DESCRIPTION
[0022] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0023] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.
[0024] In the present invention, the terms "lithium battery", "lithium-ion battery" and "lithium-ion secondary battery" all have the same meaning and refer to batteries, which generally include an electrode assembly (such as a positive electrode sheet, a negative electrode sheet and a separator), a container (shell) for accommodating the electrode assembly, and an electrolyte.
[0025] In the present invention, the term "Dv50" refers to the particle size corresponding to when the cumulative volume particle size distribution percentage of a sample reaches 50%. Dv50 can be tested using a laser particle size analyzer.
[0026] In the present invention, the term "low viscosity solvent" refers to a solvent having a viscosity of less than or equal to 0.65 mPa.s. The term "high viscosity solvent" refers to a solvent having a viscosity greater than 0.65 mPa.s. As an embodiment, the test method for solvent viscosity can refer to the rotation method in the national standard GB / T 10247-2008, and the viscosity is measured by a rheometer. The viscosity of a solvent is its inherent property and can be obtained by consulting reference books, literature, etc.
[0027] The present invention provides a battery, the battery comprising an electrode assembly, the electrode assembly comprising a positive electrode sheet, a separator and a negative electrode sheet arranged in a stacked manner;
[0028] The battery includes an electrolyte, the electrolyte includes a first solvent, and the first solvent includes a C1-C4 linear organic matter; the mass proportion of the first solvent is recorded as S1 based on the total mass of the electrolyte;
[0029] The diaphragm includes a base film, and a glue layer is disposed on at least one side of the base film (the glue layer may be directly disposed on the surface of the base film, or may not be directly disposed on the surface of the base film); the coverage of the glue layer on the base film is denoted as w; S1 and w satisfy:
[0030] In some embodiments, the ratio of S1 to w can be, for example, 0.1, 0.2, 0.5, 0.8, 1.0, 1.2, 1.5, 1.6, 2.0, 2.2, 2.5, 2.8, 3.0, 3.2, 3.5, 3.8, 4.0, preferably
[0031] In the present invention, the linear organic matter of C1-C4 has a relatively low viscosity (less than 0.7 mPa.s). The low-viscosity first solvent is used in combination with a diaphragm with a glue layer coverage of w, which can greatly improve the fast charging performance of the battery. The larger the value, the smaller the ohmic impedance of the battery, the better the fast charging performance of the battery, but the worse the safety performance of the battery; the more the first solvent (the larger S1), the smaller the viscosity of the electrolyte, the smaller the w, the smaller the glue layer coverage on the surface of the diaphragm, the faster the transmission of lithium ions in the diaphragm, and the better the fast charging performance of the battery; but When the value is too large and greater than 4, too much low-viscosity first solvent is used, and the low-viscosity first solvent is more likely to produce gas through side reactions at the positive and negative electrodes, increasing the risk of battery gas production and explosion; at the same time, the smaller the coverage of the diaphragm's glue layer, the more base film is exposed, and the greater the probability of being pierced by lithium dendrites, increasing the risk of internal short circuit in the battery; in addition, too much low-viscosity first solvent will cause the diaphragm glue layer to fall off, and after the glue layer falls off, it will cause the diaphragm to be blocked, the battery impedance will increase sharply, and the battery performance will decrease. The smaller the value, the less S1 is added, which is not conducive to improving the transmission of lithium ions and the effect of improving the fast charging performance of the battery is not good; at the same time, the larger the w is, the greater the coverage of the diaphragm glue layer is, which hinders the transmission of lithium ions; When the value is too small and less than 0.1, the amount of S1 added is too little or W is too large, resulting in obvious obstruction of lithium ion transmission and the inability to effectively improve the fast charging performance of the battery.
[0032] In some embodiments, the mass percentage S1 of the first solvent satisfies: 5%≤S1≤70%, for example, S1 may be 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, preferably 15%≤S1≤60%. When S1 and w satisfy When the mass proportion of the first solvent is adjusted to be within the above range, the impedance of lithium ion transmission in the liquid phase of the electrolyte is small, and the solvation energy is low, which can reduce the lithium ion interface transmission impedance, thereby quickly transferring lithium ions and reducing the temperature rise of the battery; at the same time, avoid S1 being too large, and the high viscosity solvent proportion is small, resulting in unstable interface generated by the electrolyte at the negative electrode, thereby causing continuous decomposition of the electrolyte, increased gas production, and a higher battery expansion rate.
[0033] In some embodiments, the coverage w of the adhesive layer on the base film satisfies: 10%≤w≤90%, for example, w can be 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, more preferably 20%≤w≤70%. When S1 and w satisfy When the coverage of the glue layer is adjusted within the above range, the transmission performance of lithium ions can be further improved, the fast charging performance and safety performance of the battery can be improved, and the diaphragm can be punctured and the internal short circuit of the battery can be avoided due to the small coverage of the glue layer. It can also be avoided that the porosity of the diaphragm is small and the transmission of lithium ions is hindered due to the large coverage of the glue layer.
[0034] In some embodiments, the structure of the diaphragm includes glue layer + base film, glue layer + heat-resistant layer + base film, glue layer + heat-resistant layer + base film + glue layer (the heat-resistant layer is close to the positive electrode sheet), glue layer + heat-resistant layer + base film + heat-resistant layer + glue layer. Preferably, the diaphragm has a glue layer + heat-resistant layer + base film + glue layer structure.
[0035] In some embodiments, the diaphragm includes a base film, a glue layer is provided on the surface of the base film close to the negative electrode sheet, a heat-resistant layer is provided on the surface of the base film close to the positive electrode sheet, and a glue layer is provided on the surface of the heat-resistant layer away from the base film, that is, the structure of the diaphragm is glue layer + heat-resistant + base film + glue layer (the heat-resistant layer is close to the positive electrode sheet).
[0036] In some embodiments, the base film includes at least one of polyethylene PE, polypropylene PP, polyethylene terephthalate, polyimide, PE and PP composite structure. The heat-resistant layer includes one or more of aluminum oxide Al2O3, boehmite, aluminum hydroxide, magnesium oxide, aluminum oxide, zirconium oxide, titanium oxide and silicon oxide. The adhesive layer is a conventional spray-coated adhesive layer, for example, including one or more of polyvinylidene fluoride PVDF, polymethyl methacrylate PMMA, vinylidene fluoride-hexafluoropropylene copolymer, polyacrylic resin, polymethyl acrylate, butyl acrylate-acrylonitrile copolymer, polyacrylonitrile, ethylene-acrylic acid copolymer, polyethyl acrylate or sodium carboxymethyl cellulose, preferably PVDF, PMMA or PVDF mixed with PMMA.
[0037] The first solvent (linear organic matter of C1-C4, low viscosity solvent) generally has a smaller molecular structure. After the electrolyte contacts the diaphragm, the free first solvent molecules will diffuse into the polymer material of the diaphragm glue layer, causing the volume of the diaphragm glue layer to expand. As the first solvent molecules continue to enter, the movement of the polymer chain segments in the glue layer is enhanced, and finally the polymer material of the glue layer gradually enters the electrolyte, causing the glue layer to dissolve and fall off. Therefore, it is also necessary to control the lithium salt concentration in the electrolyte and the coverage of the glue layer to prevent the problem of the diaphragm glue layer being dissolved and falling off, and the following technical solutions are further proposed:
[0038] In the present invention, the electrolyte further includes a lithium salt; based on the total mass of the electrolyte, the mass proportion of the lithium salt is recorded as L; the electrolyte further includes a second solvent, and the second solvent includes a C1-C10 cyclic organic compound and / or a linear organic compound with a carbon number greater than 4; based on the total mass of the electrolyte, the mass proportion of the second solvent is recorded as S2; w, S1 and S2 satisfy: The value of can be, for example, 0.001, 0.005, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, preferably
[0039] In some embodiments, the mass proportion L of the lithium salt satisfies: 5%≤L≤25%, for example, it can be 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, preferably 8%≤L≤20%.
[0040] In some embodiments, the mass proportion S2 of the second solvent satisfies: 10%≤S2≤60%, for example, it may be 10%, 20%, 30%, 40%, 50%, or 60%.
[0041] When S1 and w satisfy When adjusting the lithium salt concentration, the coverage of the adhesive layer, and the mass ratio of the first solvent and the second solvent to meet When the mass ratio of the lithium salt and the mass ratio of the second solvent are adjusted to be within the above range, The larger the value, the harder it is for the glue layer to dissolve and fall off. A value that is too large will increase the impedance of the battery. The larger L is, the more lithium salt content in the electrolyte, the first solvent coordinates with the lithium ions to form a solvation structure, the fewer free first solvent molecules are, and the fewer solvent molecules enter the interior of the gel layer polymer, making it more difficult for the gel layer to dissolve and fall off. The larger the gel layer coverage w, the better the adhesion of the gel layer, the more difficult it is to dissolve, and the gel layer is not easy to fall off; but when L is too large, the anions will also enter the solvation structure of the lithium ions, causing the conductivity of the electrolyte to decrease. At the same time, when w is too large, the obstacle for lithium ions to pass through the diaphragm will increase, causing the impedance of the battery to increase and the fast charging performance to decrease; therefore, adjust to meet It can not only reduce the shedding of the diaphragm rubber layer, but also improve the fast charging performance of the battery.
[0042] In some embodiments, the lithium salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethylsulfonyl)imide. Adding the above lithium salt to the electrolyte can improve the ionic conductivity of the electrolyte, make the migration rate of lithium ions in the electrolyte faster, and improve the fast charging performance of the battery.
[0043] In some embodiments, the first solvent includes a C1-C4 linear organic substance, and the C1-C4 linear organic substance is a low-viscosity organic substance. The C1-C4 linear organic substance includes at least one or more of ethyl acetate EA (0.426 mPa.s), methyl propionate MP (0.416 mPa.s), propyl formate PF (0.419 mPa.s), methyl acetate MA (0.364 mPa.s), ethyl formate EF (0.358 mPa.s), methyl formate MF (0.328 mPa.s), ethyl methyl carbonate EMC (0.65 mPa.s), dimethyl carbonate DMC (0.58 mPa.s), ethylene glycol dimethyl ether (0.46 mPa.s), dimethanol formal DMM (0.33 mPa.s), and acetonitrile AN (0.35 mPa.s), preferably ethyl acetate. The lower the viscosity of the first solvent, the smaller the impedance of lithium ion transmission in the electrolyte liquid phase, which can reduce the lithium ion interface transmission impedance.
[0044] In some embodiments, the second solvent includes a C1-C10 cyclic organic matter and / or a linear organic matter with a carbon number greater than 4, and the second solvent is a high-viscosity organic matter, for example, the second solvent includes at least one or more of ethylene carbonate EC (1.9mPa.s 40°C), propylene carbonate PC (2.53mPa.s), butylene carbonate BC (3.2mPa.s), γ-butyrolactone (1.73mPa.s), diethyl carbonate DEC (0.748mPa.s), propyl propionate PP (0.68mPa.s), and ethyl propionate EP (0.502mPa.s). When the electrolyte includes a low-viscosity first solvent, the solvent is adjusted to include a high-viscosity second solvent, which can make the electrolyte more stable at the interface generated at the negative electrode, reduce the decomposition and gas production of the electrolyte, and reduce the expansion of the battery.
[0045] In some embodiments, the positive electrode sheet includes a positive current collector and a positive active material layer disposed on at least one side of the positive current collector, the positive active material layer includes a positive active material, a positive conductive agent and a positive binder, and the positive active material includes lithium iron phosphate. There is no limitation on the specific types of the positive current collector, the positive conductive agent and the positive binder, and they can be freely selected from the conductive agents used in the field of lithium batteries. For example, the positive current collector is aluminum foil or carbon-coated aluminum foil. The positive conductive agent includes at least one or more of carbon black, carbon nanotube acetylene black, carbon black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. For example, the positive binder includes at least one of polyvinylidene fluoride, sodium carboxymethyl cellulose, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyethylene oxide, and one or more of aluminate coupling agents.
[0046] In some embodiments, the positive electrode sheet includes a positive electrode active material, a conductive agent, and a binder, and the positive electrode active material includes lithium iron phosphate. The lithium iron phosphate includes at least two particles with different particle sizes.
[0047] In some embodiments, the lithium iron phosphate includes at least first particles with a Dv50 of 0.05 μm-1.0 μm and second particles with a Dv50 of 1 μm-10 μm. The Dv50 of the first particles may be, for example, 0.05 μm, 0.08 μm, 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, and the Dv50 of the first particles may be, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm. Preferably, the mass ratio of the first particles to the second particles is 1:(0.1-0.6), for example, 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6. When S1 and w satisfy When adjusting the blending of the first particles and the second particles in the positive electrode sheet and controlling the particle size and mass ratio of the two lithium iron phosphate particles within the above range, large and small particles are used in combination to shorten the solid phase transmission distance of lithium ions from the surface of the particles to the inside of the particles, and the positive electrode fast charging performance is better; the lithium iron phosphate secondary particles can avoid the compaction density of the positive electrode particle powder being too low, resulting in a decrease in the battery energy density, so that the first lithium iron phosphate and the lithium iron phosphate secondary particles are blended to take into account both the fast charging performance and the energy density of the battery.
[0048] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one side of the negative electrode current collector, and the negative electrode active material includes a negative electrode active material, a negative electrode conductive agent and a negative electrode binder. There is no limitation on the specific types of negative electrode active materials, negative electrode current collectors, negative electrode conductive agents and negative electrode binders, and they can be freely selected from the conductive agents used in the field of lithium batteries. For example, negative electrode active materials include natural graphite, artificial graphite, hard carbon and other negative electrode active materials that can support 2C and above rate performance. The negative electrode current collector includes copper foil. The negative electrode conductive agent includes at least one or more of superconducting carbon, acetylene black, carbon black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. The negative electrode binder includes at least one of polyacrylic acid, sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, polyimide, polyvinyl alcohol, polyimide, polyamide-imide, styrene-butadiene rubber and polyvinylidene fluoride.
[0049] In some embodiments, the surface density of the negative electrode sheet is 7 mg / cm 2 -13 mg / cm 2 (For example, 7 mg / cm 2 , 8mg / cm2 , 9mg / cm 2 、10mg / cm 2 、11mg / cm 2 , 12mg / cm 2 、13mg / cm 2 ), and / or the compaction density of the negative electrode is 1.4 mg / cm 3 -1.8mg / cm 3 (For example, 1.4 mg / cm 3 , 1.5mg / cm 3 、1.6mg / cm 3 , 1.7mg / cm 3 、1.8mg / cm 3 ). The greater the surface density and compaction density of the negative electrode sheet, the higher the energy density of the battery, but the internal resistance of the battery will increase, the transmission of lithium ions will be affected, and the fast charging performance of the battery will be worse. When S1 and w meet When the surface density and compaction density of the negative electrode sheet are adjusted within the above range, the energy density and fast charging performance of the battery can be taken into account.
[0050] In order to improve the fast charging performance of the battery, the amount of the first solvent added is usually relatively large. When the first solvent is used more in the electrolyte and the high-viscosity solvent accounts for a smaller proportion, the interface generated by the electrolyte at the negative electrode will be unstable, thereby causing the electrolyte to continue to decompose. Therefore, it is necessary to use an appropriate amount of additives. Therefore, the present invention further proposes a technical solution of adding cyclic carbonate additives and organic additives containing heteroatoms to the electrolyte.
[0051] In some embodiments, the electrolyte includes a first additive; based on the total mass of the electrolyte, the mass proportion of the first additive is 0.1%-8%, for example, 0.1%, 0.2%, 0.4%, 0.5%, 0.8%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%. Preferably, the first additive includes a cyclic carbonate additive, for example, one or more of vinylene carbonate VC, vinyl carbonate VEC, and fluoroethylene carbonate FEC. When S1 and w satisfy When the first additive is further added to the electrolyte and the amount added is adjusted within the above range, the stability of the battery negative electrode interface can be improved, the battery impedance can be reduced, and the cycle performance and capacity retention rate of the battery can be improved.
[0052] In some embodiments, the electrolyte includes a second additive; based on the total mass of the electrolyte, the mass proportion of the second additive is 0.1%-4%, for example, it can be 0.1%, 0.5%, 1.0%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%. Preferably, the second additive includes an organic additive containing a heteroatom, for example, including tris(trimethylsilyl)phosphate TMSP, tris(trimethylsilyl)borate TMSB, vinyl sulfate DTD, methylene disulfonate MMDS, 1,3-propane sultone PS, lithium difluorophosphate LiPO2F2, lithium bis(oxalatoborate) LiBOB, lithium difluorooxalatoborate LiODFB, lithium difluorobis(oxalatophosphate) LiODFP, lithium tetrafluoroborate LiBF4. When S1 and w satisfy When an organic additive containing heteroatoms is further added to the electrolyte and the amount added is adjusted within the above range, the kinetic performance of the battery can be improved, the battery impedance can be reduced, and the cycle performance of the battery can be improved.
[0053] In some embodiments, the above technical solution can improve the fast charging performance of the battery and prevent the dissolution of the diaphragm glue layer, but the use of low-viscosity solvents and diaphragms will cause the safety performance of the battery to decrease. This is because the low-viscosity solvent has a low boiling point, is easy to decompose, and the interface formed at the positive and negative electrodes is not stable enough, which increases the probability of the low-viscosity solvent decomposing at the positive and negative electrodes, causing the battery to produce gas, causing the battery to bulge, and in severe cases, the battery to explode; on the other hand, the surface of the diaphragm is not completely covered by the glue layer, and there is a risk of puncturing the diaphragm after lithium precipitation, increasing the risk of explosion after the battery short circuits. In order to reduce the risk of battery gas expansion and battery explosion after the diaphragm is punctured, the present invention further proposes the following technical solution:
[0054] In some embodiments, the battery includes a battery housing encapsulating the electrode assembly as an embodiment, the housing can be an aluminum housing, and an explosion-proof valve is provided on at least one side of the housing, and the explosion-proof valve can be located on the top cover, side, or bottom wall of the battery housing; the orthographic projection area of the explosion-proof valve on the housing is A mm 2 ; The explosion-proof valve includes an explosion-proof disc, the central thickness of the explosion-proof disc is thinner, and the circumferential edge (edge area) is thicker, and the central thickness of the explosion-proof disc is d5 mm (also called residual thickness); A, d5 and S1 meet: For example, it can be 2, 5, 10, 20, 50, 80, 100, 120, 150, 180, 200, 220, 250, preferably When S1 and w satisfy By controlling A, d5 and S1 to meet the above conditions, the safety of the battery can be further increased. When the use of low-viscosity solvents in the electrolyte increases, S1 increases. The value decreases, the gas generated by electrolyte decomposition increases, the interface generated by the low-viscosity solvent is not stable enough, the thermal runaway temperature of the battery decreases, and the probability of battery explosion increases; when the explosion-proof valve area A decreases and the residual thickness d5 increases, As the value decreases, the probability of battery explosion increases. When the value decreases, the probability of battery explosion increases, so the control The lower limit of the value is greater than 2, which reduces the risk of battery explosion. However, when the explosion-proof valve area A is too large and the residual thickness d5 is too small, the battery is easy to open during storage and transportation, increasing the risk of battery damage and reducing the safety performance of the battery. The larger the value, the lower the battery's fast charging performance. The value is within the above range, which can take into account both the fast charging performance and safety performance of the battery.
[0055] In some embodiments, A satisfies: 50 mm 2 ≤A≤2000mm 2 , for example, A can be 50mm 2 , 100mm 2 、300mm 2 , 500mm 2 , 800mm 2 , 1000mm 2 、1200mm 2 、1500mm 2 、1800mm 2 , 2000mm 2 The larger the orthographic projection area of the explosion-proof valve is, the more effectively it can reduce the risk of explosion. However, if A is too large, it will increase the risk of the explosion-proof valve opening. The explosion-proof valve will open even when the battery is not in thermal runaway, causing battery damage. When the explosion-proof valve area A is small, it is not easy for the electrolyte to spray out of the explosion-proof valve after the explosion-proof valve opens after thermal runaway, causing battery explosion. When it is controlled within the above range, it can improve both the safety performance of the battery and the process efficiency of the battery.
[0056] In some embodiments, d5 satisfies: 0.02mm≤d5≤0.2mm, for example, d can be 0.02mm, 0.04mm, 0.05mm, 0.08mm, 0.1mm, 0.12mm, 0.15mm, 0.18mm, 0.2mm. After the battery has thermal runaway, the residual thickness d5 will affect the explosion rate of the battery. When the residual thickness is too large, the explosion-proof valve is not easy to open, resulting in a direct explosion of the battery.
[0057] In some embodiments, Figure 1 and Figure 2As shown, the shell includes a shell 1, and the shell 1 includes a first side surface and a second side surface that are relatively arranged along the X-axis direction (i.e., the length direction of the shell), the first side surface is, for example, a top cover 2, and the second side surface is, for example, a bottom wall 7. As an embodiment, the top cover 2 can be provided with a positive pole column 3 and a negative pole column 4 at both ends along the first direction of the shell 1, and the top cover 2 is also provided with a liquid injection hole 5, and the liquid injection hole 5 is provided between the positive pole column 3 and the negative pole column 4. An explosion-proof valve 6 is provided in the central part of the bottom wall 7, and the explosion-proof valve 6 can also be provided on other side walls of the shell 1. The number of explosion-proof valves 6 can be selected and adjusted according to the gas production and voltage of the battery. As an embodiment, when at least two explosion-proof valves 6 are provided, they can be provided on the bottom wall 7 and other side walls.
[0058] In some embodiments, the explosion-proof disk has a shape including circular, elliptical, racetrack, square, triangular or rectangular, etc. The explosion-proof valve can be formed by welding or stamping.
[0059] In some embodiments, the explosion-proof plate includes a middle area and an edge area surrounding the middle area, and the thickness of the middle area is smaller than that of the edge area, thereby ensuring the stability of the connection between the explosion-proof valve and the shell, so that the explosion-proof valve is not easy to explode under lower battery pressure.
[0060] In some embodiments, the explosion-proof sheet comprises a notched groove. The notched groove comprises a V-shaped groove, a trapezoidal groove, a rectangular groove, a circular groove or an elliptical groove, and the specific shape of the notched groove is not limited. The notched groove comprises a plurality of notches arranged at intervals, and the interval distance is not limited. Preferably, the intervals are evenly distributed so that the notched grooves are subjected to a relatively uniform force, so that the explosion-proof sheet and the battery housing are not completely separated when the explosion-proof valve is opened.
[0061] In some embodiments, Figure 2 , Figure 4 and Figure 5 As shown, the central part of the bottom wall 7 is provided with an explosion-proof valve 6, which includes an explosion-proof sheet 61. The explosion-proof sheet 61 is in a runway shape, and the thickness of the center (middle area) of the explosion-proof sheet 61 is relatively thin, and the circumferential edge (edge area) is relatively thick. The explosion-proof sheet 61 is provided with a runway-shaped notched groove 62 at the junction of the middle area and the edge area, and the end of the notched groove 62 is not connected, so that when the explosion-proof valve is opened, it is opened from one side, and the explosion-proof sheet 61 will not be separated from the battery housing 1 when it is torn along the notched groove 62. If the end of the notched groove 62 is connected, when the explosion-proof valve is opened, the notched groove will be evenly stressed, and the explosion-proof sheet will be completely separated and easily ejected.
[0062] In some embodiments, the housing satisfies at least one of the following conditions:
[0063] (i) The thickness d1 of the battery shell satisfies: 20mm≤d1≤100mm. The thickness d1 of the battery shell refers to the shell thickness of the side with smaller area except the side with the largest area. For example, d1 can be 20mm, 25mm, 30mm, 35mm, 40mm, 45mm, 50mm, 55mm, 58mm, 60mm, 70mm, 80mm, 90mm, 100mm;
[0064] (ii) the width d2 of the battery housing satisfies: 50 mm ≤ d2 ≤ 400 mm, for example, d2 can be 50 mm, 100 mm, 120 mm, 140 mm, 160 mm, 180 mm, 200 mm, 220 mm, 240 mm, 260 mm, 280 mm, 300 mm, 320 mm, 350 mm, 380 mm, 400 mm;
[0065] (iii) the height d3 of the battery housing satisfies: 50 mm ≤ d3 ≤ 300 mm, for example, d3 can be 50 mm, 100 mm, 120 mm, 140 mm, 160 mm, 180 mm, 200 mm, 220 mm, 240 mm, 260 mm, 280 mm, or 300 mm;
[0066] (iv) The shell thickness d4 of the side with the largest area in the battery shell satisfies: 0.2 mm≤d1≤3 mm. For example, d4 can be 0.2 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.8 mm, 1.0 mm, 1.2 mm, 1.5 mm, 1.6 mm, 1.8 mm, 2.0 mm, 2.2 mm, 2.5 mm, 2.8 mm, or 3 mm.
[0067] The smaller the shell thickness d4 of the largest side of the battery shell, the faster the heat diffuses from the inside of the battery to the outside, preventing heat accumulation, which is beneficial to reducing the temperature rise of the battery during fast charging; the larger the thickness d1 of the battery shell, the greater the heat accumulation of the battery and the higher the temperature rise; the larger the battery shell width d2 and the battery shell height d3, the larger the shell area of the battery, the faster the heat transfer and the smaller the temperature rise. When S1 and w meet When the parameters of the battery casing are adjusted within the above range, heat can be conducted quickly to prevent heat accumulation, which is beneficial to reducing the temperature rise of the battery during fast charging, reducing safety problems caused by battery overheating, and improving the safety performance of the battery.
[0068] In some embodiments, Figure 1 , Figure 3As shown, the shell 1 is surrounded by six rectangular surfaces, wherein along the Y-axis direction, two oppositely disposed rectangular surfaces with the largest area are recorded as the third side surface 11 and the fourth side surface 12, the shell thickness of the third side surface 11 and the fourth side surface 12 are both d4, and the shell thickness of the remaining side surfaces is d1, and d2 is less than d1. The distance of the shell 1 along the Y-axis direction is recorded as the width of the shell, represented by d2; the distance of the shell 1 along the Z-axis direction is recorded as the height of the shell, represented by d3.
[0069] In some embodiments, a diaphragm is provided on the surface of the electrode assembly close to the battery casing. After thermal runaway of the battery occurs, the explosion-proof valve opens. To ensure that the electrolyte can flow out of the explosion-proof valve smoothly, a diaphragm is provided on the surface of the electrode assembly close to the battery casing (the battery structure adopts the form of an outsourced diaphragm). When the explosion-proof valve is opened, the electrolyte is discharged through the diaphragm diversion. Moreover, the diaphragm outsourcing structure can further prevent the stacked core from contacting the metal aluminum shell and causing a short circuit, thereby increasing the safety performance of the battery. However, the stacked core may cause the diaphragm to wrinkle when entering the shell, and the pole piece will still contact the metal aluminum shell and cause a short circuit. In order to prevent the pole piece from contacting the metal shell and reduce the risk of battery short circuit, the following technical scheme is further proposed:
[0070] In some embodiments, the outside of the electrode assembly is at least partially wrapped with insulating tape, for example, the insulating tape includes at least one of masking tape, fiber tape, PACK high-temperature tape, PET tape, and acrylic tape. When the battery is fast charged, when the electrode assembly generates excessive current, the temperature of the battery is high, and the insulating tape can withstand high temperatures to prevent short circuit problems caused by heat accumulation, while preventing the electrode assembly from contacting the metal shell, reducing the risk of battery short circuit.
[0071] In some embodiments, the surface of the insulating tape away from the electrode assembly is provided with a Mylar film, which forms a physical isolation layer inside the battery, thereby preventing the battery from short circuiting and leaking electricity and improving the safety performance of the battery.
[0072] In some embodiments, Figure 6 As shown, the positive electrode sheet 8, the separator 9 and the negative electrode sheet 10 are stacked and wound to form a winding core, and the separator 9 is extended to wrap the positive electrode sheet 8 and the negative electrode sheet 10. The surface of the separator 9 on the outermost layer of the electrode assembly is provided with an insulating tape 11, and the insulating tape 11 is provided at least on the largest side of the electrode assembly (corresponding to the third side 11 and the fourth side 12 of the shell). Figure 7 As shown, a Mylar film 12 is provided on the surface of the insulating tape 11 away from the electrode assembly.
[0073] In some embodiments, the Mylar film satisfies at least one of the following conditions:
[0074] (a) The thickness of a single layer of Mylar film is d6. The Mylar film may have folded and overlapped areas. The total thickness of the Mylar film in the overlapped area is the sum of the thickness of each single layer of Mylar film; d6 satisfies: 0.03mm≤d6≤0.3mm, for example, d6 can be 0.03mm, 0.05mm, 0.08mm, 0.1mm, 0.15mm, 0.2mm, 0.25mm, 0.3mm, preferably 0.05mm≤d6≤0.15mm; the thicker the single layer of Mylar film, the higher the tensile strength, and it will not be easily damaged during the process of stacking the core into the shell. At the same time, it is not easy to be damaged during the use and movement of the battery, and effectively prevents the pole piece from contacting the metal shell; however, if the single layer of Mylar film is too thick, the mass will increase, and the energy density of the battery will decrease. If the Mylar film is too thin, it will easily break when the core is stacked into the shell. When the single layer thickness of the Mylar film is within the above range, it is guaranteed that the battery has good safety performance.
[0075] (b) The Mylar membrane includes a plurality of holes, the diameter of which is 1-5 mm, for example, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm; the shape of the holes includes any form such as circle, square, rectangle, triangle, etc. As an embodiment, the Mylar membrane is provided with holes on the side corresponding to the explosion-proof valve. When the diameter of the holes in the Mylar membrane is within the above range, it is conducive to the flow of electrolyte. When the explosion-proof valve is opened, the electrolyte can flow out from these holes, reducing the risk of battery explosion.
[0076] (c) The tensile strength of the Mylar film is 20 MPa-100 MPa, for example, 20 MPa, 30 MPa, 40 MPa, 50 MPa, 60 MPa, 70 MPa, 80 MPa, 90 MPa, 100 MPa. If the tensile strength of the Mylar film is too low, the Mylar film will be easily broken when entering the square shell, affecting the insulation performance of the electrode assembly and easily causing battery failure. The tensile strength of the Mylar film refers to the tensile test method for metal materials in GB / T228.1-2010.
[0077] In some embodiments, the battery is a lithium-ion secondary battery.
[0078] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0079] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0080] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.
[0081] The batteries of the examples and comparative examples of the present invention were prepared according to the following preparation method, and the differences from Example 1-1 are shown below.
[0082] Example 1-1
[0083] (1) Preparation of positive electrode sheet
[0084] Lithium iron phosphate powder (first particles and second particles with different particle sizes are mixed, and the mass ratio of the first particles to the second particles is 7:3), polyvinylidene fluoride, acetylene black, and carbon nanotubes are put into a vacuum mixer according to a mass ratio of 96:2:1.5:0.5, and N-methylpyrrolidone (NMP) is added. The mixture is fully mixed under the action of the vacuum mixer until a uniform and fluid positive electrode slurry is formed, wherein the solid content is 55wt%; the positive electrode slurry is evenly coated on a carbon-coated aluminum foil with a thickness of 12μm, and the coating single-side surface density is 17mg / cm 2 , drying, rolling, slitting and punching to obtain the positive electrode sheet.
[0085] (2) Preparation of negative electrode sheet
[0086] Graphite, styrene-butadiene rubber, sodium carboxymethyl cellulose and acetylene black were put into a vacuum mixer in a mass ratio of 96.5:1:1:1.5, and deionized water was added. The mixture was fully mixed under the action of the vacuum mixer to finally form a uniform and fluid negative electrode slurry with a solid content of 45wt%. The negative electrode slurry was evenly coated on a copper foil with a thickness of 6μm, dried, rolled and die-cut to obtain a negative electrode sheet with a surface density of 9.5mg / cm 2 , and / or the compaction density of the negative electrode is 1.6 g / cm 3 .
[0087] (3) Preparation of electrolyte
[0088] In an argon glove box with a water content of <0.1ppm and an oxygen content of <0.1ppm, ethylene carbonate (EC), ethyl methyl carbonate (EMC) and ethyl acetate (EA) are mixed evenly, and fully dried lithium hexafluorophosphate (LiPF6) and bis(fluorosulfonyl)imide lithium salt LiFSI are added thereto for stirring and dissolution. The mass of LiPF6 and LiFSI added is 10% and 5% of the total mass of the electrolyte. 4% of vinylene carbonate based on the total mass of the electrolyte is added, 1.0% of vinyl sulfate based on the total mass of the electrolyte is added, and 1.0% of lithium difluorophosphate LiPO2F2 based on the total mass of the electrolyte is added. The mixture is stirred evenly. The first solvent EA and EMC (the mass ratio of the two is 4:1) account for 40% of the mass of the electrolyte, and the second solvent EC accounts for 35% of the mass of the electrolyte. After passing the physical property test, the electrolyte is obtained.
[0089] (4) Preparation of batteries
[0090] The positive electrode sheet obtained in step (2), the negative electrode sheet obtained in step (3) and the separator (the structure of the separator is glue layer + heat-resistant layer + base film + glue layer, the glue coating layer is PVDF, and the positive electrode side of the separator contains Al2O3) are wound to obtain a bare battery cell. In the last winding, the separator is extended to wrap the core to achieve the outer packaging of the separator; the core is then wrapped with insulating adhesive paper to prevent the core from contacting the shell; then the two bare battery cells are welded to the upper ears, and the core is wrapped with Mylar film, and finally placed in a battery shell (the thickness d1 of the battery shell is 50 mm, the width d2 of the battery shell is 208 mm, and the height d3 of the battery shell is 102 mm). The bottom wall of the battery shell is provided with an explosion-proof valve, and the positive projection area of the explosion-proof valve on the shell is 1000 mm 2 The central thickness of the explosion-proof plate is d5, which is 0.1 mm. The electrolyte prepared in step (3) is injected into the dried and qualified battery cell, and the battery is obtained through the processes of standing, aging, formation, exhaust, aging, and sorting.
[0091] (5) Test battery
[0092] Electrochemical performance test: The electrochemical performance test is carried out using the following test methods using a Blue Electric charge and discharge test cabinet:
[0093] (5.1) Fast charging cycle performance test
[0094] Fast charge cycle performance test: At 25°C, use a vernier caliper to measure the thickness d1 of the battery before the cycle, charge the divided battery to 3.65V at 1C constant current and constant voltage, with a cut-off current of 0.05C, and then discharge it to 2.5V at 1C constant current, and record the initial discharge capacity C0. Then charge the battery to 20% SOC at 1C, then charge it to 80% SOC at 5C, and finally charge it to 100% SOC at 1C constant current and constant voltage, with a cut-off current of 0.05C, and then discharge it to 2.5V at 1C constant current, and repeat this cycle. After 1000 cycles of charge and discharge, calculate the capacity retention rate at the 1000th week, and record the battery thermal thickness d2 at the same time. The calculation formula is as follows:
[0095] 1000th cycle capacity retention rate (%) = (1000th cycle discharge capacity / first cycle discharge capacity) × 100%.
[0096] The battery expansion rate at the 1000th cycle (%) = (battery thickness d2 at the 1000th cycle / battery thickness d1 before the cycle) × 100%.
[0097] (5.2) Diaphragm adhesive layer peeling test
[0098] At 25°C, the divided battery is charged to 3.65V at 1C constant current and constant voltage, with a cut-off current of 0.05C, so that the battery maintains 100% SOC state, and then the battery is discharged to 50% SOC at 1C constant current. In the half-charged state, the battery is placed in an environment of 80°C for 5 hours, after which the battery is dissected and the diaphragm is removed, the diaphragm is rinsed with ethanol, and then observed with a scanning electron microscope. Compared with the fresh diaphragm, the surface of the treated diaphragm is observed with a scanning electron microscope to see whether the glue layer falls off, and the records are no fall off, slight fall off, fall off, and severe fall off.
[0099] (5.3) Safety testing
[0100] At 25°C, the divided battery is charged to 3.65V at 1C constant current and constant voltage, with a cut-off current of 0.05C, to keep the battery in 100% SOC state. The fully charged battery is subjected to a heating experiment, and two metal heating rods are used to heat the two large surfaces of the battery. A temperature sensor is used to record the temperature at the explosion-proof valve position, which represents the battery temperature. The metal rod heating temperature is set to 5°C / min until the battery explosion-proof valve opens or an explosion occurs. 500 batteries are tested as above and the explosion rate of the battery is calculated.
[0101] Referring to Example 1-1, S1, S2, w and L were adjusted in Example 1, Example 2 and Comparative Examples 1 and 2 to change the value of S1 / w; the first solvent content S1 was changed in Example 3; the first solvent content S2 was changed in Example 4; the membrane glue layer coverage w was changed in Example 5; and the lithium salt content L was changed in Example 6. The details are shown in Table 1.
[0102] Table 1
[0103]
[0104]
[0105] The test data of Example Groups 1 to 6 and Comparative Examples 1 and 2 are shown in Table 2.
[0106] Table 2
[0107]
[0108] It can be seen from Table 2 that as the S1 / W value increases, the lithium ion transmission between the positive and negative electrodes becomes faster, and the fast charging performance of the battery becomes better. However, the greater the battery expansion, the more severe the glue layer falls off, and the greater the explosion rate. The larger the L / w, the less likely the glue layer will fall off. The more low-viscosity solvents there are, the better the fast charging performance of the battery. However, the greater the expansion, the easier it is for the glue layer to fall off, and the higher the explosion rate. The more high-viscosity solvents there are, the worse the fast charging performance of the battery, the smaller the capacity retention rate, and the smaller the expansion; the more glue layers there are, the worse the fast charging performance, and the better the battery safety; the higher the lithium salt content, the less likely the glue layer will fall off. The battery provided by the present invention, through the control of the solvent and the coverage rate of the diaphragm glue layer, the mass proportion S1 of the linear organic matter of C1-C4 and the coverage rate of the diaphragm glue layer satisfy Improved the fast charging cycle performance of the battery.
[0109] Referring to Example 1-1, in Example 7, S1, A and d5 were adjusted to change the value of A / (S1*d5*1000), in Example 8, the explosion-proof valve projection area A was changed, and in Example 9, the residual thickness d5 was changed. The details are shown in Table 3.
[0110] Table 3
[0111]
[0112] Example 10 group was carried out with reference to Example 1-1. In Example 1-1, the thickness d6 of the Mylar film was 0.1 mm, in Example 10-1, the thickness d6 of the Mylar film was 0.05 mm, and in Example 10-2, the thickness d6 of the Mylar film was 0.15 mm.
[0113] The test data of Example 7-10 groups are shown in Table 4.
[0114] Table 4
[0115]
[0116] It can be seen from Table 4 that the larger the value of A / (S1*d5*1000), the smaller the explosion rate of the battery; the larger the area of the explosion-proof valve, the better the safety and the lower the explosion rate; the smaller the residual thickness, the smaller the explosion rate of the battery; the thicker the Mylar film, the better the battery safety. In the battery of the present invention, A, d5 and S1 are controlled to meet the requirements. It can take into account both the fast charging performance and safety performance of the battery.
[0117] Example 11 was carried out in accordance with Example 1-1, with the differences shown in Table 5 below.
[0118] Table 5
[0119]
[0120] It can be seen from Table 5 that when only the first particles with a smaller particle size are used in the battery, the electrolyte decomposes severely, the battery swells severely, and the capacity decays rapidly; when only the second particles with a larger particle size are used, the fast charging performance is poor and the battery produces large gas expansion.
[0121] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.
[0122] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A battery, characterized in that: The invention comprises an electrode assembly, wherein the electrode assembly comprises a positive electrode sheet, a separator and a negative electrode sheet which are stacked; The battery includes an electrolyte, the electrolyte includes a first solvent, and the first solvent includes a C1-C4 linear organic matter; the mass proportion of the first solvent is recorded as S1 based on the total mass of the electrolyte; The diaphragm comprises a base film, and a glue layer is provided on at least one side of the base film; the coverage of the glue layer on the base film is denoted as w; S1 and w satisfy:
2. The battery according to claim 1, characterized in that S1 and w satisfy: Preferably, the mass proportion S1 of the first solvent satisfies: 5%≤S1≤70%; Preferably, the coverage w of the adhesive layer on the base film satisfies: 10%≤w≤90%; Preferably, the separator comprises a base film, a surface of the base film close to the negative electrode sheet is provided with a glue layer, a surface of the base film close to the positive electrode sheet is provided with a heat-resistant layer, and a surface of the heat-resistant layer away from the base film is provided with a glue layer; Preferably, the adhesive layer includes one or more of polyvinylidene fluoride, polymethyl methacrylate, vinylidene fluoride-hexafluoropropylene copolymer, polyacrylic resin, polymethyl acrylate, butyl acrylate-acrylonitrile copolymer, polyacrylonitrile, ethylene-acrylic acid copolymer, polyethyl acrylate or sodium carboxymethyl cellulose.
3. The battery according to claim 1, characterized in that The electrolyte further includes a lithium salt; based on the total mass of the electrolyte, the mass proportion of the lithium salt is denoted as L; The electrolyte further includes a second solvent, the second solvent includes a C1-C10 cyclic organic compound and / or a linear organic compound with a carbon number greater than 4; the mass proportion of the second solvent is recorded as S2 based on the total mass of the electrolyte; L, w, S1 and S2 satisfy: Preferably, the mass proportion L of the lithium salt satisfies: 5%≤L≤25%; Preferably, the mass proportion S2 of the second solvent satisfies: 10%≤S2≤60%.
4. The battery according to claim 3, characterized in that The first solvent comprises at least one or more of ethyl acetate, methyl propionate, propyl formate, methyl acetate, ethyl formate, methyl formate, ethyl methyl carbonate, dimethyl carbonate, ethylene glycol dimethyl ether, dimethanol formal, and acetonitrile, preferably ethyl acetate; Preferably, the second solvent includes at least one or more of ethylene carbonate, propylene carbonate, butylene carbonate, γ-butyrolactone, diethyl carbonate, propyl propionate, and ethyl propionate.
5. The battery according to claim 1, characterized in that The positive electrode sheet comprises a positive electrode active material, a conductive agent and a binder, wherein the positive electrode active material comprises lithium iron phosphate; the lithium iron phosphate comprises at least two particles with different particle sizes; Preferably, the lithium iron phosphate comprises at least first particles with a Dv50 of 0.05 μm-1.0 μm and second particles with a Dv50 of 1 μm-10 μm; Preferably, the mass ratio of the first particles to the second particles is 1:(0.1-0.6); Preferably, the surface density of the negative electrode sheet is 7 mg / cm 2 -13 mg / cm 2 , and / or the compaction density of the negative electrode is 1.4 mg / cm 3 -1.8mg / cm 3 .
6. The battery according to any one of claims 1 to 5, characterized in that: The electrolyte includes a first additive; based on the total mass of the electrolyte, the mass proportion of the first additive is 0.1%-8%; preferably, the first additive includes one or more of vinylene carbonate, vinyl carbonate, and fluoroethylene carbonate; Preferably, the electrolyte includes a second additive; based on the total mass of the electrolyte, the mass proportion of the second additive is 0.1%-4%; preferably, the second additive includes one or more of tris(trimethylsilyl)phosphate, tris(trimethylsilyl)borate, vinyl sulfate, methanedisulfonic acid methylene ester, 1,3-propane sultone, lithium difluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), and lithium tetrafluoroborate.
7. The battery according to any one of claims 1 to 5, characterized in that: The battery comprises a shell encapsulating the electrode assembly, and an explosion-proof valve is provided on at least one side of the shell, and the orthographic projection area of the explosion-proof valve on the shell is Amm 2 ; The explosion-proof valve includes an explosion-proof disk, and the central thickness of the explosion-proof disk is d5 mm; A, d5 and S1 satisfy: Best Preferably, A satisfies: 50 mm 2 ≤A≤2000mm 2 ; and / or, d5 satisfies: 0.02mm≤d5≤0.2mm.
8. The battery according to claim 7, characterized in that The housing satisfies at least one of the following conditions: (i) The thickness d1 of the battery casing satisfies: 20 mm ≤ d1 ≤ 100 mm; (ii) The width d2 of the battery housing satisfies: 50 mm ≤ d2 ≤ 400 mm; (iii) The height d3 of the battery housing satisfies: 50 mm ≤ d3 ≤ 300 mm; (iv) The shell thickness d4 of the side with the largest area in the battery shell satisfies: 0.2 mm ≤ d4 ≤ 3 mm.
9. The battery according to claim 7, characterized in that A diaphragm is provided on the surface of the electrode assembly close to the battery housing; Preferably, the outside of the electrode assembly is at least partially wrapped with insulating tape; Preferably, a Mylar film is provided on the surface of the insulating tape away from the electrode assembly.
10. The battery according to claim 9, characterized in that The Mylar film satisfies at least one of the following conditions: (a) The thickness of the Mylar film is d6, and d6 satisfies: 0.03mm≤d6≤0.3mm; (b) the Mylar membrane comprises a plurality of holes, wherein the hole diameter is 1 mm to 5 mm; (c) The tensile strength of Mylar film is 20MPa-100MPa.