Method of inkjet printing

By using anti-solvents to form a mixing area in inkjet printing, the problem of uneven crystal arrangement caused by the coffee ring effect in traditional perovskite inkjet printing is solved, and the uniform growth and quality improvement of perovskite crystals are achieved. It is suitable for Large-scale mass production.

CN119072204APending Publication Date: 2024-12-03RAYLEIGH VISION INTELLIGENCE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310635772.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In traditional perovskite inkjet printing methods, the coffee ring effect caused by evaporation and drying leads to uneven arrangement of perovskite crystals, which cannot form the required array direction or pattern, affecting the quality of the material.

Method used

The first nozzle of the inkjet device uses the printing of the perovskite precursor onto the carrier, and sprays anti-solvent through the second nozzle to form a mixing area to supersaturate the perovskite precursor and precipitate the crystals, control the crystal growth position, and avoid coffee. ring effect.

Benefits of technology

The uniform growth of perovskite crystals is achieved, the material quality is improved, and the required array direction or pattern can be formed, which is suitable for large-area mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072204A_ABST
    Figure CN119072204A_ABST
Patent Text Reader

Abstract

The invention relates to an ink-jet printing method, which comprises the following steps of: printing first ink on a carrier by using a first spray head assembly of an ink-jet device to form a first liquid drop, printing second ink on the carrier by using a second spray head assembly of the ink-jet device to form a second liquid drop after a first time, and printing the second liquid drop on the carrier by using a second spray head assembly of the ink-jet device. The first liquid drop and the second liquid drop are overlapped to form a mixing area, the second liquid drop in the mixing area enables the first liquid drop in the mixing area to form supersaturation, a seed crystal is separated out in the mixing area, and finally, the second liquid drop is continuously mixed with the first liquid drop, so that the mixing area is expanded, and the seed crystal is separated out. And the seed crystal is continuously separated out in the mixing area to form a crystal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method, in particular to an inkjet printing method. Background Art

[0002] Since perovskite materials are good optoelectronic materials, they are widely used in solar cells. Generally speaking, in the process of forming a perovskite film on a substrate, the perovskite precursor material coated on the substrate is heated to volatilize the solvent in the perovskite precursor material and react the perovskite precursor to form a perovskite film.

[0003] Traditionally, the perovskite precursor is placed on a substrate and allowed to evaporate and dry to form perovskite crystals. However, this method will produce many small crystal particles, making it difficult to produce single crystals. This problem will become more prominent when perovskite materials are mass-produced on a large scale.

[0004] The current classification of perovskite production methods can be roughly divided into the following four types: (1) coating method, (2) injection coating method, (3) continuous inkjet method (CIJ) and (4) drop demand inkjet method (DOD).

[0005] Among them, the coating method and the injection coating method are suitable for large-scale mass production because they directly coat the perovskite precursor on the substrate. However, the perovskite produced by this method will produce many small crystals, resulting in poor quality of the formed perovskite film.

[0006] The continuous inkjet method continuously ejects ink droplets from the print head, and then guides these droplets as printing droplets onto the substrate, or guides them to the collector for recycling and reuse. The inkjet printing process can be applied to large areas, can avoid metal shielding or photomasks, has high material utilization rate, and the same set of inkjet printing equipment can be used to manufacture panels of different sizes. It can be produced in an atmospheric environment, does not require expensive vacuum equipment, and requires lower material and equipment costs, which are the advantages of IJP. Different from the process technology of traditional light-emitting components.

[0007] However, the above-mentioned perovskite production method requires pre-treatment of the substrate, such as thermal annealing or increasing the surface roughness of the substrate, or requires complex temperature control to evaporate the liquid of the perovskite precursor and generate crystals.

[0008] However, this method of evaporation to produce crystallization will cause the perovskite crystals to produce a coffee ring effect during the crystallization process, making it impossible for the perovskite crystals to be arranged in the desired array direction or array pattern, thus affecting the application of perovskite.

[0009] Among them, the aforementioned coffee ring effect refers to when a drop of coffee or tea falls on the table, its particulate matter will leave a stained stain on the table, and the color of the stain is uneven, the edge is darker than the middle, forming a ring-shaped spot phenomenon, the main reason for its formation is due to the influence of the shape of the liquid stain particles and the problem of flow direction.

[0010] The reason for the coffee ring effect in perovskite crystals is that the different inkjet printing parameter indicators are caused during crystallization. At this time, the perovskite crystals will form a ring-shaped coffee spot with a shallow center and a heavy outer ring on the surface of the substrate. Relatively speaking, the quality of the perovskite film formed cannot be improved.

[0011] Therefore, how to improve the inkjet printing method so that a perovskite single crystal pattern can be obtained after printing is a problem that technicians in this field want to solve. Summary of the invention

[0012] An object of the present invention is to provide an inkjet printing method, which prints a perovskite precursor onto a carrier through a first nozzle, and then changes the perovskite precursor through an anti-solvent so that the perovskite precursor forms crystals on the carrier.

[0013] In view of the above-mentioned purpose, the present invention provides an inkjet printing method, which utilizes a first nozzle assembly of an inkjet device to print a first ink on a carrier to form a first droplet, and after a first time, uses a second nozzle assembly of the inkjet device to print a second ink on the carrier to form a second droplet, and the first droplet and the second droplet overlap to form a mixing area, wherein the first droplet has a first droplet diameter, the second droplet has a second droplet diameter, the first droplet diameter is larger than the second droplet diameter, the second droplet in the mixing area makes the first droplet in the mixing area supersaturated, and precipitates a seed crystal in the mixing area, and finally the second droplet continues to mix with the first droplet to expand the mixing area, and the seed crystal continues to precipitate in the mixing area to form a crystal.

[0014] The present invention provides an embodiment, wherein after a first time, a second nozzle assembly of the inkjet device is used to print a second ink on the carrier to form a second droplet, and the first droplet and the second droplet overlap to form a mixed area, and the mixed area is between a first center point of the first droplet and a second center point of the second droplet.

[0015] The present invention provides an embodiment, wherein the second droplet in the mixing area causes the first droplet in the mixing area to form supersaturation and precipitate a seed in the mixing area, and the first droplet and the second droplet have a droplet ratio between 1:1 and 3:1.

[0016] The present invention provides an embodiment, wherein in the step of using a first nozzle assembly of an inkjet device to print a first ink on the carrier to form a first droplet, the carrier is a semiconductor material.

[0017] The present invention provides an embodiment, wherein in the step of using a first nozzle assembly of an inkjet device to print a first ink on the carrier to form a first droplet, the first nozzle assembly includes a first ink storage tank and a first nozzle, and the first nozzle is connected to the first ink storage tank.

[0018] The present invention provides an embodiment, wherein a first ink is printed on the carrier using a first nozzle assembly of an inkjet device to form a first droplet. The first ink contains a perovskite precursor and a solvent, and dimethylformamide is used as the solvent.

[0019] The present invention provides an embodiment, wherein after a first time, a second nozzle assembly of the inkjet device is used to print a second ink on the carrier to form a second droplet, and the first droplet and the second droplet overlap to form a mixed area, and the first time is between 0.5 seconds and 1.5 seconds.

[0020] The present invention provides an embodiment, wherein after a first time, a second nozzle assembly of the inkjet device is used to print a second ink on the carrier to form a second droplet, and the first droplet and the second droplet overlap to form a mixed area. The second nozzle assembly includes a second ink storage tank and a second nozzle, and the second nozzle is connected to the second ink storage tank.

[0021] The present invention provides an embodiment, wherein after a first time, a second nozzle assembly of the inkjet device is used to print a second ink on the carrier to form a second droplet, and in the step of overlapping the first droplet and the second droplet to form a mixed area, the second ink is an anti-solvent, and the anti-solvent is ethylene glycol, isopropyl alcohol, toluene or n-hexane.

[0022] The present invention provides an embodiment in which the size of the crystals is controlled in the mixing region and the position of the carrier. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 :It is a schematic diagram of the steps of an inkjet printing method according to an embodiment of the present invention; Figure 2A :It is a schematic diagram of the operation of the inkjet printing method according to one embodiment of the present invention; Figure 2B:It is a schematic diagram of the operation of the inkjet printing method according to one embodiment of the present invention; Figure 2C :It is a schematic diagram of the operation of the inkjet printing method according to one embodiment of the present invention; and Figure 2D : It is a schematic diagram of the operation of the inkjet printing method according to one embodiment of the present invention.

Figure number comparison

[0024] In order to further understand and appreciate the structural features and effects of the present invention, a preferred embodiment and detailed description are provided as follows:

[0025] The conventional method of producing perovskite crystals by evaporation will cause the perovskite crystals to produce a coffee ring effect during the crystallization process. The reason for the coffee ring effect of the perovskite crystals is that the inkjet printing parameter indicators are different during crystallization. At this time, the perovskite crystals will form a ring-shaped coffee spot with a shallow center and a heavy outer ring on the surface of the substrate. Relatively speaking, the quality of the formed perovskite crystals cannot be improved, so that the arrangement of the perovskite crystals cannot form the required array direction or array pattern, thereby affecting the application.

[0026] The present invention is an improved inkjet printing method, in which a perovskite precursor is printed onto a carrier through a first nozzle on an inkjet device, and then the perovskite precursor is changed through an anti-solvent so that the perovskite precursor forms crystals on the carrier.

[0027] Hereinafter, the present invention will be described in detail by illustrating various embodiments of the present invention with reference to the drawings. However, the concept of the present invention may be embodied in many different forms and should not be construed as being limited to the exemplary embodiments described herein.

[0028] First, see Figure 1 , which is a schematic diagram of the steps of an inkjet printing method according to an embodiment of the present invention. The steps of the inkjet printing method according to this embodiment are as follows:.

[0029] Step S10: using a first nozzle assembly of an inkjet device to print a first ink on a carrier to form a first droplet;

[0030] Step S20: After the first time, use a second nozzle assembly of the inkjet device to print a second ink on the carrier to form a second droplet, and the first droplet and the second droplet overlap to form a mixed area;

[0031] Step S30: the second liquid droplets in the mixing region supersaturate the first liquid droplets in the mixing region and precipitate crystal seeds in the mixing region; and

[0032] Step S40: The second liquid droplet continues to mix with the first liquid droplet to expand the mixing area, and the crystal seeds continue to precipitate in the mixing area to form crystals.

[0033] In this embodiment, please refer to the steps described in step S10. FIG. 2A to FIG. 2D , which is an operation schematic diagram of an inkjet printing method according to an embodiment of the present invention. As shown in the figure, in this embodiment, a first nozzle assembly 12 of an inkjet device 10 is used to print a first ink 16 on a carrier 1, and the first ink 16 forms a first droplet 20 on the carrier 1. The first droplet 20 has a first droplet diameter D1, and the carrier 1 is a semiconductor material.

[0034] Please refer to Figure 2A In this embodiment, the first nozzle assembly 12 includes a first ink storage tank 122 and a first nozzle 124 . The first nozzle 124 is connected to the first ink storage tank 122 . The first ink storage tank 122 is used to store the first ink 16 .

[0035] In this embodiment, the first ink 16 includes a perovskite precursor and a solvent. The solvent is dimethylformamide. The first ink 16 dissolves PbBr2 (1M) and H3NH3Br (1M) in dimethylformamide (DMF).

[0036] Next, please refer to Figure 2BIn step S20 of the present embodiment, after a first time, a second nozzle assembly 14 of the inkjet device 10 is used to print a second ink 18 on the carrier 1 to form a second droplet 30. The first droplet 20 and the second droplet 30 overlap to form a mixed area P1. The first time is between 0.5 seconds and 1.5 seconds. The second droplet 30 of the present embodiment has a second droplet diameter D2. The first time is between 0.5 seconds and 1.5 seconds.

[0037] In this embodiment, the second nozzle assembly 14 includes a second ink storage tank 142 and a second nozzle 144 . The second nozzle 144 is connected to the second ink storage tank 142 . The second ink storage tank 142 is used to store the second ink 18 .

[0038] In this embodiment, the second ink 18 is an anti-solvent, and the anti-solvent is ethylene glycol (EG), iso-propanol (IPA), toluene (TL) or n-hexane. The anti-solvent is used to make the first droplet 20 reach a supersaturated state.

[0039] Please refer to Figure 2C In step S30 of this embodiment, the second liquid droplet 30 in the mixing region P1 supersaturates the first liquid droplet 20 in the mixing region P1 and precipitates a seed crystal 40 in the mixing region P1.

[0040] In this embodiment, the mixing area P1 is between a first center point C1 of the first liquid droplet 20 and a second center point C2 of the second liquid droplet 30 .

[0041] Finally, please refer to Figure 2D In this embodiment, as described in step S40, the second droplet 30 continues to mix with the first droplet 20 (eg Figure 2D The mixed region P1 is enlarged, and the seed crystal 40 is continuously precipitated in the mixed region P1 to form a crystal 50. The mixed region P1 is an initial growth point of the crystal 50. That is to say, the position of the seed crystal 40 precipitated in the mixed region P1 is the initial growth position of the crystal 50 (the initial growth point). That is to say, the size of the crystal is controlled in the mixed region and is controlled to be set at the position of the carrier.

[0042] In this embodiment, the first droplet diameter D1 is greater than the second droplet diameter D2 , and the size of the crystal 50 is controlled by controlling the droplet size of the first droplet 20 .

[0043] Furthermore, in this embodiment, the first liquid droplet 20 and the second liquid droplet 30 have a liquid droplet ratio between 1:1 and 3:1. By controlling the liquid droplet ratio between the first liquid droplet 20 and the second liquid droplet 30, the volume of the crystal 50 is controlled.

[0044] In addition, a crystal growth temperature of the crystal 50 in this embodiment is room temperature, which is different from the high temperature environment of the prior art (droplet evaporation method), thus saving energy and being able to quickly obtain the crystal 50 .

[0045] The conventional droplet evaporation method will cause the perovskite crystal to produce a coffee ring effect during the crystallization process. The reason for the coffee ring effect of the perovskite crystal is that the inkjet printing parameter indicators are different during crystallization. At this time, the perovskite crystal will form a ring-shaped coffee spot with a shallow center and a heavy outer ring on the substrate surface. Relatively speaking, the quality of the formed perovskite crystal cannot be improved, so that the arrangement of the perovskite crystal cannot form the required array direction or array pattern, thus affecting the application.

[0046] The advantage of this embodiment is that the edges of the first liquid droplet 20 and the second liquid droplet 30 are brought into contact, so that the droplet concentration of the first liquid droplet 20 at the edge is increased by the second liquid droplet 30, making it supersaturated, thereby precipitating the crystal seed 40, and effectively controlling the growth position of the crystal seed 40. Through the characteristics of the first liquid droplet 20 and the second liquid droplet 30, the crystal seed 40 can quickly grow into the crystal 50. This embodiment can avoid the coffee ring effect of the perovskite crystal 50, and can directly pattern the crystal 50.

[0047] This embodiment lists an implementation aspect as follows:

[0048] In order to produce the crystal 50 in this embodiment, the first nozzle assembly 12 and the second nozzle assembly 14 need to be printed on the carrier 1, but they cannot be printed directly at the same place. If they are printed at the same position, many tiny crystals 50 will be produced in the overlapping area.

[0049] Therefore, to control the nucleation and growth of perovskite (the crystal 50), the proper distance between the first droplet 20 and the second droplet 30 printed by both the precursor (the first ink 16) and the antisolvent (the second ink 18) is crucial.

[0050] In this embodiment, it is found that the morphology of the grown perovskite (the crystal 50) is strongly dependent on the position where the antisolvent (the second ink 18) overlaps the precursor (the first ink 16). If it is ultimately desired to grow a single perovskite (the crystal 50), only one nuclei 40 can be formed in the mixing region P1, and the formation of multiple nuclei can be avoided.

[0051] Therefore, in order to obtain a single perovskite (the crystal 50), the precursor (the first ink 16) and the antisolvent (the second ink 18) are first printed on the carrier according to the droplet ratio of 3:1. In this example, the first droplet diameter D1 of the first droplet 20 of the precursor (the first ink 16) is greater than the second droplet diameter D2 of the second droplet 30 of the antisolvent (the second ink 18).

[0052] When the second droplet 30 of the antisolvent (the second ink 18) is printed to the edge of the first droplet 20 of the precursor (the first ink 16), the mixing area P1 is formed. The second droplet 30 of the antisolvent (the second ink 18) will make the first droplet in the mixing area form an oversaturated state in the mixing area P1, so that the seed crystal 40 is precipitated.

[0053] The second droplet 30 of the subsequent antisolvent (the second ink 18 ) continues to mix with the first droplet 20 of the precursor (the first ink 16 ), so that the mixing area P1 is expanded, and the seed crystal 40 continues to precipitate in the mixing area P1 to form a single perovskite (the crystal 50 ).

[0054] Using the edge deposition strategy in this embodiment, nucleation and growth of various sizes in the precursor (the first ink 16) can be easily controlled to form large-diameter single perovskite crystals (the crystals 50) on various substrates (the carrier 1, regardless of the hydrophilicity or crystal orientation of the surface).

[0055] The embodiments described above are an inkjet printing method of the present invention, in which a perovskite precursor is printed onto a carrier through a first nozzle on an inkjet device, and then the perovskite precursor is changed through an anti-solvent so that the perovskite precursor forms crystals on the carrier, thereby avoiding the coffee ring effect of the crystals, and patterning can be performed directly on the crystals.

[0056] The order of execution of each step in the above embodiment does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiment of the present application.

[0057] The above is only a preferred embodiment of the present invention and is not intended to limit the scope of the present invention. All equivalent changes and modifications to the shape, structure, characteristics and spirit described in the claims of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A method of inkjet printing, characterized in that: It contains: Using a first nozzle assembly of an inkjet device to print a first ink on a carrier to form a first droplet, wherein the first droplet has a first droplet diameter; After a first time, a second ink is printed on the carrier using a second nozzle assembly of the inkjet device to form a second droplet, wherein the first droplet and the second droplet overlap to form a mixed region, wherein the second droplet has a second droplet diameter, and the first droplet diameter is larger than the second droplet diameter; The second liquid droplet in the mixing region causes the first liquid droplet in the mixing region to form supersaturation and precipitate a seed crystal in the mixing region; and The second liquid droplet is continuously mixed with the first liquid droplet, so that the mixed region is expanded, and the crystal seed is continuously precipitated in the mixed region to form a crystal.

2. The inkjet printing method according to claim 1, characterized in that: After a first time, a second nozzle assembly of the inkjet device is used to print a second ink on the carrier to form a second droplet. In the step of overlapping the first droplet and the second droplet to form a mixed area, the mixed area is between a first center point of the first droplet and a second center point of the second droplet.

3. The inkjet printing method according to claim 1, characterized in that: In the step where the second liquid droplet in the mixing region supersaturates the first liquid droplet in the mixing region and precipitates a seed crystal in the mixing region, the first liquid droplet and the second liquid droplet have a droplet ratio between 1:1 and 3:

1.

4. The inkjet printing method according to claim 1, characterized in that: In the step of using a first nozzle assembly of an inkjet device to print a first ink on the carrier to form a first liquid droplet, the carrier is a semiconductor material.

5. The inkjet printing method according to claim 1, characterized in that: In the step of using a first nozzle assembly of an inkjet device to print a first ink on the carrier to form a first droplet, the first nozzle assembly includes a first ink storage tank and a first nozzle, and the first nozzle is connected to the first ink storage tank.

6. The inkjet printing method according to claim 1, characterized in that: In the step of using a first nozzle assembly of an inkjet device to print a first ink on the carrier to form a first droplet, the first ink contains a perovskite precursor salt and a solvent, and the solvent is dimethylformamide.

7. The inkjet printing method according to claim 1, characterized in that: After a first time, a second nozzle assembly of the inkjet device is used to print a second ink on the carrier to form a second droplet, and the first droplet and the second droplet overlap to form a mixed area. The first time is between 0.5 seconds and 1.5 seconds.

8. The inkjet printing method according to claim 1, characterized in that: After a first time, a second nozzle assembly of the inkjet device is used to print a second ink on the carrier to form a second droplet. In the step of overlapping the first droplet and the second droplet to form a mixed area, the second nozzle assembly includes a second ink storage tank and a second nozzle, and the second nozzle is connected to the second ink storage tank.

9. The inkjet printing method according to claim 1, characterized in that: After a first time, a second nozzle assembly of the inkjet device is used to print a second ink on the carrier to form a second droplet. In the step of overlapping the first droplet and the second droplet to form a mixed area, the second ink is an anti-solvent, and the anti-solvent is ethylene glycol, isopropanol, toluene or n-hexane.

10. The inkjet printing method according to claim 1, characterized in that: The size of the crystal is controlled in the mixing region and positioned on the carrier.