Diaphragm and preparation method thereof
By using a heat-resistant layer composed of polymer fibers and inorganic ceramic particles in the separator to regulate the pore structure, the problems of heat shrinkage and coating peeling in traditional polyolefin separators at high temperatures are solved, and the membrane rupture temperature and thermal safety of the separator are improved performance.
Patent Information
- Application Number
- CN202411236974.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional polyolefin membranes are prone to heat shrinkage and cracking at high temperatures. The adhesive dissolution after ceramic particles are applied, causing the coating to fall off, resulting in poor flatness of the membrane and insufficient thermal safety performance.
Polymer fibers and inorganic ceramic particles are used to form a heat-resistant layer. By regulating the pore structure of the substrate layer and the heat-resistant layer, the membrane rupture temperature and longitudinal elastic modulus of the membrane are improved, the curling rate and powder loss are reduced, and the thermal safety performance is enhanced. .
The rupture temperature of the diaphragm is increased, the curling and powder loss problems are reduced, the thermal safety performance is improved, and the stability and flatness of the diaphragm under high temperature and external forces are ensured.
Smart Images

Figure CN119069954A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to a diaphragm and a method for preparing the same. Background Art
[0002] Diaphragm is an important component of secondary battery, which is mainly used to separate positive electrode and negative electrode to prevent internal short circuit of secondary battery. Traditional diaphragm mainly adopts polyolefin porous film, such as single-layer film or multi-layer composite film of polyethylene (PE) and polypropylene (PP). However, the melting point of polyolefin diaphragm is low, and severe thermal shrinkage or even film breakage will occur when the temperature is too high, resulting in thermal shrinkage and close contact between the positive and negative electrodes, further leading to internal short circuit, fire and even explosion. In the prior art, there is a polyolefin porous film coated with ceramic particles to solve the thermal shrinkage problem of polyolefin porous film, but the simple ceramic particle coating, because the ceramic particles are small, needs to be fixed to each other by acrylic adhesive, and the adhesive will dissolve during the heating process, causing the ceramic particles to fall off from the polyolefin porous film, resulting in the fragmentation of the coating film.
[0003] In the prior art, polymer materials such as aramid and polyimide can also be used as coating materials. When used as a coating together with ceramic particles, they can improve the heat resistance, wettability and oxidation resistance of the polyolefin diaphragm. However, the molecular chain of the above-mentioned polymer material is relatively rigid, and the thermal expansion coefficient between it and the polyolefin porous membrane is quite different. It is difficult to release the stress in time during the drying process, which leads to curling of the diaphragm. At the same time, the longitudinal strength of the coated diaphragm is low and the elongation is large, which makes it very easy to over-stretch, further increasing the internal stress of the finished diaphragm, resulting in undesirable phenomena such as rib bursting during the aging process. Due to the high rigidity of the coating and the low elongation at break, when used in batteries, if the coating falls off the polyolefin porous membrane when the wound battery is hit by external force, the ceramic particles in the coating are hard and can easily puncture the diaphragm and cause a short circuit in the battery.
[0004] Therefore, it is urgent to find a new solution to solve the problem of poor flatness of the diaphragm caused by excessive stretching during the diaphragm coating process, while inhibiting the coating from falling off the surface of the base film and improving the thermal safety performance of the diaphragm. Summary of the invention
[0005] The purpose of this application is to provide a diaphragm and a preparation method thereof, so as to increase the rupture temperature of the diaphragm, reduce the curling rate of the diaphragm, improve the powder loss phenomenon of the diaphragm, and enhance the thermal safety performance of the diaphragm. The specific technical scheme is as follows:
[0006] The first aspect of the present application provides a diaphragm, which comprises a substrate layer and a heat-resistant layer located on at least one surface of the substrate layer, wherein the substrate layer comprises polyolefin, and the heat-resistant layer comprises polymer fibers and inorganic ceramic particles; the diaphragm satisfies:
[0007] 1≤B L50 / B W50 ≤6, 0.1μm≤B L 50≤0.6μm, 0.04μm≤T L 50≤0.2μm;
[0008] Among them, B W50 is the average length of the pores in the substrate layer along the thickness direction in the longitudinal section, B L50 T is the average length of the pores in the longitudinal section of the substrate layer in a direction perpendicular to the section thickness; W50 is the average length of the pores in the heat-resistant layer in the longitudinal section along the thickness direction of the section, T L50 It is the average length of the pores in the longitudinal section of the heat-resistant layer in a direction perpendicular to the section thickness.
[0009] In some embodiments, 0.5≤T L50 / T W50 ≤4.
[0010] In some embodiments, the polymer fibers have an average diameter of 10-80 nm.
[0011] In some embodiments, the polymer is selected from at least one of para-aramid, meta-aramid, and polyimide.
[0012] In some embodiments, the polyolefin is selected from one or more copolymers or blends of polyethylene, polypropylene, polybutene, and poly-4-methylpentene, and the weight average molecular weight of the polyolefin is 100,000-3,000,000, preferably 100,000-2,400,000.
[0013] In some embodiments, the material of the inorganic ceramic particles is selected from at least one of alumina, silica, boehmite, magnesium hydroxide, titanium dioxide, barium sulfate, and barium titanate.
[0014] In some embodiments, the inorganic ceramic particles include at least one of nano inorganic ceramic particles and micro nano inorganic ceramic particles, the Dv50 of the nano inorganic ceramic particles is D1, 0.01μm≤D1≤0.1μm, and the Dv50 of the micro nano inorganic ceramic particles is D2, 0.1μm<D2≤2μm; preferably, the inorganic ceramic particles include nano inorganic ceramic particles and micro nano inorganic ceramic particles, and the mass ratio H of the nano inorganic ceramic particles to the micro nano inorganic ceramic particles is (1-8):1.
[0015] In some embodiments, based on the total mass of the heat-resistant layer, the mass percentage M1 of the polymer fiber is 30-70%, and the mass percentage M2 of the inorganic ceramic particles is 30-70%; the mass percentage of the polymer fibers on the surface of the heat-resistant layer is greater than the mass percentage of the inorganic ceramic particles on the surface of the heat-resistant layer.
[0016] In some embodiments, the substrate layer has a thickness of 5-16 μm.
[0017] In some embodiments, the separator has a thickness of 10-18 μm.
[0018] In some embodiments, the elastic modulus of the separator in a longitudinal direction (MD) is greater than the elastic modulus in a transverse direction (TD), and the elastic modulus of the separator in a longitudinal direction is ≥2500 MPa.
[0019] In some embodiments, the longitudinal elongation at break of the separator is less than the transverse elongation at break, and the longitudinal elongation at break of the separator is 5-100%; the transverse elongation at break of the separator is 25-170%.
[0020] In some embodiments, the membrane has a transverse curl of ≤15%.
[0021] In some embodiments, the rupture temperature of the membrane is ≥ 250°C.
[0022] In some embodiments, the air permeability per unit thickness of the heat-resistant layer is 15-45s / 100cc / μm.
[0023] The second aspect of the present application provides a method for preparing the diaphragm provided in the first aspect of the present application, which comprises the following steps:
[0024] 1) mixing polyolefin and porogen, kneading and extruding to prepare a cast sheet;
[0025] 2) stretching the cast sheet, wherein the temperature of the cast sheet is 120-140° C. during stretching, and the temperature difference between different points in the temperature field of the stretching region is less than 0.5° C., and an oil film is obtained after stretching, wherein the stretching includes a first longitudinal stretching and a first transverse stretching;
[0026] 3) extracting and drying the oil film, and then expanding and heat-setting to obtain the substrate layer, wherein the expanding includes a second longitudinal stretching and a second transverse stretching;
[0027] 4) coating the polymer coating liquid on at least one surface of the substrate layer, and obtaining the diaphragm through coagulation, water washing and drying;
[0028] Among them, the stretching ratio product L1 of the first longitudinal stretching and the second longitudinal stretching is 5.5-14, the stretching ratio product L2 of the first transverse stretching and the second transverse stretching is 1-6.5, and L1>L2; based on the total mass of the polymer coating liquid, the mass percentage of the polymer fiber is 2-10%.
[0029] In some embodiments, the maximum tension F used in the entire production line during the coating process in step 4) satisfies: Where E B is the longitudinal elastic modulus of the substrate layer, D is the thickness of the substrate layer, W is the width of the substrate layer, E B ≥2500MPa, D is 0.005-0.016mm, W is 500-1100mm.
[0030] In some embodiments, the solidification method in step 4) is selected from solidification bath solidification or constant temperature and humidity solidification;
[0031] The solvent for solidification by coagulation bath includes a first organic solvent and a poor solvent. Based on the total mass of the solvent for solidification by coagulation bath, the mass percentage content P1 of the first organic solvent is 45-75%, and the mass percentage content P2 of the poor solvent is 25-55%; the first organic solvent is selected from at least one of N-methylpyrrolidone (NMP), N,N-dimethylacetamide, and dimethyl sulfoxide, and the poor solvent is selected from at least one of water, ethanol, methanol, ethylene glycol, and tripropylene glycol;
[0032] The constant temperature and humidity curing includes a curing temperature of 40-70° C., a curing humidity of 55-85%, and a curing time of 3-30 seconds.
[0033] In some embodiments, the polymer is selected from at least one of para-aramid and meta-aramid, and the steps of preparing the polymer coating liquid include: in a nitrogen environment at normal pressure, adjusting the temperature to 1-10° C., mixing and stirring the polymer glue and inorganic ceramic particles, and then adding a second organic solvent containing a co-solvent concentration of 2-10wt%, stirring and mixing to obtain the polymer coating liquid;
[0034] The polymer glue comprises polymer fibers, chloride ions and a third organic solvent. Based on the total mass of the polymer glue, the mass percentage W1 of the polymer fibers is 2-10%, and the mass percentage W2 of the chloride ions is 0.5-10%. The rotational viscosity of the polymer glue is 3000-200000 mPa·s, and the logarithmic viscosity is 1-3 dL / g. The mass ratio of the polymer fibers to the inorganic ceramic particles is (30-70): (70-30), and the co-solvent is selected from at least one of CaCl2, KOH, LiCl, and pyridine.
[0035] Or, the polymer is selected from polyimide, and the preparation steps of the polymer coating liquid include: in a nitrogen environment at normal pressure, the temperature is adjusted to 1-10°C, the polymer glue and the inorganic ceramic particles are mixed and stirred, and then a second organic solvent is added, and the mixture is stirred and mixed uniformly to obtain the polymer coating liquid; wherein the polymer glue comprises polymer fibers and a third organic solvent, and based on the total mass of the polymer glue, the mass percentage content W1 of the polymer fiber is 2-10%; the rotational viscosity of the polymer glue is 3000-200000mpa·s, the logarithmic viscosity is 1-3dL / g, and the mass ratio of the polymer fiber to the inorganic ceramic particles is (30-70): (70-30);
[0036] The second organic solvent and the third organic solvent are each independently selected from at least one of N-methylpyrrolidone, N,N-dimethylformamide, acetone, and N,N-dimethylacetamide.
[0037] In some embodiments, the mass ratio of the polyolefin to the porogen is 1:(2-5).
[0038] The present application provides a diaphragm and a preparation method thereof, wherein the diaphragm comprises a substrate layer and a heat-resistant layer located on at least one surface of the substrate layer, wherein the substrate layer comprises polyolefin, and the heat-resistant layer comprises polymer fibers and inorganic ceramic particles; the diaphragm satisfies: 1≤B L50 / B W50 ≤6, 0.1μm≤B L 50≤0.6μm, 0.04μm≤T L 50≤0.2μm. This application reduces the rigidity difference between the heat-resistant layer and the substrate layer by regulating the size of the internal structural pores of the substrate layer and the heat-resistant layer, thereby increasing the membrane breaking temperature of the diaphragm and alleviating the problem of the diaphragm being easily broken during long-term high-temperature treatment. At the same time, it greatly reduces the diaphragm curling phenomenon that is prone to occur after the heat-resistant layer is coated, and improves the problem of powder loss that is prone to occur when the diaphragm is stretched or impacted by the outside world, thereby improving the thermal safety performance of the diaphragm.
[0039] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.
[0041] Figure 1 This is a SEM photograph of the MD-ZD cross section in the longitudinal direction of the diaphragm of Example 1-1;
[0042] Figure 2 This is a SEM photograph of the surface of the heat-resistant layer of the diaphragm of Example 1-1. DETAILED DESCRIPTION
[0043] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.
[0044] The first aspect of the present application provides a diaphragm, which comprises a substrate layer and a heat-resistant layer located on at least one surface of the substrate layer, wherein the substrate layer comprises polyolefin, and the heat-resistant layer comprises polymer fibers and inorganic ceramic particles; the diaphragm satisfies:
[0045] 1≤B L50 / B W50 ≤6, 0.1μm≤B L 50≤0.6μm, 0.04μm≤T L 50≤0.2μm;
[0046] Among them, B W50 is the average length of the pores in the substrate layer along the thickness direction in the longitudinal section, B L50 T is the average length of the pores in the longitudinal section of the substrate layer in a direction perpendicular to the section thickness; W50 is the average length of the pores in the heat-resistant layer in the longitudinal section along the thickness direction of the section, T L50 is the average length of the pores in the longitudinal section of the heat-resistant layer in the direction perpendicular to the section thickness. L50 / B W50 It can be 1, 1.2, 1.5, 1.8, 2, 2.3, 2.5, 2.8, 3, 3.5, 4, 4.2, 4.6, 5, 5.3, 5.5, 5.8, 6 or a range consisting of any two of the values. It can be 0.8, 1, 1.2, 1.5, 1.8, 2, 2.3, 2.5, 2.8, 3, 3.5, 4, 4.2, 4.6, 5, 5.3, 5.5, 5.8, 6 or a range consisting of any two of the values. L50 can be 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.55 μm, 0.6 μm or a range consisting of any two of these values, T L 50 can be 0.04μm, 0.07μm, 0.1μm, 0.12μm, 0.13μm, 0.15μm, 0.16μm, 0.18μm, 0.2μm or a range consisting of any two of these values. The present application reduces the rigidity difference between the heat-resistant layer and the substrate layer by regulating the size of the internal structural pores of the substrate layer and the heat-resistant layer, thereby increasing the membrane breaking temperature of the diaphragm, alleviating the problem of easy fracture of the membrane during long-term high-temperature treatment, and greatly reducing the curling phenomenon of the diaphragm that is prone to occur after the heat-resistant layer is coated, and improving the problem of powder loss that is prone to occur when the diaphragm is stretched or subjected to external impact.
[0047] In some embodiments, 0.5≤T L50 / T W50 ≤4. For example, T L50 / T W50 It can be 0.5, 0.8, 1, 1.2, 1.5, 1.8, 2, 2.3, 2.5, 2.8, 3, 3.5, 4 or a range consisting of any two of these values. L50 / T W50 In the above range, the thermal safety performance of the separator can be further improved.
[0048] In some embodiments, the average diameter of the polymer fiber is 10-80 nm. For example, the average diameter of the polymer fiber can be 10 nm, 20 nm, 30 nm, 50 nm, 60 nm, 70 nm, 80 nm, or a range consisting of any two of these values. The present application further improves the mechanical strength of the heat-resistant layer, the membrane breaking temperature of the diaphragm, and the flatness of the diaphragm by regulating the average diameter of the polymer fiber within the above range.
[0049] In some embodiments, the polymer is selected from at least one of para-aramid, meta-aramid, and polyimide. By using the above polymer materials, a diaphragm with good thermal safety performance can be obtained.
[0050] The present application does not particularly limit the type of the polyimide, as long as the purpose of the present application can be achieved; in some embodiments, the polyimide may be a soluble polyimide, and the polyimide may be a polymer containing the following characteristic groups:
[0051]
[0052] Wherein R is a substituted or unsubstituted aromatic, alicyclic, heterocyclic or aliphatic group. The polyimide includes at least one of aliphatic polyimide, aromatic polyimide and copolymerized polyimide thereof such as block copolymerized polyimide and graft copolymerized polyimide containing the above-mentioned characteristic groups. The polyimide can also be at least one of polyamide-imide, polyhydrazine-imide and polyester-imide. In some embodiments, the polyimide is an aromatic polyimide, which is a high temperature resistant polymer suitable for preparing a diaphragm for a secondary battery such as a lithium ion battery. The aromatic polyimide includes a monomer as shown in the following general formula:
[0053] in Independently of each other
[0054]
[0055] or a mixture thereof;
[0056] -R′- are independently
[0057]
[0058] where -R″- is independently
[0059]
[0060] X and X' are each independently selected from hydrogen, alkyl, cycloalkyl, aryl, fluoroalkyl, hydroxyl, alkoxy, phenoxy, cyano, nitro, amino, acetamido, ester, acyl, halide, carboxyl; preferably, -H, -Br, -Cl, -F, -NO2, -CN, -H, -CH3, -CH2CH3, -CH2CH2CH3, isopropyl, isobutyl, tert-butyl, cyclopentyl, cyclohexyl, phenyl, naphthyl;
[0061] n is independently 1, 2, 3 or 4;
[0062] -Ar2- are independently
[0063]
[0064] The polyimide glue described in the present application can be a polyimide / organic solvent glue after thermal imidization, or can be a glue obtained by dissolving the precipitated polyimide in an organic solvent.
[0065] In some embodiments, the polyolefin is selected from one or more copolymers or multiple blends of polyethylene, polypropylene, polybutene, and poly-4-methylpentene, and the weight average molecular weight of the polyolefin is 100,000-3,000,000, preferably 100,000-2,400,000. For example, the weight average molecular weight of the polyolefin can be 100,000, 300,000, 500,000, 700,000, 1,000,000, 1,200,000, 1,500,000, 1,700,000, 2,000,000, 2,200,000, 2,400,000, 2,600,000, 2,800,000, 3,000,000, or a range consisting of any two of these values.
[0066] In some embodiments, the material of the inorganic ceramic particles is selected from at least one of alumina, silica, boehmite, magnesium hydroxide, titanium dioxide, barium sulfate, and barium titanate.
[0067] In some embodiments, the inorganic ceramic particles include at least one of nano inorganic ceramic particles and micro nano inorganic ceramic particles, the Dv50 of the nano inorganic ceramic particles is D1, 0.01μm≤D1≤0.1μm, and the Dv50 of the micro nano inorganic ceramic particles is D2, 0.1μm<D2≤2μm; preferably, the inorganic ceramic particles include nano inorganic ceramic particles and micro nano inorganic ceramic particles, and the mass ratio H of the nano inorganic ceramic particles to the micro nano inorganic ceramic particles is (1-8):1. For example, D1 may be 0.01 μm, 0.02 μm, 0.03 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.1 μm, or a range consisting of any two of the values therein; D2 may be 0.11 μm, 0.2 μm, 0.3 μm, 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.3 μm, 1.5 μm, 1.6 μm, 1.8 μm, 2 μm, or a range consisting of any two of the values therein; and H may be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, or a range consisting of any two of the values therein. By using inorganic ceramic particles within the particle size range of the present application, a diaphragm with a higher rupture temperature and a lower curling rate can be obtained; when nano inorganic ceramic particles and micro-nano inorganic ceramic particles with a mass ratio within the above range are used at the same time, the rupture temperature of the diaphragm can be further increased while reducing the curling rate of the diaphragm.
[0068] In some embodiments, based on the total mass of the heat-resistant layer, the mass percentage content M1 of the polymer fiber is 30-70%, and the mass percentage content M2 of the inorganic ceramic particles is 30-70%; the mass percentage content of the polymer fiber on the surface of the heat-resistant layer is greater than the mass percentage content of the inorganic ceramic particles on the surface of the heat-resistant layer. For example, M1 can be 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 63%, 65%, 67%, 70% or a range consisting of any two of the values, and M2 can be 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 63%, 65%, 67%, 70% or a range consisting of any two of the values. In the present application, during the preparation of the heat-resistant layer, the inorganic ceramic particles will spontaneously deposit downward, so that the polymer fiber content on the surface of the heat-resistant layer is higher than the content of the inorganic ceramic particles. By regulating the mass percentage content M1 of the polymer fiber and the mass percentage content M2 of the inorganic ceramic particles within the above range, the present application can ensure that the diaphragm has good heat resistance, and at the same time, the air permeability of the diaphragm and the ion permeability when used in a secondary battery can be guaranteed.
[0069] In some embodiments, the thickness of the substrate layer is 5-16 μm. For example, the thickness of the substrate layer can be 5 μm, 6 μm, 7 μm, 8 μm, 10 μm, 11 μm, 12 μm, 13 μm, 15 μm, 16 μm, or a range consisting of any two of the values. In some embodiments, the thickness of the diaphragm is 10-18 μm. For example, the thickness of the diaphragm can be 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, 13 μm, 13.5 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, or a range consisting of any two of the values. The present application regulates the thickness of the diaphragm within the above range, and the diaphragm can have excellent mechanical strength and heat resistance. When used in a secondary battery, the secondary battery can have a lower internal resistance and a higher ionic conductivity, so that the overall performance of the secondary battery is better.
[0070] In some embodiments, the longitudinal elastic modulus of the diaphragm is greater than the transverse elastic modulus, and the longitudinal elastic modulus of the diaphragm is ≥2500MPa. In some embodiments, the longitudinal elastic modulus of the diaphragm is 2500-6000MPa. For example, the longitudinal elastic modulus of the diaphragm can be 2500MPa, 2800MPa, 3000MPa, 3300MPa, 3500MPa, 3700MPa, 4000MPa, 4500MPa, 5000MPa, 5200MPa, 5500MPa, 5800MPa, 6000MPa or a range consisting of any two of the values. In some embodiments, the transverse elastic modulus of the diaphragm is 1500-3000MPa. For example, the transverse elastic modulus of the diaphragm can be 1500MPa, 1700MPa, 2000MPa, 2200MPa, 2500MPa, 2800MPa, 3000MPa or a range consisting of any two of these values. The present application reduces the risk of over-stretching during the preparation of the diaphragm by regulating the longitudinal elastic modulus and the transverse elastic modulus of the diaphragm to meet the above range, thereby improving the flatness of the diaphragm and reducing the curling rate of the diaphragm.
[0071] In some embodiments, the longitudinal elongation at break of the separator is less than the transverse elongation at break, and the longitudinal elongation at break of the separator is 5-100%; the transverse elongation at break of the separator is 25-170%. For example, the longitudinal elongation at break of the diaphragm can be 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 70%, 80%, 85%, 90%, 92%, 95%, 97%, 100%, or a range consisting of any two of the values therein; the transverse elongation at break of the diaphragm can be 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, 105%, 110%, 115%, 120%, 125%, 130%, 135%, 140%, 145%, 150%, 160%, 170%, or a range consisting of any two of the values therein. The present application regulates the longitudinal elongation at break and the transverse elongation at break of the diaphragm to meet the above-mentioned range, thereby reducing the risk of over-stretching during the preparation of the diaphragm, thereby improving the flatness of the diaphragm, reducing the curling rate of the diaphragm, and also reducing the risk of defects such as excessive creases and folds during the winding process of the diaphragm.
[0072] In some embodiments, the transverse curvature of the diaphragm is ≤15%. For example, the transverse curvature of the diaphragm can be 0%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 2%, 2.5%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, or a range consisting of any two of the values. The transverse curvature of the diaphragm described in the present application meets the above range, which can reduce the risk of excessive stretching of the diaphragm during the coating process of the heat-resistant layer, avoid hole knot deformation of the heat-resistant layer in the MD direction, and thus improve the flatness of the diaphragm.
[0073] In some embodiments, the rupture temperature of the diaphragm is ≥ 250°C. For example, the rupture temperature of the diaphragm can be 250°C, 260°C, 280°C, 300°C, 320°C, 350°C, 380°C, 400°C, 420°C, 450°C, or a range consisting of any two of the values. The rupture temperature of the diaphragm described in the present application meets the above range, which is conducive to reducing the risk of the diaphragm being easily broken and improving the thermal safety performance of the diaphragm.
[0074] In some embodiments, the air permeability per unit thickness of the heat-resistant layer is 15-45s / 100cc / μm. For example, the air permeability per unit thickness of the heat-resistant layer may be 15s / 100cc / μm, 18s / 100cc / μm, 20s / 100cc / μm, 22s / 100cc / μm, 25s / 100cc / μm, 28s / 100cc / μm, 30s / 100cc / μm, 33s / 100cc / μm, 35s / 100cc / μm, 38s / 100cc / μm, 40s / 100cc / μm, 42s / 100cc / μm, 45s / 100cc / μm, or a range consisting of any two of these values. The present application adjusts the air permeability of the heat-resistant layer per unit thickness within the above range. When the separator is used in a secondary battery, the secondary battery can have a lower internal resistance and a higher ion conductivity, thereby improving the overall performance of the secondary battery.
[0075] The second aspect of the present application provides a method for preparing the diaphragm provided in the first aspect of the present application, which comprises the following steps:
[0076] 1) mixing polyolefin and porogen, kneading and extruding to prepare a cast sheet;
[0077] 2) stretching the cast sheet, wherein the temperature of the cast sheet is 120-140° C. during stretching, and the temperature difference between different points in the temperature field of the stretching region is less than 0.5° C., and an oil film is obtained after stretching, wherein the stretching includes a first longitudinal stretching and a first transverse stretching;
[0078] 3) extracting and drying the oil film, and then expanding and heat-setting to obtain the substrate layer, wherein the expanding includes a second longitudinal stretching and a second transverse stretching;
[0079] 4) coating the polymer coating liquid on at least one surface of the substrate layer, and obtaining the diaphragm through coagulation, water washing and drying;
[0080] Wherein, the product of the stretching ratios L1 of the first longitudinal stretching and the second longitudinal stretching is 5.5-14, the product of the stretching ratios L2 of the first transverse stretching and the second transverse stretching is 1-6.5, and L1>L2; based on the total mass of the polymer coating liquid, the mass percentage of the polymer fiber is 2-10%. For example, the temperature of the cast sheet during stretching can be 120°C, 125°C, 130°C, 135°C, 140°C or a range consisting of any two of the values. L1 can be 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 10, 10.5, 11, 11.5, 12, 12.5, 13, 14 or a range consisting of any two of the values; L2 can be 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5 or a range consisting of any two of the values. The mass percentage of the polymer fiber may be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or a range consisting of any two of these values.
[0081] In step 1), the present application has no particular limitation on the mixing temperature, as long as the purpose of the present application can be achieved. For example, the extrusion temperature is below 220°C, preferably 190-215°C.
[0082] In step 2), the present application does not have any particular limitation on the stretching speed, as long as the purpose of the present application can be achieved. Exemplarily, the stretching speed is 30-50 m / min. The uniformity of the temperature field needs to be controlled during the stretching, and the temperature difference between different points of the temperature field in the stretching area is controlled to be less than 0.5°C. Preferably, the temperature difference between different points of the temperature field in the stretching area is controlled to be less than 0.3°C.
[0083] In step 3), the extraction solvent can be selected from at least one of dichloromethane and cyclohexane; the present application has no particular limitation on the drying temperature, as long as the purpose of the present application can be achieved, for example, the drying temperature is 30-50°C.
[0084] In step 4), the present application has no particular limitation on the drying temperature, as long as the purpose of the present application can be achieved. For example, the drying temperature is 60-90°C.
[0085] In some embodiments, the viscosity of the polymer coating liquid is 1000-20000 mPa·s. For example, the viscosity of the polymer coating liquid can be 1000 mPa·s, 2000 mPa·s, 3000 mPa·s, 5000 mPa·s, 10000 mPa·s, 12000 mPa·s, 15000 mPa·s, 16000 mPa·s, 18000 mPa·s, 20000 mPa·s, or a range consisting of any two of these values.
[0086] In some embodiments, the maximum tension F used in the entire production line during the coating process in step 4) satisfies: Where E B is the longitudinal elastic modulus of the substrate layer, D is the thickness of the substrate layer, W is the width of the substrate layer, E B ≥2500MPa, D is 0.005-0.016mm, W is 500-1100mm. For example, E B It can be 2500MPa, 2800MPa, 3000MPa, 3300MPa, 3500MPa, 3700MPa, 4000MPa, 4500MPa, 5000MPa or a range consisting of any two of them; D can be 0.005mm, 0.006mm, 0.007mm, 0.008mm, 0.01mm, 0.011mm, 0.012mm, 0.013mm, 0.015mm, 0.016mm or a range consisting of any two of them; W can be 500mm, 600mm, 700mm, 800mm, 900mm, 1000mm, 1100mm or a range consisting of any two of them. The polymer coating liquid is prone to slipping during coating, and the maximum tension used in the entire production line during the coating process is adjusted. The risk of slipping can be greatly reduced, thereby improving the yield rate of the diaphragm.
[0087] In some embodiments, the solidification method in step 4) is selected from solidification bath solidification or constant temperature and humidity solidification;
[0088] The solvent for solidification in the coagulation bath includes a first organic solvent and a poor solvent. Based on the total mass of the solvent for solidification in the coagulation bath, the mass percentage P1 of the first organic solvent is 45-75%, and the mass percentage P2 of the poor solvent is 25-55%; the first organic solvent is selected from at least one of N-methylpyrrolidone, N,N-dimethylacetamide, and dimethyl sulfoxide, and the poor solvent is selected from at least one of water, ethanol, methanol, ethylene glycol, and tripropylene glycol; for example, P1 can be 45%, 50%, 55%, 60%, 65%, 70%, 75% or a range consisting of any two of the values therein, and P2 can be 25%, 30%, 35%, 40%, 45%, 50%, 55% or a range consisting of any two of the values therein.
[0089] The constant temperature and humidity curing includes a curing temperature of 40-70°C, a curing humidity of 55-85%, and a curing time of 3-30s. For example, the curing temperature can be 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, or a range consisting of any two of them; the curing humidity can be 55%, 60%, 65%, 70%, 75%, 80%, 85%, or a range consisting of any two of them. The curing time can be 3s, 5s, 8s, 10s, 12s, 15s, 18s, 20s, 23s, 25s, 27s, 30s, or a range consisting of any two of them.
[0090] In some embodiments, the polymer is selected from at least one of para-aramid and meta-aramid, and the steps of preparing the polymer coating liquid include: in a nitrogen environment at normal pressure, adjusting the temperature to 1-10° C., mixing and stirring the polymer glue and inorganic ceramic particles, and then adding a second organic solvent containing a co-solvent concentration of 2-10wt%, stirring and mixing to obtain the polymer coating liquid;
[0091] The polymer glue comprises polymer fibers, chloride ions and a third organic solvent. Based on the total mass of the polymer glue, the mass percentage W1 of the polymer fibers is 2-10%, and the mass percentage W2 of the chloride ions is 0.5-10%. The rotational viscosity of the polymer glue is 3000-200000 mPa·s, and the logarithmic viscosity is 1-3 dL / g. The mass ratio of the polymer fibers to the inorganic ceramic particles is (30-70): (70-30), and the co-solvent is selected from at least one of CaCl2, KOH, LiCl, and pyridine.
[0092] Or, the polymer is selected from polyimide, and the preparation steps of the polymer coating liquid include: in a nitrogen environment at normal pressure, the temperature is adjusted to 1-10°C, the polymer glue and the inorganic ceramic particles are mixed and stirred, and then a second organic solvent is added, and the mixture is stirred and mixed uniformly to obtain the polymer coating liquid; wherein the polymer glue comprises polymer fibers and a third organic solvent, and based on the total mass of the polymer glue, the mass percentage content W1 of the polymer fiber is 2-10%; the rotational viscosity of the polymer glue is 3000-200000mpa·s, the logarithmic viscosity is 1-3dL / g, and the mass ratio of the polymer fiber to the inorganic ceramic particles is (30-70): (70-30);
[0093] The second organic solvent and the third organic solvent are each independently selected from at least one of N-methylpyrrolidone, N,N-dimethylformamide, acetone, and N,N-dimethylacetamide.
[0094] For example, the regulating temperature is 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, 10°C or a range consisting of any two of the values. The cosolvent concentration is 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt% or a range consisting of any two of the values. W1 can be 2%, 2.5%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or a range consisting of any two of the values, and W2 can be 0.5%, 0.8%, 1%, 1.2%, 1.5%, 2%, 2.5%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or a range consisting of any two of the values. The rotational viscosity of the polymer glue may be 3000 mPa·s, 5000 mPa·s, 10000 mPa·s, 20000 mPa·s, 30000 mPa·s, 50000 mPa·s, 80000 mPa·s, 100000 mPa·s, 120000 mPa·s, 150000 mPa·s, 180000 mPa·s, 200000 mPa·s, or a range consisting of any two of the values thereof; the inherent logarithmic viscosity of the polymer glue may be 1 dL / g, 1.2 dL / g, 1.5 dL / g, 1.8 dL / g, 2 dL / g, 2.3 dL / g, 2.5 dL / g, 2.8 dL / g, 3 dL / g, or a range consisting of any two of the values thereof.
[0095] In some embodiments, the mass ratio of the polyolefin to the porogen is 1:(2-5). For example, the mass ratio of the polyolefin to the porogen may be 1:2, 1:3, 1:4, 1:5, or a range consisting of any two of these values.
[0096] In some embodiments, the porogen is paraffin oil.
[0097] The present application has no particular limitation on the thickness of the cast sheet, as long as the purpose of the present application can be achieved; in some embodiments, the thickness of the cast sheet is 0.3-2.5 mm. For example, the thickness of the cast sheet can be 0.3 mm, 0.5 mm, 0.8 mm, 1 mm, 1.3 mm, 1.5 mm, 1.7 mm, 2 mm, 2.2 mm, 2.5 mm, or a range consisting of any two of these values.
[0098] In the present application, the B of the separator of the present application can be changed by adjusting the stretch ratio product L1 of the first longitudinal stretching and the second longitudinal stretching, and the stretch ratio product L2 of the first transverse stretching and the second transverse stretching in the above preparation method. W50 , B L50 , T W50 , T L50 Specifically, when L1 increases, the B L50 Increase, B W50 When L1 decreases, the B L50 Reduce, B W50 Increase; when L2 increases, the B W50 When L2 decreases, the B W50 By adjusting the maximum tension F used in the entire production line during the coating process in the above-mentioned preparation method, the B of the diaphragm of the present application can be changed. W50 , B L50 , T W50 , T L50 Specifically, as F increases, the T of the diaphragm L50 Increase, T W50 When F decreases, the T of the diaphragm L50 Reduce, T W50 By adjusting the mass percentage content P1 of the first organic solvent in the above-mentioned coagulation bath solidification method, the B of the diaphragm of the present application can be changed. W50 , B L50 , T W50 , T L50 Specifically, when P1 increases, the TL of the diaphragm 50 and T W50 When P1 decreases, the T L50 and T W50 By adjusting the curing temperature in the above-mentioned constant temperature and humidity curing method, the B of the diaphragm of the present application can be changed. W50 , B L50 , T W50 , T L50 Specifically, when the curing temperature increases, the TL50 and T W50 When the curing temperature decreases, the T L50 and T W50 By adjusting the curing humidity in the above-mentioned constant temperature and humidity curing method, the B of the diaphragm of the present application can be changed. W50 , B L50 , T W50 , T L50 Specifically, when the curing humidity increases, the T L50 and T W50 When the curing humidity decreases, the T L50 and T W50 All decreased.
[0099] In the present application, the average diameter of the polymer fibers can be changed by regulating the content ratio of the polymer fibers in the polymer coating liquid. Specifically, when the content ratio of the polymer fibers in the polymer coating liquid increases, the average diameter of the polymer fibers increases; when the content ratio of the polymer fibers in the polymer coating liquid decreases, the average diameter of the polymer fibers decreases.
[0100] Example
[0101] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.
[0102] Test methods and equipment:
[0103] Determination of rotational viscosity of polymer glue and polymer coating liquid: Under certain conditions (humidity ≤ 1%, temperature: 25 ± 1 ° C), use a 250 ml beaker to take about 250 ml of polymer glue or polymer coating liquid, fix the rotor on the viscometer (Brookfield, USA, RVDV-2T), the liquid submerges the rotor and is flush with the test scale line on the rotor, and the viscosity of the liquid is measured. The rotor speed is selected between 15-100 rpm. The rotor is selected according to the actual viscosity of the liquid to ensure that the test result is between 30-80% of the test range, that is, the rotational viscosity of the polymer glue or polymer coating liquid is obtained.
[0104] Determination of the logarithmic viscosity of polymer glue: Take a polymer glue containing 0.10g of polymer and add it to 20mL of concentrated sulfuric acid (concentration of 98.3wt%), stir at 80℃ until the polymer is completely dissolved, use the same capillary viscometer (German standard Ubbelohde viscometer) to measure the outflow time t0 and t of the concentrated sulfuric acid and the dilute solution of the polymer with a concentration of 0.005g / mL dissolved in concentrated sulfuric acid at a specified temperature of 30℃, respectively, and calculate the logarithmic viscosity of the polymer glue using the formula δ=2ln(t / t0).
[0105] Determination of average particle size Dv50: The inorganic ceramic particles were measured using a particle size measuring device (Nikkiso Co., Ltd., Microtrac UPA150 particle size analyzer). As measurement conditions, the load index was set to 0.15-0.3 and the measurement time was 300 seconds. The value of the 50% particle size obtained was Dv50.
[0106] B L50 , B W50 、T L50 、T W50 Determination of:
[0107] By means of ion polishing, a smooth longitudinal-normal (MD-ZD) section was prepared along the longitudinal direction of the diaphragm. The section was observed using a scanning electron microscope (SEM, Zeiss, ZEISS SIGMA300). The maximum length of a single pore in the substrate layer along the thickness direction of the longitudinal section was measured using the ruler on the electron microscope. The average value of all pores was calculated as B. L50 ; Measure the maximum length of a single pore in the longitudinal section of the substrate layer in the direction perpendicular to the section thickness, and calculate the average value of all pores to be B W50 ; Measure the maximum length of a single pore in the heat-resistant layer along the thickness direction of the longitudinal section, and calculate the average value of all pores to be T L50 ; Measure the maximum length of a single pore in the longitudinal section of the heat-resistant layer in the direction perpendicular to the section thickness, and calculate the average value of all pores to be T W50 .
[0108] Determination of the average diameter of the polymer fibers: The surface of the diaphragm was observed with a SEM, and 5 photos with a magnification of 20,000 times were randomly taken at different positions. After outlining the hole contours with a pen, the diameter of the polymer fibers was marked with the software provided by the scanning area electron microscope, and then the average value was calculated as the average diameter of the polymer fibers.
[0109] Determination of the transverse curvature of the diaphragm: Cut a 100-150mm long diaphragm with a heat-resistant layer completely covering the surface of the substrate layer, flatten the diaphragm under the action of external force, measure the length of the diaphragm in the TD direction at this time, and record it as L1 (mm); place the diaphragm horizontally on the table, and allow the diaphragm to curl naturally in the TD direction without applying external force, measure the length of the curled diaphragm projected onto the horizontal table in the TD direction, and record it as L2 (mm). Calculate the transverse curvature of the diaphragm = (L1-L2) / L1×100%.
[0110] Air permeability measurement: Cut a 100mm×100mm substrate layer or diaphragm, use the American Gurley 4110N air permeability tester, use the 100cc test gas mode for testing, record the time for the test gas to pass through the substrate layer or diaphragm, and get the air permeability of the substrate layer or the diaphragm. The air permeability of the heat-resistant layer = the air permeability of the diaphragm - the air permeability of the substrate layer. The air permeability of the unit thickness of the heat-resistant layer = the air permeability of the heat-resistant layer / the thickness of the heat-resistant layer.
[0111] Thickness test: Use a micrometer to test the thickness of the substrate layer, and then test the thickness of the diaphragm after coating the heat-resistant layer. The thickness of the heat-resistant layer = the thickness of the diaphragm - the thickness of the substrate layer.
[0112] Elongation at break determination: Refer to the national standard GB13022-91 "Test method for tensile properties of plastic films" to determine the elongation at break of the diaphragm or substrate layer samples, cut 200mm×25mm diaphragm or substrate layer samples, use a steel ruler to confirm that the distance between the tensile clamps of the tensile testing machine is 100±5mm, the pressure between the clamps is 0.6MPa, the test speed is 250m / min, and the elongation at break is directly read when the tensile fracture occurs.
[0113] Elastic modulus determination: refer to the national standard GB13022-91 "Test method for tensile properties of plastic films" to determine the elastic modulus of the membrane or substrate layer sample, cut a 200mm×25mm membrane or substrate layer sample, the distance between the tensile clamps of the tensile testing machine is 100±5mm, make a stress-strain curve according to the requirements of 7.3 in the standard, calculate the tensile elastic modulus from the initial straight line part of the curve, and use E t (MPa) is expressed as follows:
[0114]
[0115] Where: σ: stress, MPa; ε: strain.
[0116] Membrane rupture temperature determination: The diaphragm size was cut to 80 mm × 4 mm and a thermomechanical analyzer (NETZSCH, TMA402F1 / F3 ), under the test conditions of nitrogen atmosphere, air flow of 100ml / min, tension of 0.03N, heating rate of 5℃ / min, and termination temperature of 400℃, the thermomechanical analysis (TMA) curve was measured, with temperature as the horizontal axis and deformation as the vertical axis. As the temperature increases, the deformation of the diaphragm changes. When the diaphragm ruptures, the deformation in the vertical direction of the TMA curve reaches the maximum value. At this time, the corresponding temperature on the horizontal axis is the rupture temperature of the diaphragm.
[0117] Powder loss test: Cut the diaphragm into a size of 25mm×200mm, stretch it under a tensile force of 50N, and observe whether powder loss occurs.
[0118] Example 1-1
[0119] <Preparation of substrate layer>
[0120] 30 parts by weight of polyethylene powder (weight average molecular weight 600,000-800,000, Ticona Celanese) and 70 parts by weight of paraffin oil (60#, Zhejiang Zhengxin) were mixed, and then put into a twin-screw extruder for kneading at 200±10°C to prepare a mixture melt gel. The mixture melt gel was extruded using a T-die, and then rapidly cooled on a thermostatic metal pair of rollers with a surface temperature of 15°C, and rolled into a sheet to obtain a cast sheet with a thickness of 0.87 mm.
[0121] The cast sheet was pulled and stretched, and rapidly stretched at 120°C at a speed of 40m / min, wherein the stretching ratios were 7.5 and 4.0 in the MD and TD directions, respectively, and the temperature difference between different points in the temperature field in the stretching area was controlled to be less than 0.3°C, and an oil film was obtained after stretching.
[0122] The oil film was pulled into dichloromethane for extraction, and the paraffin oil in the oil film was extracted. Then it was dried with constant temperature hot air at 40°C, and the residual dichloromethane in the diaphragm was taken out. During the extraction and drying process, the diaphragm TD direction shrank slightly due to the traction in the MD direction, with a shrinkage rate of 15%. Then it was expanded and heat-set at 131°C, in which no stretching was performed in the MD direction, and the stretching ratio in the TD direction was 1.1, to obtain a polyethylene porous membrane with uniform fiber structure orientation, which was then cut with a slitting machine to obtain a substrate layer with a width of 810 mm and a thickness of 12 μm. The tensile modulus of the substrate layer in the MD direction was measured to be 4500 MPa.
[0123] <Preparation of Separator>
[0124] Add 84kg of NMP solvent (Henan Maiqi Chemical Co., Ltd., purity ≥99.5%) and 5.45kg of anhydrous calcium chloride (Xilong Science Co., Ltd., analytical grade) to a 200kg reactor, heat to 80°C under nitrogen atmosphere, stir for 4h to completely dissolve the calcium chloride; then add 2.658kg of p-phenylenediamine (Inner Mongolia Kailidi Chemical Co., Ltd., purity >99.5%), and continue stirring until the solid is completely dissolved. Remove the air in the reactor by vacuum filtration, the internal pressure is lower than -60bar, add 99.99% high-purity nitrogen to keep the inside at normal pressure, use chilled water to reduce the temperature of the solution to 10±0.5°C, and slowly add 4.940kg of terephthaloyl chloride (Ningxia Fenghua Biotechnology Co., Ltd., purity >99.5%) in batches to obtain a para-aramid polymer solution. Calcium oxide (analytical grade, Tianjin Xintaiyi Technology Co., Ltd.) was added to adjust the pH value of the adhesive solution to between pH 4 and 8, and the solution was further diluted with NMP to obtain a 5% para-aramid adhesive solution. The rotational viscosity was tested to be 69000 mPa·s and the logarithmic viscosity was 2.0 dL / g.
[0125] Then, 80 kg of 5% para-aramid glue was added into a double planetary mixer, and 8 kg of Al2O3 (D1 was 0.05±0.03 μm nano Al2O3 and D2 was 0.3±0.15 μm micro-nano Al2O3, mass ratio = 3:1) was added three times (the mass ratio of addition was 40:40:20), and after stirring for 30 minutes, 80 kg of NMP / CaCl2 solution (CaCl2 solid content was 5 wt%) was added, and stirring was continued for 90 minutes to disperse and mix the slurry evenly to obtain a slurry with a viscosity of 9000 mPa·s. The slurry was filtered through a 300-mesh filter before use to obtain a para-aramid coating liquid, in which the mass percentage of para-aramid fiber in the para-aramid coating liquid was 2.38%.
[0126] A coating machine was used to evenly coat the para-aramid coating liquid onto one side of the substrate layer with a width of 810 mm prepared above. The immersion phase inversion method was used to obtain a diaphragm including a substrate layer and a heat-resistant layer through coagulation bath curing, deionized water washing, and drying. The solvent for coagulation bath curing was NMP and ultrapure water in a mass ratio of 2:1, and the NMP content P1 was 67 wt%. The maximum tension F used in the entire production line during the coating process was 160 N, and a diaphragm with a thickness of 16 μm was obtained.
[0127] Example 1-2 to Example 1-16
[0128] Except that the corresponding preparation parameters in <Preparation of substrate layer> and <Preparation of diaphragm> are adjusted according to Table 1, the rest is the same as Example 1-1, wherein, The curing is performed by solidification bath curing or constant temperature and humidity curing, and the masses of Al2O3 and NMP / CaCl2 solution in the polymer coating liquid remain unchanged.
[0129] Example 2-1 to Example 2-9
[0130] Except for adjusting the corresponding preparation parameters in <Preparation of substrate layer> and <Preparation of separator> according to Table 3, the rest is the same as Example 1-1.
[0131] Embodiment 2-10
[0132] Except that the added 5% para-aramid glue with a mass fraction is replaced by a 5% polyimide glue with a mass fraction in <Preparation of Diaphragm>, and the added 80kg NMP / CaCl2 solution (CaCl2 solid content is 5wt%) is replaced by 80kg NMP, the rest is the same as Example 1-1, wherein the preparation step of the polyimide glue is: dissolving a polyimide with a Mw of 30,000-100,000 in NMP to obtain a polyimide glue with a mass fraction of 5%, and the rotational viscosity thereof is tested to be 30,000 mpa·s, and the logarithmic viscosity is 2.0 dL / g, wherein the structural formula of the polyimide is:
[0133]
[0134] Example 3-1 to Example 3-5
[0135] Except for adjusting the corresponding preparation parameters in <Preparation of Diaphragm> according to Table 5, the rest is the same as Example 1-1, wherein the total mass of the polymer fibers and the inorganic ceramic particles remains unchanged.
[0136] Comparative Example 1-1 to Comparative Example 1-5
[0137] Except for adjusting the corresponding preparation parameters in <Preparation of substrate layer> and <Preparation of diaphragm> according to Table 1, the rest is the same as Example 1-1, wherein the curing is coagulation bath curing or constant temperature and humidity curing, and the mass of Al2O3 and NMP / CaCl2 solution in the polymer coating liquid remains unchanged.
[0138]
[0139]
[0140]
[0141]
[0142]
[0143] The MD-ZD cross-sectional SEM photograph of the longitudinal direction of the diaphragm of Example 1-1 is as follows: Figure 1 As shown, the SEM photo of the surface of the heat-resistant layer of the diaphragm is as follows Figure 2 As shown. According to the results of Table 2, Table 4 and Table 6, by adjusting the pore size of the diaphragm of the present application, the average diameter of the polymer fiber and the particle size Dv50 of the inorganic ceramic particles within the scope of the present application, the curling rate of the diaphragm can be reduced, the powdering phenomenon of the diaphragm can be improved, and the membrane breaking temperature of the diaphragm can be increased. At the same time, the air permeability of the heat-resistant layer of the diaphragm of the present application can be taken into account to ensure the ion pass rate of the diaphragm.
[0144] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A diaphragm comprising a substrate layer and a heat-resistant layer located on at least one surface of the substrate layer, wherein the substrate layer comprises polyolefin, and the heat-resistant layer comprises polymer fibers and inorganic ceramic particles; the diaphragm satisfies: in, B W50 is the average length of the pores in the substrate layer along the thickness direction in the longitudinal section, B L50 is the average length of the pores in the longitudinal section of the substrate layer in a direction perpendicular to the section thickness; T W50 is the average length of the pores in the heat-resistant layer in the longitudinal section along the thickness direction of the section, T L50 It is the average length of the pores in the longitudinal section of the heat-resistant layer in a direction perpendicular to the section thickness.
2. The diaphragm according to claim 1, wherein 0.5≤T L50 / T W50 ≤4。 3. The diaphragm according to claim 1, wherein The average diameter of the polymer fibers is 10-80 nm.
4. The diaphragm according to claim 1, wherein The polymer is selected from at least one of para-aramid, meta-aramid and polyimide.
5. The diaphragm according to claim 1, wherein The polyolefin is selected from one or more copolymers or blends of polyethylene, polypropylene, polybutene, and poly-4-methylpentene. The weight average molecular weight of the polyolefin is 100,000-3,000,000, preferably 100,000-2,400,000.
6. The diaphragm according to claim 1, wherein The material of the inorganic ceramic particles is at least one selected from alumina, silica, boehmite, magnesium hydroxide, titanium dioxide, barium sulfate, and barium titanate.
7. The diaphragm according to claim 6, wherein: The inorganic ceramic particles include at least one of nano inorganic ceramic particles and micro nano inorganic ceramic particles, the Dv50 of the nano inorganic ceramic particles is D1, 0.01μm≤D1≤0.1μm, and the Dv50 of the micro nano inorganic ceramic particles is D2, 0.1μm<D2≤2μm; preferably, the inorganic ceramic particles include nano inorganic ceramic particles and micro nano inorganic ceramic particles, and the mass ratio H of the nano inorganic ceramic particles to the micro nano inorganic ceramic particles is (1-8):
1.
8. The diaphragm according to claim 1, wherein Based on the total mass of the heat-resistant layer, the mass percentage M1 of the polymer fiber is 30-70%, and the mass percentage M2 of the inorganic ceramic particles is 30-70%; the mass percentage of the polymer fiber on the surface of the heat-resistant layer is greater than the mass percentage of the inorganic ceramic particles on the surface of the heat-resistant layer.
9. The diaphragm according to claim 1, wherein: The thickness of the substrate layer is 5-16 μm, and the thickness of the separator is 10-18 μm.
10. The diaphragm according to any one of claims 1 to 9, wherein: The diaphragm satisfies at least one of the following characteristics: a) the longitudinal elastic modulus of the diaphragm is greater than the transverse elastic modulus, and the longitudinal elastic modulus of the diaphragm is ≥2500MPa; b) the longitudinal elongation at break of the diaphragm is less than the transverse elongation at break, the longitudinal elongation at break of the diaphragm is 5-100%; the transverse elongation at break of the diaphragm is 25-170%; d) the transverse curvature of the separator is ≤15%; e) The rupture temperature of the diaphragm is ≥ 250°C; f) The air permeability per unit thickness of the heat-resistant layer is 15-45s / 100cc / μm.
11. The method for preparing a diaphragm according to any one of claims 1 to 10, comprising the following steps: 1) mixing polyolefin and porogen, kneading and extruding to prepare a cast sheet; 2) stretching the cast sheet, wherein the temperature of the cast sheet is 120-140° C. during stretching, and the temperature difference between different points in the temperature field of the stretching region is less than 0.5° C., and an oil film is obtained after stretching, wherein the stretching includes a first longitudinal stretching and a first transverse stretching; 3) extracting and drying the oil film, and then expanding and heat-setting to obtain the substrate layer, wherein the expanding includes a second longitudinal stretching and a second transverse stretching; 4) coating the polymer coating liquid on at least one surface of the substrate layer, and obtaining the diaphragm through coagulation, water washing and drying; Among them, the stretching ratio product L1 of the first longitudinal stretching and the second longitudinal stretching is 5.5-14, the stretching ratio product L2 of the first transverse stretching and the second transverse stretching is 1-6.5, and L1>L2; based on the total mass of the polymer coating liquid, the mass percentage of the polymer fiber is 2-10%.
12. The preparation method according to claim 11, wherein In step 4), the maximum tension F used in the entire production line during the coating process satisfies: Where E B is the longitudinal elastic modulus of the substrate layer, D is the thickness of the substrate layer, W is the width of the substrate layer, E B ≥2500MPa, D is 0.005-0.016mm, W is 500-1100mm.
13. The preparation method according to claim 11, wherein: Step 4) The solidification method is selected from solidification bath solidification or constant temperature and humidity solidification; The solvent for solidification by coagulation bath includes a first organic solvent and a poor solvent. Based on the total mass of the solvent for solidification by coagulation bath, the mass percentage content P1 of the first organic solvent is 45-75%, and the mass percentage content P2 of the poor solvent is 25-55%; the first organic solvent is selected from at least one of N-methylpyrrolidone, N,N-dimethylacetamide, and dimethyl sulfoxide, and the poor solvent is selected from at least one of water, ethanol, methanol, ethylene glycol, and tripropylene glycol; The constant temperature and humidity curing includes a curing temperature of 40-70° C., a curing humidity of 55-85%, and a curing time of 3-30 seconds.
14. The preparation method according to any one of claims 11 to 13, wherein The polymer is selected from at least one of para-aramid and meta-aramid. The preparation steps of the polymer coating liquid include: in a nitrogen environment at normal pressure, the temperature is adjusted to 1-10°C, the polymer glue and the inorganic ceramic particles are mixed and stirred, and then a second organic solvent containing a co-solvent concentration of 2-10wt% is added, and the mixture is stirred and mixed uniformly to obtain the polymer coating liquid; wherein the polymer glue includes polymer fibers, chloride ions and a third organic solvent, based on the total mass of the polymer glue, the mass percentage content W1 of the polymer fibers is 2-10%, and the mass percentage content W2 of the chloride ions is 0.5-10%; the rotational viscosity of the polymer glue is 3000-200000mpa·s, the logarithmic viscosity is 1-3dL / g, the mass ratio of the polymer fibers to the inorganic ceramic particles is (30-70): (70-30), and the co-solvent is selected from at least one of CaCl2, KOH, LiCl, and pyridine; Or, the polymer is selected from polyimide, and the preparation steps of the polymer coating liquid include: in a nitrogen environment at normal pressure, the temperature is adjusted to 1-10°C, the polymer glue and the inorganic ceramic particles are mixed and stirred, and then a second organic solvent is added, and the mixture is stirred and mixed uniformly to obtain the polymer coating liquid; wherein the polymer glue comprises polymer fibers and a third organic solvent, and based on the total mass of the polymer glue, the mass percentage content W1 of the polymer fiber is 2-10%; the rotational viscosity of the polymer glue is 3000-200000mpa·s, the logarithmic viscosity is 1-3dL / g, and the mass ratio of the polymer fiber to the inorganic ceramic particles is (30-70): (70-30); The second organic solvent and the third organic solvent are each independently selected from at least one of N-methylpyrrolidone, N,N-dimethylformamide, acetone, and N,N-dimethylacetamide.
15. The preparation method according to any one of claims 11 to 13, wherein The mass ratio of the polyolefin to the porogen is 1:(2-5).
Citation Information
Cited By
Separator and preparation method therefor
WO2026051275A1