Brake element carrier body, brake disc or brake drum, and method for producing brake element carrier body

By coating the metal matrix of the brake disc, it diffuses into the substrate and forming intermetallic compounds, the problem of rapid wear of the friction surface of the traditional brake disc is solved, and higher wear resistance and corrosion protection are achieved , ensuring the stability of the braking effect.

CN119072591APending Publication Date: 2024-12-03GOTEC BRAKE DISC COATINGS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380018043.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-21
Filing Date
2023-01-23
Publication Date
2024-12-03

Smart Images

  • Figure CN119072591A_ABST
    Figure CN119072591A_ABST
Patent Text Reader

Abstract

The invention relates to a brake element carrier body having a metallic main body (2), a surface (3) of the main body (2) being at least partially, preferably completely, coated with an alloy (5), which has been diffused into the main body (2) in a diffusion zone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a brake element carrier body, a brake disc or a brake drum, a brake pad back plate or a brake shoe, a method for manufacturing a brake element carrier body, a method for manufacturing a brake disc or a brake drum, a method for manufacturing a brake pad back plate or a brake shoe, a brake disc or a brake drum, a brake pad back plate or a brake shoe, and a brake system. Background Art

[0002] Reducing particle pollution and extending service life to reduce waste have been top priorities in industry for decades. In the automotive industry, the focus is no longer just on reducing exhaust emissions from combustion engines; in order to continue to meet particle limit values, tire and brake wear is also becoming increasingly important.

[0003] In motor vehicles having both an electric motor and a combustion engine, more wear-resistant friction elements for the brakes can contribute to this.

[0004] Brake discs for vehicles, running wheels or rail guides or industrial systems are made of metal or ceramic materials and have several specific areas that fulfill their functions. One of these areas is the friction surface of the brake disc. In order to achieve the desired braking effect, the brake pad acts on the friction surface with a defined normal force. The kinetic energy applied to the friction surface is converted into thermal energy, i.e. heat, by sliding friction.

[0005] In conventional brake discs, the friction surface of the brake disc is protected from corrosion by painting or spraying it. The materials used for this purpose usually have low tribological qualities (i.e. low friction coefficient and high wear). This only works for a short time, because the friction during the braking process disappears very quickly.

[0006] When the corrosion layer is removed, the base material (usually steel or grey cast iron) is completely exposed and corrosion can begin unhindered. In vehicles that rarely require conventional braking using brake discs (e.g. electric or hybrid vehicles), corrosion continues rapidly after the top layer has been removed. This first leads to a considerable increase in the wear of the friction surface of the brake disc. In addition, in this case, emergency braking in an emergency situation cannot be achieved to the required extent due to the rust layer that has already formed. In the worst case, this situation can lead to accidents or other negative consequences. Summary of the invention

[0007] The present invention is based on the object of providing an improvement or alternative to the prior art.

[0008] According to a first aspect of the invention, this object is achieved by a brake element carrier body having a metallic basic body, wherein a surface of the basic body is at least partially coated with an alloy which diffuses into the basic body in a diffusion zone.

[0009] In a preferred embodiment, the substrate is fully coated with the alloy.

[0010] Furthermore, it is explicitly pointed out that in the context of this patent application, indefinite articles and numerical indications (such as "one", "two", etc.) should generally be understood as the specification of "at least" (i.e. "at least one...", "at least two...", etc.), unless it can be inferred from the respective context or it is obvious or technically necessary for a qualified expert to imply only "exactly one...", "exactly two...", etc.

[0011] Diffusion is usually understood as the equalization of concentration differences between several substances until equilibrium is reached. Diffusion can be a process of equalization of thermally activated concentration differences in solids, liquids or gases that are not subject to external influences. In a perfect crystal lattice, each lattice particle oscillates around its fixed lattice position and cannot leave this position. For diffusion in crystalline solids, the presence of lattice defects is therefore an essential prerequisite. Only when these lattice defects are present can atoms or ions change position and lead to the occurrence of material transport. Various mechanisms can usually be employed here:

[0012] - particles jump into the lattice interstices, causing the interstices to cross the lattice, creating a net particle flow,

[0013] - Smaller particles can move in the lattice interstices, resulting in high diffusion coefficients,

[0014] - Two particles exchange positions or ring exchange occurs between multiple particles.

[0015] The chemical synthesis process is necessarily coupled with a diffusion process of the alloy into the metal matrix, which results in the formation of intermetallic compounds in the diffusion zone that improve wear resistance. The intermetallic compounds are embedded in a tougher, more ductile solid solution matrix consisting of the reactants of the diffusion partners, and this heterogeneous solid combination of different characteristic components is the core prerequisite for the desired functional optimization of the brake disc.

[0016] The appearance and performance characteristics of the solid solution matrix are very different from those of the metal from which it is derived. Intermetallic phases are matte, bright in color (light gray to dark gray), and have a smooth surface after machining. In addition, they are stabilized by their higher lattice energy and therefore have higher melting temperatures than their reactants. In addition, they have reduced conductivity of heat and electrical current, and they are sensitive to chemical reaction partners (i.e., to air, water, electrolytes, and The reactivity towards oxidants such as acidic media is significantly reduced, thus providing corrosion resistance and oxidation stability. The diffusion zone is also characterized by higher mechanical strength and increased hardness.

[0017] Preferably, the alloy is fully diffused into the matrix. Otherwise, alloy residues still present on the surface of the matrix will be removed from the surface.

[0018] Due to the diffusion zone of the brake element carrier body, the tribological properties of the material are improved and the corrosion resistance is increased.

[0019] If the alloy is based on aluminum and silicon, both corrosion protection and wear resistance can be further improved. This advantage is even more pronounced when silicon is present in an amount of 5 to 50 mass %, preferably 10 to 40 mass %, more preferably 15 to 30 mass %. Even in the range of 5 to 10 mass % or 7 to 15 mass %, the effect of silicon in the alloy on tribological properties, low thermal expansion and increased strength and wear resistance can be seen.

[0020] In general, the alloy also contains other alloying elements besides aluminum and silicon. These are the main alloying elements and the minor alloying elements. The main alloying elements are mainly elements of the second and / or third and / or fourth main group and / or the first and / or second and / or fourth and / or seventh subgroup of the periodic table. For the minor alloying elements, they are mainly selected from the elements of the third and / or fourth main group and / or the fourth and / or fifth and / or sixth and / or eighth subgroup of the periodic table.

[0021] In an aluminum-based alloy having a silicon content of 5 to 50 mass%, preferably 10 to 40 mass%, more preferably 15 to 30 mass%, at least one main alloying element is selected. The main alloying element is one or more of the following elements: magnesium, boron, titanium, manganese, copper or zinc. These elements may be present in the alloy in the following ranges:

[0022]

[0023] For example, magnesium, copper and zinc influence hardness and increase it, while manganese and titanium have a positive effect on heat and corrosion resistance.

[0024] In addition to the main alloying elements, there may be minor alloying elements in the alloy. Minor alloying elements are one or more of the following elements: gallium, indium, germanium, tin, zirconium, vanadium, chromium, iron, cobalt or nickel. These elements may be present in the alloy in the following ranges:

[0025]

[0026] In this alloy, the balance consists of aluminum and unavoidable impurities arising from the manufacturing process.

[0027] Among these alloys, ternary and quaternary alloys have proven to be particularly advantageous. These are alloys in which the typical alloying elements include three (ternary) or four (quaternary) substances. Only the components that determine the typical properties are calculated. The following ternary and quaternary alloys may also contain some of the major or minor alloying elements already listed.

[0028] Advantageous ternary alloys are as follows:

[0029] Al88 Si10 Mg2, Al88 Si10 B2, Al88 Si10 Ti2, Al88 Si10 Mn2, Al88 Si10 Cu2, Al88 Si10Zn2, Al83 Si15 Mg2, Al83 Si15 B2, Al83 Si15 Ti2, Al83 Si15 Mn2, Al83 Si15Cu2, Al83Si15 Zn2, Al78 Si20 Mg2, Al78 Si20 B2, Al78 Si20 Ti2, Al78 Si20 Mn2, Al78Si20 Cu2, Al78 Si20 Zn2.

[0030] Advantageous quaternary alloys are as follows:

[0031] Al86 Si10 Mn2 Mg2, Al86 Si10 Mn2 B2, Al86 Si10 Mn2 Ti2, Al86 Si10 Mn2Cu2, Al86Si10 Mn2 Zn2, Al81 Si15 Mn2 Mg2, Al81 Si15 Mn2 B2, Al81 Si15 Mn2 Ti2, Al81 Si15 Mn2Cu2, Al81 Si15 Mn2 Zn2, Al76 Si20 Mn2 Mg2, Al76 Si20 Mn2 B2, Al76Si20 Mn2 Ti2, Al76 Si20 Mn2 Cu2, Al76 Si20 Mn2 Zn2.

[0032] Another advantageous alloy is composed of 76.7 to 83.4 mass% of aluminum and 8.3 to 12.3 mass% of silicon and one or more elements selected from Mg, B, Ti, Mn, Cu, Zn, Ga, Ge, Sn, Sb, Zr, V, Cr, Co, Ni and unavoidable impurities generated during the manufacturing process. The sum of all composition components must be 100 mass%.

[0033] A particularly advantageous aluminum-based alloy is AlSi10, which has a silicon content of 10% by mass and the proportions of the main alloying elements in the following mass percentage ranges:

[0034] Magnesium < 0.5%,

[0035] Titanium < 0.05%,

[0036] Manganese < 0.1%,

[0037] Copper < 0.005%, and

[0038] Zinc < 0.005%.

[0039] The ranges of the proportions of the secondary alloying elements in the preferred aluminum-based AlSi10 alloy (mass %) are as follows:

[0040] Iron < 0.2%.

[0041] Therefore, the mass ratio of aluminum is the balance excluding inevitable impurities generated by the manufacturing conditions, that is, about 90 mass %. The sum of all components of the composition is 100 mass %.

[0042] Another particularly advantageous aluminum-based alloy has a silicon content of 10.04% by mass and the proportions of the main alloying elements are in the following mass percentage ranges:

[0043] Magnesium 0.31%,

[0044] Titanium 0.02%,

[0045] Manganese 0.01%,

[0046] Copper 0.001%, and

[0047] Zinc 0.003%.

[0048] The ranges of the proportions of the secondary alloying elements in the preferred aluminum-based AlSi10 alloy (mass %) are as follows:

[0049] Iron 0.16%.

[0050] Therefore, the mass ratio of aluminum is the balance excluding inevitable impurities generated by manufacturing conditions, that is, about 89.456 mass %. The sum of all components of the composition is 100 mass %.

[0051] The successfully tested samples (prototype) were composed in such a way that the alloy consisted of the following composition (mass %):

[0052] Al: 76.7 to 83.4;

[0053] Si: 8.3 to 12.3;

[0054] and

[0055] One or more elements selected from the group consisting of Mg, B, Ti, Mn, Cu, Zn, Ga, Ge, Sn, Sb, Zr, V, Cr, Co, Ni, Fe, and impurities;

[0056] The sum of all components of the composition must be 100% by mass.

[0057] Specifically, the samples were intended to have the following alloys (each in mass %):

[0058] -Si: 10% ±2%, preferably ±1%;

[0059] and / or

[0060] -Fe: <0.2%,

[0061] Preferably <0.18%,

[0062] Preferably 0.17%±0.02% or 0.16%±0.01%,

[0063] Specifically, 0.16%;

[0064] and / or

[0065] -Cu: <0.005%,

[0066] Preferably <0.003%,

[0067] Preferably 0.0015%±0.001%,

[0068] Specifically, 0.001%;

[0069] and / or

[0070] -Mg: <0.5%,

[0071] Preferably <0.4%,

[0072] Preferably 0.35% ± 0.05%, preferably 0.31% ± 0.03%,

[0073] Specifically, 0.31%;

[0074] and / or

[0075] -Mn: <0.1%,

[0076] Preferably <0.5%,

[0077] Preferably 0.01%±0.005%,

[0078] Specifically 0.01%;

[0079] and / or

[0080] -Ti: < 0.05%,

[0081] Preferably <0.035%,

[0082] Preferably 0.025% ± 0.01%,

[0083] Specifically, 0.02%;

[0084] and / or

[0085] -Zn: <0.005%,

[0086] Preferably <0.004%,

[0087] Preferably 0.0035%±0.001%,

[0088] Specifically, 0.003%;

[0089] Among them, it is preferred that at least 2, preferably at least 3, preferably at least 4, preferably at least 5, preferably at least 6 of the above-mentioned elements exist in any combination.

[0090] More preferably, all 7 of the above elements are present.

[0091] In particular B, Ga, Ge, Sn, Sb, Zr, V, Cr, Co, Ni and / or may additionally be present, but preferably the alloy contains no such elements,

[0092] The sum of all ingredients of the composition must be 100% by mass.

[0093] Each of the above alloys individually contributes to corrosion protection and improved wear resistance. They all have high mechanical strength, which means they all have high load-bearing capacity, pressure stability and dimensional stability.

[0094] In order to achieve the desired effect of increased corrosion protection and improved wear resistance, alloys can advantageously contain dopants. These dopants are foreign atoms which can penetrate into another solid at sufficiently high temperatures, move and embed themselves therein. The mechanisms which can play a role here are as follows:

[0095] - gap diffusion, i.e. through empty spaces in the crystal lattice,

[0096] - interstitial diffusion, i.e. between atoms in the crystal lattice,

[0097] - Place change, that is, the lattice positions of adjacent atoms are exchanged.

[0098] Diffusion occurs following Fick's law with or without dopants. This depends on various factors, such as the materials of the foreign substance and the target substance and their properties (crystal orientation), concentration differences, temperature, and the concentration of other dopants in the lattice. For the purpose of simplicity, in this patent application, only the term "crystal" is used to refer to the lattice. The speed at which diffusion occurs depends on the size of the atoms and the type of diffusion in the substrate. A small diffusion coefficient usually leads to a long processing time. As mentioned above, an important aspect of diffusion and the resulting doping profile is the concentration difference. The doping profile is mainly determined by the characteristics of the dopant source. The dopant source can be a non-depletable source or a depletable source. In the case of a non-depletable dopant source, it is assumed that the dopant concentration at the surface of the crystal is constant, so the foreign atoms diffused deep into the crystal are directly replaced from the dopant source. This means that as the diffusion time and temperature increase, the dopant diffuses deeper into the crystal, the amount of dopant increases, and the concentration at the surface remains constant. In contrast, in the diffusion from a depletable dopant source, the amount of dopant is constant. Here, the penetration depth of the dopant increases with increasing diffusion time and temperature, but at the same time the concentration at the surface decreases.

[0099] The dopants used for the alloy are selected from the third main group and / or the first and / or third and / or fourth and / or fifth and / or sixth and / or seventh and / or eighth subgroups of the periodic table and / or the lanthanides.

[0100] The alloy may contain one or two dopants. In particular cases, three, four or more dopants or additives may be used.

[0101] Preferably, the following elements (mass %) are used as dopants:

[0102]

[0103] These (when added to the above alloys) lead to the selective formation of the desired intermetallic phases, as they act as catalysts or inhibitors. The diffusion of the alloy and the addition of the dopant leads to a change in the structure. According to the proposal, the diffusion zone has a different structure than the carrier body. This increases the hardness of the brake disc carrier body and thus also increases the wear resistance of the brake disc carrier body.

[0104] Steel, cast steel, centrifugal casting, grey cast iron or ductile iron are suitable for the base body of the brake element carrier body. An aluminium base body is also possible.

[0105] These metals are ideal for diffusing the above alloys, with or without dopants. The diffusion zone resulting from the diffusion of the alloy into the matrix has a higher hardness (in Vickers) than the matrix material. This forms the basis for the improved wear behavior.

[0106] In order to produce a diffusion zone with sufficient hardness, it is advantageous if the alloy layer has a thickness of 0.1 mm to 0.4 mm. An alloy layer thickness of 0.2 mm to 0.3 mm has proven to be particularly advantageous.

[0107] Particularly good wear resistance (ie hardness) and associated good corrosion protection are achieved when the thickness of the diffusion zone is 0.05 mm to 0.6 mm. The desired properties are particularly evident when the thickness of the diffusion zone is 0.2 mm to 0.3 mm.

[0108] The increase in hardness is due to diffusion into the diffusion zone of the brake element carrier body. This has a medium hardness. The average hardness of the diffusion zone is increased by a factor of 1.0 to 8, preferably 1.5 to 5, compared to the average hardness of the carrier body.

[0109] The improvement, i.e. the increase in hardness compared to the base body, depends on the base material. Thus, in the case of a carrier body of gray cast iron or centrifugal casting or steel or cast steel, the average hardness of the diffusion zone is increased by a factor of 2.5 to 8, in particular by a factor of 2 to 5, compared to the average hardness of the carrier body. In the case of a carrier body of aluminum, the average hardness of the diffusion zone is increased by a factor of 1.5 to 4, in particular by a factor of 1.5 to 3, compared to the average hardness of the carrier body, in terms of HV hardness.

[0110] The maximum deviation of the hardness distribution along the longitudinal, transverse and vertical axes of the diffusion zone or along the radius and angular coordinates of the diffusion zone from the average hardness (HV hardness) of the diffusion zone is 10% to 15%.

[0111] The structure of the diffusion zone is different from that of the matrix, and the diffusion zone has a solid solution matrix formed by binary or ternary or higher intermetallic phases.

[0112] A solid solution (Mc) is a crystal or microcrystal consisting of at least two different chemical elements in which foreign atoms or ions are statistically distributed. These atoms or ions can be inserted into interstitial sites (intercalation solid solution or interstitial solution) or can replace atoms of other elements by substitution (substitutional solid solution). If solid solutions have metallic properties, they are also called alloys (Wikipedia).

[0113] Intermetallic compounds (also called intermetallic phases or intermediate phases) are homogeneous chemical compounds of two or more metals. Compared to alloys, they exhibit a lattice structure that is different from the lattice structure of the constituent metals.

[0114] Here, there is no pure metal precipitation in the solid solution matrix of the diffusion zone.

[0115] By diffusing the alloy, in particular the alloy with dopants, into the matrix of the brake element carrier body, the proposed diffusion zone can be realized in a targeted and purpose-oriented manner in the sense of a functional layer. This results in a graded layer system, within which the boundaries between the individual phases are almost parallel.

[0116] The intermetallic phase of the proposed brake element carrier element has a gradually increasing concentration of iron or carbon and a gradually decreasing concentration of aluminum and / or silicon and / or dopants as the distance from the substrate surface increases.

[0117] In other words, the diffusion zone has a hierarchical structure of discrete, precisely defined binary, ternary or higher order intermetallic phases of Daltonic bulk chemistry with varying proportions of the original matrix elements iron and carbon and varying proportions of the layer elements aluminum, silicon, various alloying elements and dopants introduced into the matrix by diffusion.

[0118] The solid solution matrix is ​​characterized by increased toughness and ductility compared to the intermetallic phases embedded in the solid solution matrix.

[0119] Diffusion alloys with and without dopants provide the diffusion zone with a higher melting point and / or worse, lower thermal conductivity and / or worse, lower electrical conductivity and / or higher mechanical strength and / or higher hardness and / or reactivity to chemical reactants than the base metal.

[0120] It should be clearly pointed out here again that the desired effect, namely improved wear resistance and corrosion protection, is achieved due to the fact that the intermetallic phases formed during the diffusion of the alloys (especially alloys with dopants) are an integral part of the overall structure of the matrix diffusion zone. Even though these intermetallic phases are of metallic origin, they themselves exhibit ceramic properties. This is due to the change in the bonding conditions in the lattice electron field, whereby the intermetallic compounds have a valence defined by the localized electron pairs. This makes Acidic media attack is more difficult, resulting in the required high corrosion resistance.

[0121] According to a second aspect of the invention, this object is achieved by a brake disc or brake drum having a brake element carrier body, which has an area designed as a friction surface and an area designed as a contact surface. In another embodiment, the brake element carrier body used here can be designed as described above. A brake disc with two opposing friction surfaces is particularly advantageous.

[0122] Such brake discs or brake drums offer more effective long-term corrosion protection and increased wear resistance.

[0123] Both friction surface and contact surface form the functional area of ​​the brake disc or brake drum. The friction surface is the surface on which the brake pad acts with a defined normal force, whereby the desired braking effect is achieved by sliding friction between the two. The contact surface is a surface that extends at least partially in the radial direction. It is oriented in the circumferential direction of the brake disc, whereby the normal vector also acts in the circumferential direction. This allows the transmission of braking torques. The contact surface can be located, for example, on the brake chamber of the brake disc.

[0124] The recommended alloy layer thickness on the brake disc or brake drum is 0.1 mm to 0.4 mm. A particularly good diffusion effect is achieved with an alloy layer thickness of 0.2 mm to 0.3 mm.

[0125] It is proposed that a particularly hard, wear-resistant brake disk or brake drum has a diffusion zone with a thickness of 0.05 mm to 0.6 mm, preferably 0.3 mm to 0.6 mm.

[0126] During braking, the friction surface is particularly affected. Therefore, the thickness of the applied alloy layer and the resulting diffusion zone can have different thicknesses at the friction surface and the contact surface. It is particularly advantageous if the thickness of the diffusion zone of the friction surface is 0.3 mm to 0.6 mm.

[0127] For the desired braking process, it is particularly advantageous if the friction surface and the contact surface are annular. However, it is also possible that only one of the two surfaces is annular.

[0128] During the braking process, heat can be generated due to friction. If the temperatures generated are too high, this can have a negative impact not only on the service life of the brake disc or brake drum, but also on the braking process itself. Therefore, it is advisable, for example, to provide ventilation channels to achieve internally ventilated brake discs. These can be provided on and in the base body, or on or in the base body.

[0129] According to a third aspect of the invention, this object is achieved by a brake pad back plate or a brake shoe comprising a brake element carrier plate. Here, in special cases, a brake element carrier plate may also be provided as described above.

[0130] In order to achieve an optimal effect of the diffusion, it is advantageous if the thickness of the alloy layer on the brake pad back plate or the brake shoe is 0.1 mm to 0.3 mm, preferably 0.1 mm to 0.2 mm.

[0131] Increased hardness and wear resistance can be achieved when the thickness of the diffusion zone in the brake pad back plate or brake shoe is 0.05 mm to 0.3 mm. A diffusion zone thickness of 0.05 mm to 0.15 mm has proven to be particularly advantageous.

[0132] In order to enable braking operation during use, it is recommended that brake pads be applied to the outer surface of the alloy.

[0133] According to a fourth aspect of the present invention, the object is achieved by: a method for manufacturing a brake element carrier body, comprising the following steps:

[0134] 1. Provide a substrate,

[0135] 2. Use hard ceramic material for sandblasting to remove the oxide layer on the surface of the substrate.

[0136] 3. Applying an aluminum-based alloy to a carrier body,

[0137] 4. Tempering the carrier body with the applied alloy.

[0138] The method can be used in particular for producing the above-mentioned brake element carrier body.

[0139] The carrier body provided for the brake element carrier body may be cast or stamped.

[0140] Grit blasting is particularly important. This removes iron oxides from the surface of the brake disc to be coated. If these iron oxides are not removed, they can act as a barrier to the inward diffusion of elements of the applied alloy into the metal matrix structure.

[0141] In the case of heating of the base body prior to the sandblasting, a particularly good diffusion effect (ie, rapid diffusion) can be achieved with regard to production time, and the quality or depth of the diffusion can be achieved.

[0142] Materials with a low embedding affinity for the matrix material are particularly suitable for sandblasting. Use hard ceramic materials. Corundum, quartz, boron carbide, titanium carbide, silicon carbide and chromium carbide have proven to be particularly suitable. These can be used for sandblasting alone or in combination.

[0143] The sandblasting process not only removes unwanted elements from the substrate surface, but also prepares it for the subsequent application of the alloy. This should diffuse quickly and easily into the structure of the metal substrate. This can be achieved advantageously if the sandblasting process produces a roughness Rz of 5 μm to 10 μm on the substrate surface. The roughness leads to a close micro-form-locking bond between the applied alloy layer and the substrate material.

[0144] For sandblasting with hard ceramic materials, a particle size of 0.5 mm to 1.5 mm, in particular 0.8 mm to 1.2 mm, has proven to be particularly effective for producing the roughness.

[0145] It has proven to be very effective and efficient if the sandblasting is carried out at an angle of 45°±10° to the surface of the brake element carrier body.

[0146] According to the invention, in step 3 of the method, an aluminum-based alloy is applied to the carrier body. The alloy is based on aluminum and silicon and may, but does not necessarily, contain dopants. The variety of alloys and dopants has been described in detail above. Here, please refer to the above.

[0147] According to the present invention, the alloying is performed by a high velocity flame spraying process, an arc wire spraying process or a powder coating process.

[0148] In high velocity flame spraying (HVOF), gases are continuously burned at high pressure in a combustion chamber into which powdered spray additives are fed into the central axis. When using HVOF, a high flow rate of the gas jet is advantageous; this is achieved by the high pressure of the fuel gas / oxygen mixture generated in the combustion chamber and the expansion nozzle usually arranged downstream. This accelerates the spray particles to high particle velocities, resulting in extremely dense spray layers with excellent bonding properties. Propane, propylene, ethylene, acetylene and hydrogen can be used as fuel gases.

[0149] In arc wire spraying, two wire-shaped spray additives made of the same or different materials are melted in an electric arc and spun onto the prepared workpiece surface using an atomizing gas (e.g., compressed air).

[0150] In powder coating, powder is sprayed onto a material, usually electrically conductive, and then tempered. The powder melts on the metal surface and forms a uniform layer that protects against corrosion, for example.

[0151] Applying the alloy to the substrate directly after blasting is particularly useful as this reduces the risk of iron oxide re-forming or depositing on the substrate surface.

[0152] Step 4 involves tempering the carrier body with the applied alloy. This accelerates the diffusion process and allows controlled incorporation of the dopant into the lattice structure.

[0153] The heat treatment of the coated brake disc, also called tempering, leads to an inward diffusion of alloying elements of the layer sprayed on the surface of the substrate. During the tempering treatment, the product is exposed to a certain temperature T for a period of time t in order to generate, accelerate or promote certain processes (e.g. chemical processes). At temperatures below the melting point of the respective sprayed layer, this inward diffusion takes place very slowly, but above the melting point, it takes place much faster. The range of +590°C to +750°C has proven to be a functionally and economically suitable interval for the maximum holding temperature. The tempering treatment or the tempering of the substrate with the applied alloy can be carried out along a temperature profile of 600°C to 750°C. The temperature profile can be linear, exponential or periodic. The temperature profile can also have a heating phase, a holding phase and a cooling phase.

[0154] At the beginning of the tempering treatment, the maximum concentration gradient between the material systems still exists as a driving gradient for diffusion. For the initial rapid diffusion, it is sufficient that the temperature of the molten layer is only slightly above its melting point. As the diffusion proceeds, the driving concentration gradient tends to flatten out, so in order to maintain rapid diffusion, the level of the holding temperature is increased continuously or in steps to compensate for the effect of the reduced gradient through higher thermodynamics. Thus, the temperature profile can be adapted to the concentration gradient of the alloy diffusing into the metal of the matrix.

[0155] The reason for adjusting the holding temperature is to minimize the collective thermal impact on the metal matrix structure and protect it during the heat treatment. When melting the sprayed layer so that it diffuses rapidly inward into the matrix, the melt forms an effective barrier to oxygen from the air, which is captured by the air-facing surface of the melt and chemically bound there in the form of aluminum oxide. The formed oxide layer prevents oxygen from further entering the melt. Therefore, during the tempering process, no oxygen from the air is stored in the diffusion layer. Due to the high electropositivity of aluminum and its position in the chemical sequence, it binds oxygen more preferentially than silicon.

[0156] In order to obtain an improved result (ie a hard and wear-resistant diffusion zone, ie complete, at least substantially complete diffusion of the alloy into the matrix), tempering is carried out according to the invention for 180 to 360 minutes, preferably 210 to 300 minutes.

[0157] According to a fifth aspect of the present invention, the object is achieved by: a method for manufacturing a brake disc or a brake drum, comprising the following steps:

[0158] 1. Provide a brake element carrier body;

[0159] 2. Remove alloy until the diffusion zone is reached to create the friction surface.

[0160] The method can be used to manufacture the above brake disc or brake drum. The brake element carrier body provided in step 1 can be the above brake element carrier body or a brake element carrier body manufactured according to the above method. Therefore, here, please refer to the above.

[0161] In order to produce a clean, brake-usable friction surface, the excess alloy must be removed until the diffusion zone is reached. According to the proposal, the removal can be carried out mechanically. In this case, grinding or turning the alloy is proposed. By removing the excess alloy, one or more friction surfaces of the brake disc are formed. The friction surface has the properties of the solid solution matrix of the diffusion zone, i.e. it is very hard and wear-resistant.

[0162] The removal depends on the material and the thickness of the alloy layer. However, it has proven to be advantageous to remove at most 0.05 mm or at most 1 mm or at most 1.5 mm of alloy. The removal can be carried out in more than one step so that the surface can be assessed from time to time.

[0163] Furthermore, the brake disc or brake drum can have a metal matrix having a diffusion zone consisting of matrix materials iron and carbon and previously sprayed main layer materials aluminum, silicon, magnesium and manganese, the diffusion zone being produced by heat treatment and inward diffusion of the layer materials; wherein the single layer thickness of the diffusion zone is 0.05 mm to 0.6 mm, preferably 0.3 mm to 0.6 mm.

[0164] In this case, the diffusion zone contains the elements iron, carbon, aluminum, silicon, magnesium and manganese, wherein the elements iron, aluminum, silicon and manganese form new binary, ternary and quaternary intermetallic phases in the form of many self-sufficient and individually growing crystals, which are embedded in the same new parallel coexisting solid solution matrix composed of the above six elements.

[0165] Furthermore, the resulting diffusion layer can be designed in such a way that in the newly formed solid solution matrix, the matrix elements iron and carbon increase continuously with increasing depth, while the sprayed layer elements aluminum, silicon, magnesium and manganese decrease continuously with increasing depth. In the crystals of the newly formed intermetallic phase, the concentrations of the above elements also change with increasing depth, qualitatively following the same trend, but not continuously, but in the form of discrete jumps depending on the compositional recipe of the respective main intermetallic phase.

[0166] According to a sixth aspect of the present invention, the object is achieved by: a method for manufacturing a brake pad backing plate or a brake drum, comprising the following steps:

[0167] 1. Provide a brake element carrier body;

[0168] 2. Apply the brake pad to the alloy surface to create a friction surface or contact surface.

[0169] The method can be used to manufacture the above-mentioned brake pad back plate or brake shoe. The brake element carrier body provided in step 1 can be the above-mentioned brake element carrier body or a brake element carrier body manufactured according to the above-mentioned method. Therefore, here, please refer to the above.

[0170] The brake pad applied in step 2 can be bonded or welded to the alloy surface of the brake element carrier body. Thus, bonding and welding of the brake pad is feasible.

[0171] Brake pads can be constructed as follows:

[0172] - 30 to 65 mass % of metal (steel, iron or brass) mixed with graphite, filler and binder, or

[0173] - 10% to 30% by mass of metal (copper or steel), fibers made of glass, rubber, carbon or aramid, which can provide better braking performance at high speeds, or

[0174] - organic or mineral fibers and high temperature resistant synthetic or natural resins, which reduce brake pad wear and create less visible dust, or

[0175] - Ceramic fibers, fillers and binders, such as carbon fiber reinforced silicon carbide, which can reduce volume, or

[0176] - sintered metal powders, which have a longer service life and improved heat resistance, reducing the loss of braking effect during intensive use, or

[0177] - Low proportion of metal and high proportion of organic or mineral fibers, resulting in quieter operation and less wear.

[0178] According to a seventh aspect of the present invention, the object is achieved by: a brake system comprising a brake disc or brake drum as described above and a brake pad back plate or brake shoe as described above.

[0179] Disc brakes consist of a brake disc and a brake pad backing plate. The essential components of drum brakes include brake drums and brake shoes.

[0180] According to a further aspect of the invention, the object is achieved by a motor vehicle, a rail vehicle, a stationary industrial brake system or a wind turbine comprising the brake system. BRIEF DESCRIPTION OF THE DRAWINGS

[0181] Figure 1 : A cross section of a brake element carrier body for a brake disc or brake drum or for a brake pad back plate or brake shoe during sandblasting;

[0182] Figure 2 : A cross section of a brake element carrier body for a brake disc or brake drum or for a brake pad back plate or brake shoe with an applied alloy;

[0183] Figure 3 : cross section of a brake element carrier body for a brake disc or brake drum or for a brake pad back plate or brake shoe during the tempering process;

[0184] Figure 4 : Cross section of a brake element carrier body for a brake disc or brake drum or for a brake pad back plate or brake shoe after tempering;

[0185] Figure 5 : Cross section of a brake element carrier body for a brake disc or brake drum during removal of excess alloy;

[0186] Figure 6 : Cross section of brake disc or brake drum;

[0187] Figure 7 : Schematic diagram of a brake disc with a brake chamber;

[0188] Figure 8 : Schematic diagram of brake pad back plate;

[0189] Fig. 9 : Cross-section of the brake system including the brake disc and brake pad backing plate. DETAILED DESCRIPTION

[0190] Figures 1 to 5 A method for manufacturing a brake element carrier body for a brake disc or brake drum or for a brake pad back plate or brake shoe is shown.The claimed brake element carrier body for a brake disc or brake drum or for a brake pad back plate is described in the course of the following description of the figures.

[0191] During the manufacturing process of a brake element carrier body 1 for a brake disc or brake drum or for a brake pad back plate or brake shoe, a base body 2 is provided, which is made of a metal. In this case, the base body 2 is made of gray cast iron. In other embodiments, the base body 2 is made of steel, cast steel, centrifugal casting or ductile iron.

[0192] In order to obtain a clean and oxide-free (especially iron oxide-free) surface, it is necessary to remove these oxide layers ( Figure 1 ). In the present embodiment, the surface 3 of the substrate 2 is sandblasted with corundum having a particle size of 0.5 mm to 1.5 mm, thereby producing the desired roughness of 5 μm to 10 μm. The sandblasting is performed at an angle of about 40°. Angles between 35° and 55° are particularly suitable for sandblasting.

[0193] In other embodiments, quartz, boron carbide, titanium carbide, silicon carbide or chromium carbide are used to remove these oxide layers. Mixtures of hard ceramic materials can also be used. Only care should be taken here to ensure that the substances used have no affinity for diffusion into the matrix.

[0194] Prior to this treatment, the substrate may be heated, which improves the removal of the oxide layer.

[0195] After the sandblasting, the aluminum-based alloy 5 is applied to the base body. Figure 2 The state after alloy 5 is applied to surface 3 of substrate 2 is shown. Alloy 5 can be applied as one or more layers. In the embodiment, alloy layer thickness (ALT) is applied with a thickness of 0.25 mm. Generally, the desired effect can be achieved when the alloy layer thickness is 0.1 mm to 0.4 mm, preferably 0.2 mm to 0.3 mm.

[0196] For alloys based on aluminum, a combination with silicon has proven to be particularly advantageous for wear resistance. Silicon should be 5 to 50% by mass. Alloys with an aluminum content of 70 to 90% by mass and a silicon content of 5 to 25% by mass have proven to be particularly advantageous. In a first example, an alloy Al88 Si10 Mg2 with antimony as a dopant is applied, which is applied here using a high-velocity flame spraying process.

[0197] Table 1 below shows other preferred aluminum silicon alloys, and Table 2 shows usable dopants.

[0198]

[0199]

[0200]

[0201] In other embodiments, one of the aluminum silicon alloys No. 1 to No. 33 may be combined with more than one of the dopants a) to t). Since the dopants are incorporated into the crystal lattice of the substrate 1 together with the alloy, corrosion protection and wear resistance are improved.

[0202] The diffusion process can then begin: the alloy 5 diffuses into the matrix 2 .

[0203] After application, the carrier body with the applied alloy is tempered. The tempering is carried out in a tempering furnace 6. The temperature range is between 590° C. and 750° C., the temperature profile here being a period of 270 minutes. The temperature profile has a heating phase, a holding phase and a cooling phase. During the heating phase, the carrier body with the alloy is heated linearly from 590° C. to 750° C. over a period of about 60 minutes, held at 750° C. for 150 minutes in the holding phase and cooled from 750° C. to 590° C. in 60 minutes in the cooling phase. However, a cycle can also be run here. The duration of the tempering treatment can vary. In all examples, the best results were obtained with a tempering time of 180 minutes to 360 minutes, and the best results were obtained with a tempering time of 210 minutes to 300 minutes. After that, no improvement can be observed from a longer tempering treatment.

[0204] Tempering activates the equalization process of the concentration difference between the matrix 2 and the alloy 5. The atoms and ions of the alloy and the dopant settle in the lattice defects of the matrix crystal lattice and are deposited there. This process forms a diffusion zone 7, which consists of a solid solution matrix with an intermetallic phase.

[0205] In the present example, a diffusion zone with a thickness of 0.2 mm to 0.3 mm has been established. Good results were achieved at 0.05 mm to 0.6 mm. During the tempering treatment, the alloy was fully or almost fully diffused. In the example, the alloy was not fully diffused, which means that remnants of the alloy are still present ( Figure 4 ).

[0206] This is not a problem for the brake element carrier body and is even advantageous for the storage of the brake element carrier body.

[0207] From the final manufacturing result of the brake element carrier body 1 (such as Figure 4 Starting with the brake pad backing plate 12 or the brake shoe (not shown here), the brake pad backing plate 12 or the brake shoe (not shown here) can now be manufactured. A brake pad 13 made of sintered metal is applied (in this case bonded on). A smaller alloy layer thickness ALT can be used for the brake element carrier body for the brake pad backing plate 12 or the brake shoe. For this range of applications, a layer thickness of 0.1 mm to 0.3 mm is suitable, resulting in a diffusion zone 7 with a layer thickness of 0.05 mm to 0.3 mm, preferably 0.05 mm to 0.15 mm.

[0208] To manufacture a brake disc or brake drum, the brake element carrier body is Figures 1 to 4 The finished brake disc 8 or brake drum requires a friction surface 9 and a contact surface 10 for braking. To achieve this, excess alloy 5 ( Figure 4 ).according to Figure 5 The excess alloy 5a is removed mechanically (i.e., by grinding or turning) to expose the diffusion zone 7, thereby producing Figure 7 The finished brake disc or brake drum shown has a cross section as shown in Figure 6 This is particularly necessary for the braking function, since otherwise the pressed brake pads would be damaged, which would have a negative impact on the service life of both parts of the brake system.

[0209] Brake disc 8( Figure 7 ) is composed of a brake element carrier body 1, the brake element carrier body 1 is according to Figures 1 to 4 The brake disc is manufactured from 200 mm / s and has a friction surface 9 and a contact surface 10. The friction surface 9 is formed by removing excess alloy 5a up to the diffusion zone 7. In order to transmit torque, the brake disc has a brake chamber 11 with the contact surface 10.

[0210] Brake pad backing plate 12( Figure 8 ) comprises a brake element carrier body 1 and a brake pad 13, wherein the brake element carrier body 1 is according to Figures 1 to 4To manufacture, the brake pad 13 is bonded in this embodiment. In the embodiment shown, a brake pad 12 made of sintered metal powder is used.

[0211] Braking system 14( Fig. 9 ) comprises a brake disc 8 and a brake pad backing plate 12. The brake system shows the braking process, when the brake pad 13 of the brake pad backing plate 12 is pressed with a normal force onto the friction surface 9 of the brake disc. The pressure is applied by a hydraulic piston.

[0212] The brake system may be used, for example, in motor vehicles, rail cars, wind turbines or stationary industrial brake systems.

[0213] List of reference symbols used:

[0214] 1 Brake element carrier body

[0215] 2 Matrix

[0216] 3 Surface

[0217] 4 Hard ceramic materials

[0218] 5 Aluminum-based alloys

[0219] 5a Excess alloy

[0220] 6 tempering furnace

[0221] 7 Diffusion zone

[0222] 8 Brake disc

[0223] 9 Friction Surface

[0224] 10 Application surface

[0225] 11 Brake chamber

[0226] 12 Brake pad backing plate

[0227] 13 Brake pads

[0228] 14 Braking system

[0229] LSD alloy layer thickness

Claims

1. Brake element carrier body, - has a metal base, in, - the surface of the base body is at least partially, preferably completely, coated with the alloy, and - In the diffusion zone, the alloy diffuses into the matrix.

2. The brake element carrier body according to claim 1, It is characterized in that The alloy is an alloy based on aluminum and silicon.

3. The brake element carrier body according to claim 1 or 2, It is characterized in that The alloy contains silicon in a numerical range of 5 mass % (lower limit) to 50 mass % (upper limit), wherein: The lower limit may be specifically defined as 6 mass %, 7 mass %, 8 mass %, 9 mass % or 10 mass % of silicon, and The upper limit may be specifically defined as 40 mass%, 30 mass%, 20 mass%, 15 mass%, 14 mass%, 13 mass%, 12 mass%, 11 mass% or 10 mass% of silicon, Preferably, the numerical range may be limited to 10% to 40% by mass, 15% to 30% by mass, 10% ± 5% by mass, 10% ± 4% by mass, 10% ± 3% by mass, 10% ± 2% by mass or 10% ± 1% by mass of silicon.

4. The brake element carrier body according to claim 3, It is characterized in that The alloy contains silicon in a numerical range of 9 mass % as a lower limit to 11 mass % as an upper limit.

5. A brake element carrier body according to any one of the preceding claims, It is characterized in that The alloy is an alloy based on aluminum and silicon containing a main alloying element, wherein the main alloying element is selected from the second and / or third and / or fourth main group and / or the first and / or second and / or fourth and / or seventh subgroup of the periodic table of the elements, Preferably, the alloy contains secondary alloying elements, wherein the secondary alloying elements are selected from the third and / or fourth main group and / or the fourth and / or fifth and / or sixth and / or eighth subgroup of the periodic table of the elements.

6. A brake element carrier body according to any one of the preceding claims, It is characterized in that The alloy comprises 5% to 50% by mass of silicon and one or more main alloying elements, wherein the main alloying elements are selected from one of the following elements (in mass %): Magnesium: 0.1 to 2, and / or boron: 0.1 to 10, and / or Titanium: 0.1 to 5, and / or Manganese: 0.5 to 5, and / or Copper: 0.1 to 5, and / or Zinc: 0.1 to 5, The remainder consists of aluminum and impurities.

7. The brake element carrier body according to claim 6, It is characterized in that The alloy contains one or more minor alloying elements, wherein the minor alloying elements are selected from one of the following elements (in mass %): Gallium: 0.1 to 1, and / or indium: 0.1 to 1, and / or germanium: 0.1 to 1, and / or tin: 0.1 to 1, and / or zirconium: 0.1 to 1, and / or vanadium: 0.1 to 1, and / or Chromium: 0.1 to 1, and / or iron: 0.1 to 1, and / or Cobalt: 0.1 to 1, and / or Nickel: 0.1 to 1.

8. Braking element carrier body according to any one of the preceding claims, It is characterized in that The alloy is one of the following ternary alloys: Al88 Si10 Mg2, Al88 Si10 B2, Al88 Si10 Ti2, Al88 Si10 Mn2, Al88 Si10 Cu2, Al88 Si10 Zn2, Al83 Si15 Mg2, Al83 Si15 B2, Al83 Si15 Ti2, Al83 Si15 Mn2, Al83 Si15 Cu2, Al83 Si15 Zn2, Al78 Si20 Mg2, Al78 Si20 B2, Al78 Si20 Ti2, Al78 Si20 Mn2, Al78 Si20 Cu2, Al78 Si20 Zn2.

9. A brake element carrier body according to any one of the preceding claims, It is characterized in that The alloy is one of the following quaternary alloys: Al86 Si10 Mn2 Mg2, Al86 Si10 Mn2 B2, Al86 Si10 Mn2 Ti2, Al86 Si10 Mn2 Cu2, Al86 Si10 Mn2 Zn2, Al81 Si15 Mn2 Mg2, Al81 Si15 Mn2 B2, Al81 Si15 Mn2 Ti2, Al81 Si15 Mn2 Cu2, Al81 Si15 Mn2 Zn2, Al76 Si20 Mn2 Mg2, Al76 Si20 Mn2 B2, Al76 Si20 Mn2 Ti2, Al76 Si20 Mn2 Cu2, Al76 Si20 Mn2 Zn2.

10. A brake element carrier body according to any one of the preceding claims, It is characterized in that The alloy consists of the following composition (in mass %): Al: 76.7 to 83.4, Si: 8.3 to 12.3, One or more elements selected from the group consisting of Mg, B, Ti, Mn, Cu, Zn, Ga, Ge, Sn, Sb, Zr, V, Cr, Co, Ni, Fe, and Impurities; Therein, the sum of all ingredients of the composition must be 100% by weight.

11. The brake element carrier body according to claim 10, It is characterized in that The alloy consists of the following composition (in mass %): -Si: 10% ±2%, preferably ±1%; and / or -Fe: <0.2%, Preferably <0.18%, Preferably 0.17%±0.02% or 0.16%±0.01%, Specifically, 0.16%; and / or -Cu: <0.005%, Preferably <0.003%, Preferably 0.0015%±0.001%, Specifically, 0.001%; and / or -Mg: <0.5%, Preferably <0.4%, Preferably 0.35% ± 0.05%, preferably 0.31% ± 0.03%, Specifically, 0.31%; and / or -Mn: <0.1%, Preferably <0.5%, Preferably 0.01%±0.005%, Specifically 0.01%; and / or -Ti: < 0.05%, Preferably <0.035%, Preferably 0.025% ± 0.01%, Specifically, 0.02%; and / or -Zn: <0.005%, Preferably <0.004%, Preferably 0.0035%±0.001%, Specifically, 0.003%; Among them, it is preferred that at least 2, preferably at least 3, preferably at least 4, preferably at least 5, preferably at least 6 of the above elements are present in any combination. More preferably, all 7 of the above elements are present. In particular B, Ga, Ge, Sn, Sb, Zr, V, Cr, Co, Ni and / or may additionally be present, but preferably the alloy contains no such elements, The sum of all ingredients of the composition must be 100% by mass.

12. A brake element carrier body according to any one of the preceding claims, It is characterized in that The alloy contains a dopant; preferably, the dopant is selected from the third main group and / or the first and / or third and / or fourth and / or fifth and / or sixth and / or seventh and / or eighth subgroups of the periodic table and / or lanthanides.

13. A brake element carrier body according to any one of the preceding claims, It is characterized in that The alloy contains one or two or three or more dopants.

14. A brake element carrier body according to any one of the preceding claims, It is characterized in that The dopant is selected from one or more of the following elements (in mass %): Antimony: 0.1 to 1, and / or Bismuth: 0.01 to 0.1, and / or Scandium: 0.01 to 0.1, and / or Yttrium: 0.01 to 0.1, and / or Lanthanum: 0.01 to 0.1, and / or Ce: 0.01 to 0.1, and / or Hafnium: 0.01 to 0.1, and / or Niobium: 0.01 to 0.1, and / or Tantalum: 0.01 to 0.1, and / or Molybdenum: 0.01 to 0.1, and / or Tungsten: 0.01 to 0.1, and / or Rhenium: 0.01 to 0.1, and / or Ruthenium: 0.01 to 0.1, and / or Osmium: 0.01 to 0.1, and / or Rhodium: 0.01 to 0.1, and / or Iridium: 0.01 to 0.1, and / or Palladium: 0.01 to 0.1, and / or Platinum: 0.01 to 0.1, and / or Silver: 0.01 to 0.1, and / or Gold: 0.01 to 0.

1.

15. Braking element carrier body according to any one of the preceding claims, It is characterized in that The base body is made of steel, cast steel, centrifugal casting, grey cast iron or ductile iron.

16. A brake element carrier body according to any one of the preceding claims, It is characterized in that The base body is made of aluminum.

17. A brake element carrier body according to any one of the preceding claims, It is characterized in that The thickness of the alloy layer is 0.1 mm to 0.4 mm, preferably 0.2 mm to 0.3 mm.

18. Braking element carrier body according to any one of the preceding claims, It is characterized in that The thickness of the diffusion zone is 0.05 mm to 0.6 mm, preferably 0.2 mm to 0.3 mm.

19. A brake element carrier body according to any one of the preceding claims, It is characterized in that The diffusion region has a different structure than the carrier body.

20. A brake element carrier body according to any one of the preceding claims, It is characterized in that The diffusion zone has a solid solution matrix formed by binary or ternary or higher metallic phases.

21. The brake element carrier body according to claim 20, It is characterized in that As the distance from the substrate surface increases, the concentration of iron or carbon in the solid solution matrix increases continuously, and the concentration of aluminum and / or silicon and / or dopants decreases continuously.

22. The brake element carrier body according to claim 17 or 18, It is characterized in that As the distance from the substrate surface increases, the concentration of iron or carbon in the intermetallic phase gradually increases, and the concentration of aluminum and / or silicon and / or dopants gradually decreases.

23. The brake element carrier body according to any one of claims 20 to 22, It is characterized in that The solid solution matrix has increased toughness and ductility compared to the intermetallic phases embedded in the solid solution matrix.

24. A brake element carrier body according to any one of the preceding claims, It is characterized in that The diffusion zone has a higher melting point and / or a lower thermal conductivity and / or a lower electrical conductivity and / or a higher mechanical strength and / or a higher hardness and / or a lower reactivity towards chemical reaction partners than the base metal.

25. A brake element carrier body according to any one of the preceding claims, It is characterized in that There is a solid solution matrix in the diffusion zone without pure metal precipitation.

26. A brake element carrier body according to any one of the preceding claims, It is characterized in that The diffusion zone has a medium hardness, wherein the average hardness of the diffusion zone is increased by 1.0 to 8 times, preferably 1.5 to 5 times, compared to the average hardness of the carrier body.

27. A brake element carrier body according to any one of the preceding claims, It is characterized in that In the case of a carrier body of grey cast iron or centrifugal casting or steel or cast steel, the average hardness of the diffusion zone is increased by a factor of 2.5 to 8, in particular by a factor of 2 to 5, compared to the average hardness of the carrier body.

28. A brake element carrier body according to any one of the preceding claims, It is characterized in that In the case where the carrier material of the carrier body is aluminum, the average hardness of the diffusion zone is increased by a factor of 1.5 to 4, in particular by a factor of 1.5 to 3, in HV hardness compared to the average hardness of the carrier body.

29. A brake element carrier body according to any one of the preceding claims, It is characterized in that The maximum deviation of the hardness distribution along the longitudinal, transverse and vertical axes or along the radius and angular coordinates of the diffusion zone from the average hardness (HV hardness) of the diffusion zone is 10% to 15%.

30. A brake disk or brake drum having a brake element carrier body, in particular a brake element carrier body according to any one of claims 1 to 29, which has a region designed as a friction surface and a region designed as a contact surface.

31. A brake disc or brake drum according to claim 30, It is characterized in that The thickness of the alloy layer is 0.1 mm to 0.4 mm, preferably 0.2 mm to 0.3 mm.

32. A brake disc or brake drum according to claim 30 or 31, It is characterized in that The thickness of the diffusion zone is 0.05 mm to 0.6 mm, preferably 0.3 mm to 0.6 mm.

33. A brake disc or brake drum according to any one of claims 30 to 32, It is characterized in that The thickness of the diffusion zone of the friction surface is 0.3 mm to 0.6 mm.

34. A brake disc or brake drum according to any one of claims 30 to 33, It is characterized in that The friction surface and / or the contact surface is annular.

35. A brake disc or brake drum according to any one of claims 30 to 34, It is characterized in that The ventilation channels are located on and / or in the base body.

36. Brake disc or brake drum, comprising a metal matrix having a diffusion zone consisting of matrix materials iron and carbon and previously sprayed main layer materials aluminum, silicon, magnesium and manganese, the diffusion zone being produced by heat treatment and inward diffusion of the layer materials, the layer thickness of the diffusion zone being 0.05 mm to 0.6 mm, preferably 0.3 mm to 0.6 mm.

37. A brake disc or brake drum according to claim 36, It is characterized in that The diffusion zone contains the elements iron, carbon, aluminum, silicon, magnesium and manganese, wherein the elements iron, aluminum, silicon and manganese form new binary, ternary and quaternary intermetallic phases in the form of many self-sufficient and individually grown crystals, and the intermetallic phases are embedded in the same new parallel coexisting solid solution matrix composed of the above six elements.

38. A brake disc or brake drum according to claim 36 or 37, It is characterized in that The obtained diffusion layer is designed in such a way that in the newly formed solid solution matrix, the base elements iron and carbon increase continuously with increasing depth, while the sprayed layer elements aluminum, silicon, magnesium and manganese decrease continuously with increasing depth. In the crystals of the newly formed intermetallic phase, the concentrations of the above elements also change with increasing depth, qualitatively following the same trend, but not continuously, but in the form of discrete jumps according to the compositional recipe of the respective main intermetallic phase.

39. Brake pad backing plate or brake shoe comprising a brake element carrier plate, in particular a brake element carrier plate according to any one of claims 1 to 29.

40. A brake pad backing plate or brake shoe according to claim 39, It is characterized in that The thickness of the alloy layer is 0.1 mm to 0.3 mm, preferably 0.1 mm to 0.2 mm.

41. A brake pad backing plate or brake shoe according to claim 39 or 40, It is characterized in that The diffusion layer has a thickness of 0.05 mm to 0.3 mm, preferably 0.05 mm to 0.15 mm.

42. A brake pad backing plate or brake shoe according to any one of claims 39 to 41, It is characterized in that Brake pads are applied to the outer surface of the alloy.

43. A method for producing a brake element carrier body, in particular a brake element carrier body according to claims 1 to 29, comprising the following steps:

1. Provide a substrate, 2. Use hard ceramic material for sandblasting to remove the oxide layer on the surface of the substrate.

3. Applying an aluminum-based alloy to a carrier body, 4. Tempering the carrier body with the applied alloy.

44. The method according to claim 43, It is characterized in that The substrate is heated prior to blasting.

45. The method according to claim 43 or 44, It is characterized in that The hard ceramic material used in the sandblasting treatment is corundum and / or quartz and / or boron carbide and / or titanium carbide and / or silicon carbide and / or chromium carbide.

46. ​​The method according to any one of claims 43 to 45, It is characterized in that The sandblasting produces a roughness Rz of 5 μm to 10 μm on the surface of the substrate.

47. The method according to any one of claims 43 to 46, It is characterized in that The particle size of the hard ceramic material is 0.5 mm to 1.5 mm, in particular 0.8 mm to 1.2 mm.

48. The method according to any one of claims 43 to 47, It is characterized in that The sandblasting is performed at an angle to the surface of the brake element carrier body, said angle being 45°±10°.

49. The method according to any one of claims 43 to 48, It is characterized in that The alloy is an alloy based on aluminum and silicon.

50. The method according to any one of claims 43 to 49, It is characterized in that The alloy contains 5 to 50 mass % silicon.

51. The method according to any one of claims 43 to 50, It is characterized in that The alloy is an alloy based on aluminum and silicon with the main alloying elements, Wherein, the main alloying elements are selected from the second and / or third and / or fourth main group and / or the first and / or second and / or fourth and / or seventh subgroup of the periodic table, The secondary alloying elements are selected from the third and / or fourth main group and / or the fourth and / or fifth and / or sixth and / or eighth subgroup of the Periodic Table of the Elements.

52. The method according to claim 51, It is characterized in that The alloy contains secondary alloying elements which are selected from the third and / or fourth main group and / or the fourth and / or fifth and / or sixth and / or eighth subgroup of the periodic table.

53. The method according to any one of claims 43 to 52, It is characterized in that The alloy is composed of one or more main alloying elements, and the main alloying element is selected from one of the following elements (in mass %): Magnesium: 0.1 to 2, and / or boron: 0.1 to 10, and / or Silicon: 5 to 50, and / or Titanium: 0.1 to 5, and / or Manganese: 0.5 to 5, and / or Copper: 0.1 to 5, and / or Zinc: 0.1 to 5, The remainder consists of aluminum and unavoidable manufacturing-related impurities.

54. A brake element carrier body according to any one of claims 43 to 53, It is characterized in that The alloy contains one or more minor alloying elements, wherein the minor alloying elements are selected from one of the following elements (in mass %): Gallium: 0.1 to 1, and / or indium: 0.1 to 1, and / or germanium: 0.1 to 1, and / or tin: 0.1 to 1, and / or zirconium: 0.1 to 1, and / or vanadium: 0.1 to 1, and / or Chromium: 0.1 to 1, and / or iron: 0.1 to 1, and / or Cobalt: 0.1 to 1, and / or Nickel: 0.1 to 1.

55. The method according to any one of claims 43 to 54, It is characterized in that The alloy is one of the following ternary alloys: Al88 Si10 Mg2, Al88 Si10 B2, Al88 Si10 Ti2, Al88 Si10 Mn2, Al88 Si10 Cu2, Al88 Si10 Zn2, Al83 Si15 Mg2, Al83 Si15 B2, Al83 Si15 Ti2, Al83 Si15 Mn2, Al83 Si15 Cu2, Al83 Si15 Zn2, Al78 Si20 Mg2, Al78 Si20 B2, Al78 Si20 Ti2, Al78 Si20 Mn2, Al78 Si20 Cu2, Al78 Si20 Zn2.

56. The method according to any one of claims 43 to 55, It is characterized in that The alloy is one of the following quaternary alloys: Al86 Si10 Mn2 Mg2, Al86 Si10 Mn2 B2, Al86 Si10 Mn2 Ti2, Al86 Si10 Mn2 Cu2, Al86 Si10 Mn2 Zn2, Al81 Si15 Mn2 Mg2, Al81 Si15 Mn2 B2, Al81 Si15 Mn2 Ti2, Al81 Si15 Mn2 Cu2, Al81 Si15 Mn2 Zn2, Al76 Si20 Mn2 Mg2, Al76 Si20 Mn2 B2, Al76 Si20 Mn2 Ti2, Al76 Si20 Mn2 Cu2, Al76 Si20 Mn2 Zn2.

57. The method according to any one of claims 43 to 56, It is characterized in that The alloy consists of the following composition (in mass %): Al: 76.7 to 83.4, Si: 8.3 to 12.3, The remainder consists of Mg, B, Ti, Mn, Cu, Zn, Ga, Ge, Sn, Sb, Zr, V, Cr, Co, Ni and unavoidable production-related impurities.

58. The method according to any one of claims 43 to 57, It is characterized in that The alloy contains a dopant.

59. The method according to any one of claims 43 to 58, It is characterized in that The dopant is selected from the third main group and / or the first and / or third and / or fourth and / or fifth and / or sixth and / or seventh and / or eighth subgroup of the periodic table and / or lanthanides.

60. The method according to any one of claims 43 to 59, It is characterized in that The alloy contains one or two or three or more dopants, and the dopant consists of one of the following elements (in mass %): Antimony: 0.1 to 1, and / or Bismuth: 0.01 to 0.1, and / or Scandium: 0.01 to 0.1, and / or Yttrium: 0.01 to 0.1, and / or Lanthanum: 0.01 to 0.1, and / or Ce: 0.01 to 0.1, and / or Hafnium: 0.01 to 0.1, and / or Niobium: 0.01 to 0.1, and / or Tantalum: 0.01 to 0.1, and / or Molybdenum: 0.01 to 0.1, and / or Tungsten: 0.01 to 0.1, and / or Rhenium: 0.01 to 0.1, and / or Ruthenium: 0.01 to 0.1, and / or Osmium: 0.01 to 0.1, and / or Rhodium: 0.01 to 0.1, and / or Iridium: 0.01 to 0.1, and / or Palladium: 0.01 to 0.1, and / or Platinum: 0.01 to 0.1, and / or Silver: 0.01 to 0.1, and / or Gold: 0.01 to 0.

1.

61. The method according to any one of claims 43 to 60, It is characterized in that Dopants of the alloy act as selectively active catalysts and / or inhibitors.

62. The method according to claims 43 to 61, It is characterized in that The thickness of the alloy layer is 0.1 mm to 0.4 mm, preferably 0.2 mm to 0.3 mm.

63. The method according to any one of claims 43 to 62, It is characterized in that The alloying is performed by a high velocity flame spraying process, an arc wire spraying process or a powder coating process.

64. The method according to any one of claims 43 to 63, It is characterized in that The tempering is performed at a temperature between 590°C and 750°C.

65. The method according to any one of claims 43 to 64, It is characterized in that The tempering is carried out along a temperature profile between 600° C. and 750° C., which is linear, exponential or cyclical, or has a heating phase, a holding phase and a cooling phase.

66. The method according to any one of claims 43 to 65, It is characterized in that The temperature profile is adapted to the concentration gradient of the alloy diffusing into the base metal.

67. The method according to any one of claims 43 to 66, It is characterized in that Tempering is carried out for 180 to 360 minutes, preferably 210 to 300 minutes.

68. The method according to any one of claims 43 to 67, It is characterized in that The carrier body is cast and / or stamped.

69. A method for manufacturing a brake disc or brake drum, in particular a brake disc or brake drum according to claims 30 to 38, comprising the following steps: a. providing a brake element carrier body according to claims 1 to 29 or a brake element carrier body manufactured by the method of claims 43 to 65, and b. Removal of alloy until the diffusion zone is reached, creating a friction surface and / or contact surface.

70. The method according to claim 69, It is characterized in that The alloy is removed mechanically.

71. The method according to claim 69 or 70, It is characterized in that The alloy is ground or turned.

72. The method according to any one of claims 69 to 71, It is characterized in that The alloy is removed by at most 0.05 mm or at most 1 mm or at most 1.5 mm.

73. A method of manufacturing a brake pad backing plate or brake shoe, in particular a brake pad backing plate or brake shoe as claimed in claims 30 to 42, wherein The following steps are involved: a. providing a brake element carrier body according to claims 1 to 29 or a brake element manufactured by the method of claims 43 to 65, and b. Applying brake pads to the alloy surface creates a friction surface or contact surface.

74. The method according to claim 73, It is characterized in that The brake pads are glued and / or welded on.

75. The method according to claim 73 or 74, It is characterized in that Brake pads contain one or more of the following materials: - metal and / or sintered metal powder, in particular steel, iron, copper or brass, and / or - Graphite and / or - Glass and / or - rubber and / or -Carbon and / or - aramid and / or - synthetic resins and / or - natural resins and / or - Ceramic fibers and / or - Adhesive.

76. A brake disc or brake drum manufactured by the method of any one of claims 69 to 72.

77. A brake pad backing plate or brake shoe manufactured according to any one of claims 73 to 75.

78. Braking system, which is composed of: - a brake disc or brake drum according to any one of claims 30 to 38, or a brake disc or brake drum manufactured by a method according to any one of claims 69 to 72, and - a brake pad backing plate or brake shoe as claimed in claims 39 to 42, or a brake pad backing plate or brake shoe manufactured by the method of any one of claims 73 to 75, - wherein the brake disc or brake drum and the brake pad back plate or brake shoe are manufactured on a brake element carrier body according to claims 1 to 29 or a brake element carrier body according to any one of claims 43 to 65.

79. A motor vehicle or aircraft having a braking system as claimed in claim 78.

80. A railcar having the braking system of claim 78.

81. A stationary industrial brake system having the brake system of claim 78.

82. A wind turbine having the braking system of claim 78.