Separator, secondary battery, electrochemical device, and power device
By using organic coatings of low melting point first polymer and low swelling second polymer in the battery isolation film, the problem of degradation in the cell hot box window and safety performance improvement is solved, and the battery is realized at high temperature Improved stability and performance.
Patent Information
- Application Number
- CN202380036692.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-08-11
AI Technical Summary
When the prior art improves the hot box window and safety performance of the battery cell, it is easy to cause the battery to degrade the cycle performance and high-temperature storage performance, and the polyvinylidene fluoride coating with low bonding performance may cause the battery to deform.
Using a barrier film, including a base film and an organic coating, the coating contains a first polymer with a low melting point and a second polymer with a low swelling degree, ensuring that during battery charging and discharge by adjusting its proportion and particle size. Maintain adhesion and reduce heat accumulation at high temperatures to avoid clogging of base membrane pores.
It effectively improves the safety performance and circulation performance of the battery cell, ensuring the stability and performance of the battery at high temperatures.
Smart Images

Figure CN119072820A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a separator, a secondary battery and an electrochemical device containing the separator, and an electrical device containing the secondary battery or the electrochemical device. Background Art
[0002] The rapid increase in battery cell charge rate and the increase in battery cell energy density are not conducive to the improvement of the hot box window of the battery cell (the safe temperature at which the battery cell can be placed in a hot box for testing after charging without catching fire, exploding or smoking). In order to improve the hot box window of the battery cell and improve the safety performance of the battery cell, two methods are usually used: adjusting the solvent system of the electrolyte; or using a polyvinylidene fluoride coating with low adhesion properties to coat the isolation membrane. However, the adjustment of the electrolyte system will deteriorate the cycle performance of the battery cell, and there is a risk of deterioration in the low-temperature performance of the battery cell; and the use of a polyvinylidene fluoride coating with too low adhesion can easily cause deformation of the battery cell and deteriorate the high-temperature storage performance of the battery cell. Summary of the invention
[0003] In view of this, the first aspect of the present application provides an isolation film, comprising:
[0004] Basement membrane;
[0005] An organic coating layer disposed on a surface of the base film, the organic coating layer comprising a first polymer and a second polymer;
[0006] The melting point T of the first polymer satisfies 60°C≤T≤100°C;
[0007] The swelling degree D of the second polymer when placed in an electrolyte at 60° C. for 24 hours is ≤30%, and the mass ratio of lithium hexafluorophosphate, ethylene carbonate, diethyl carbonate, propylene carbonate and propyl propionate in the electrolyte is 8.7:20:30:20:30.
[0008] In the isolation membrane provided in the first aspect, the first polymer can maintain the adhesion requirements during the battery charge and discharge cycle, and can also improve the high-temperature storage performance; when the battery generates heat during charge and discharge, the low-melting-point first polymer is more likely to soften, and the adhesion is significantly reduced, so that the interface between the isolation membrane and the battery electrode (positive electrode) is opened, which helps to reduce heat accumulation and improve the safety performance of the battery cell hot box; the second polymer has a low swelling degree D and can maintain its original morphology in the battery cell, will not block the pores of the base film, and can effectively improve the problem of melting and film formation of the low-melting-point first polymer during the hot pressing process of the battery cell, thereby improving the cycle performance of the battery cell.
[0009] In combination with the first aspect, in some embodiments, in the organic coating, the weight percentage of the first polymer is greater than or equal to 40% and less than or equal to 95%, and the weight percentage of the second polymer is less than or equal to 50%.
[0010] It can be seen that the present application improves the hot box test window of the battery cell while ensuring the performance of the battery cell by reasonably formulating the ratio of the first polymer to the second polymer. The higher the content of the first polymer, the better the high-temperature failure effect, but if the content is too high, the isolation membrane is prone to blockage, resulting in a decrease in the dynamics of the battery cell and poor cycle performance; the higher the content of the second polymer, the better the cycle performance of the battery cell, but if the content is too high, the adhesion of the isolation membrane at room temperature is too low, which is easy to cause poor high-temperature storage performance, and the battery cell is at risk of deformation, which will lead to a decrease in cycle performance.
[0011] In combination with the first aspect, in some embodiments, in the organic coating, the weight percentage of the first polymer is greater than or equal to 60% and less than or equal to 95%, and the weight percentage of the second polymer is less than or equal to 30%.
[0012] In combination with the first aspect, in some embodiments, when the isolation membrane is applied to an electrochemical battery cell, the swelling degree D of the second polymer and the content H of the linear carboxylic acid ester in the electrolyte satisfy D=K*H+0.1, where 0.01≤K≤0.08.
[0013] In combination with the first aspect, in some embodiments, 10%≤H≤50%.
[0014] It can be seen that by adjusting the ratio of the first polymer to the second polymer and the linear carboxylate content of the electrolyte, the hot box test pass rate can be improved while ensuring the performance of the battery cell.
[0015] In combination with the first aspect, in some embodiments, the median particle size Dv50 of the first polymer satisfies 1.0 μm≤Dv50≤2 μm.
[0016] It can be seen that when the particle size of the first polymer is too large, the adhesion of the organic coating will deteriorate and the thickness will increase, resulting in a lower volume energy density of the battery cell; when the particle size of the first polymer is too small, the isolation membrane will be blocked, resulting in poor cycle performance of the battery. In the present application, by setting a suitable particle size range for the first polymer, the adhesion and appropriate thickness of the organic coating can be ensured.
[0017] In combination with the first aspect, in some embodiments, the melting point T of the first polymer satisfies 60°C≤T≤85°C.
[0018] In combination with the first aspect, in some embodiments, the second polymer is spherical or quasi-spherical, and the sphericity R of the second polymer satisfies 0.7≤R<1.
[0019] In combination with the first aspect, in some embodiments, the second polymer is spherical or quasi-spherical, and the sphericity R of the second polymer satisfies 0.8≤R<1.
[0020] It can be seen that the second polymer has a high sphericity, which can achieve better results with a smaller amount of the second polymer. The spherical or quasi-spherical second polymer has a lower packing density in the organic coating, which can increase the porosity of the organic coating and improve the cycle performance of the battery cell.
[0021] In combination with the first aspect, in some embodiments, the swelling degree D of the second polymer when placed in an electrolyte at 85° C. for 24 hours satisfies 10%≤D≤50%.
[0022] It can be seen that, by selecting a second polymer with a low swelling degree, when the isolation membrane is applied to the battery cell, even if the temperature rises, the second polymer can better maintain the original morphology, and the second polymer has a higher melting point than the first polymer, for example, the melting point is higher than 130°C, and can maintain the original morphology in the battery cell, and will not block the pores of the base film, and can effectively improve the problem of melting and film formation of the low-melting-point first polymer during the hot pressing process of the battery cell, and improve the cycle performance of the battery cell. The selection of substances with different swelling degrees is achieved by selecting different types of substances, molecular weights or different crosslinking degrees.
[0023] In combination with the first aspect, in some embodiments, the first polymer includes a graft copolymer, the monomer of the polymer body in the graft copolymer includes at least one of ethylene, propylene, vinylidene fluoride, acrylic acid, acrylate, styrene, acrylonitrile, maleic anhydride, vinyl chloride and allyl chloride, and the monomer used for grafting includes at least one of maleic anhydride, acrylate and acrylic acid; the weight percentage of the graft copolymer in the first polymer is greater than or equal to 3% and less than or equal to 10%.
[0024] In combination with the first aspect, in some embodiments, the second polymer includes a polymer of at least one monomer selected from the group consisting of vinylidene fluoride, hexafluoropropylene, propylene, vinyl chloride, styrene, butadiene, acrylate, and acrylic acid, and the second polymer is at least one of a homopolymer, a copolymer, and a blended polymer.
[0025] In a second aspect, the present application provides a secondary battery, which includes a positive electrode sheet, a negative electrode sheet, and the above-mentioned isolation film arranged between the positive electrode sheet and the negative electrode sheet, wherein the organic coating is located between the positive electrode sheet and the base film.
[0026] In a third aspect, the present application provides an electrochemical device, which includes a positive electrode sheet, a negative electrode sheet, and the above-mentioned isolation membrane arranged between the positive electrode sheet and the negative electrode sheet, wherein the organic coating is located between the positive electrode sheet and the base film.
[0027] In a fourth aspect, the present application provides an electrical device, the secondary battery or the electrochemical device mentioned above. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic structural diagram of an isolation membrane according to one embodiment of the present application.
[0029] Figure 2 Schematic diagram of the working mechanism of the isolation membrane according to one embodiment of the present application.
[0030] Description of main component symbols:
[0031] Isolation film 10
[0032] Basement membrane 11
[0033] Organic coating 13
[0034] Inorganic coating 15
[0035] Other organic coatings17
[0036] Positive electrode 20
[0037] Negative electrode 30 DETAILED DESCRIPTION
[0038] The embodiments of the present application are described below in conjunction with the drawings in the embodiments of the present application.
[0039] The separator is a very critical part of the battery. It is a layer of separator material set between the positive and negative electrodes of the battery, which has a direct impact on the safety performance and cost of the battery. The main function of the separator is to isolate the positive and negative electrodes and prevent the electrons in the battery from passing freely, while allowing the ions in the electrolyte to pass freely.
[0040] The present application provides a secondary battery separator that can effectively improve the thermal window of the battery cell and enhance the safety performance of the battery cell. Figure 1 The isolation film 10 includes a base film 11 and an organic coating 13 disposed on a surface of the base film 11. Figure 2 When in use, the side of the separator 10 having the organic coating 13 faces the positive electrode sheet 20. The organic coating 13 contains a first polymer and a second polymer.
[0041] The present application has no particular restrictions on the type of base film 11, as long as the purpose of the present application can be achieved. The base film 11 may be a resin, glass fiber, inorganic material, etc. formed by a material that is stable to the electrolyte. In some embodiments, the base film 11 includes a porous sheet or a non-woven fabric-like material with excellent liquid retention. Examples of materials for the resin or glass fiber separator base film may include, but are not limited to, polyolefins, aromatic polyamides, polytetrafluoroethylene, polyether sulfone, etc. Taking polyolefins as an example, the material of the base film 11 may be selected from one or more of polypropylene and polyethylene.
[0042] The present application does not limit the thickness of the base film 11 as long as the purpose of the present application can be achieved. For example, the thickness of the base film 11 can be 5 to 50 μm, preferably 5 to 30 μm.
[0043] In the present application, the melting point T of the first polymer is relatively low, 60° C. ≤ T ≤ 100° C. Further, in some embodiments, the melting point T of the first polymer satisfies 60° C. ≤ T ≤ 85° C.
[0044] The first polymer provides the viscosity of the organic coating 13. At a temperature below the melting point (e.g., room temperature), the first polymer has high bonding properties, can maintain the bonding force requirements during the battery charge and discharge cycle, and can also improve the high-temperature storage performance of the battery. The present application selects a first polymer with a low melting point so that when the battery is charged and discharged and generates heat, for example, when the temperature rises to the melting point T or above, the first polymer with a low melting point is more likely to soften and produce fluidity, and the bonding force is significantly reduced, so that the interface between the isolation membrane and the positive electrode plate is opened, which helps to reduce heat accumulation and improve the safety performance of the battery cell hot box.
[0045] When the particle size of the first polymer is too large, the adhesion of the organic coating 13 will deteriorate and the thickness will increase, resulting in a lower volume energy density of the battery cell; if the particle size of the first polymer is too small, the isolation membrane will be blocked, resulting in poor cycle performance of the battery. In the present application, the median particle size Dv50 of the first polymer satisfies 0.8μm<Dv50<2μm. In some embodiments, the median particle size Dv50 of the first polymer satisfies 1.0μm≤Dv50≤2μm. By setting the first polymer within a suitable particle size range, the adhesion of the organic coating 13 can be ensured and it has a suitable thickness.
[0046] When the separator 10 is used in a battery, the electrolyte will penetrate into the porous separator 10, and the organic coating is also equivalent to being immersed in the electrolyte. The swelling degree D of the second polymer in the electrolyte at 60° C. for 24 hours is ≤30%, and the mass ratio of lithium hexafluorophosphate, ethylene carbonate, diethyl carbonate, propylene carbonate, and propyl propionate in the electrolyte is 8.7:20:30:20:30.
[0047] Furthermore, in some embodiments, the swelling degree of the second polymer when placed in an electrolyte at 85°C for 24 hours is 10%≤D≤50%. In the present application, the definition of swelling degree is: when the polymer molecules adsorb solvent molecules to reach swelling equilibrium, the ratio of the volume after swelling to the volume before swelling minus 1. Generally, the swelling degree of a polymer is related to the polymer material composition, molecular weight, length of the molecular chain, and the degree of cross-linking of the molecular chain. The present application can ensure the swelling degree of the second polymer by selecting appropriate material composition, large molecular weight, long molecular chain or a large degree of cross-linking of the molecular chain.
[0048] The present application selects a second polymer with high strength and low swelling degree, so that when the isolation film 10 is applied to the battery cell, the second polymer can also maintain its original morphology. In addition, the second polymer has a higher melting point than the first polymer, for example, a melting point higher than 130°C, and can maintain its original morphology in the battery cell without blocking the pores of the base film 11. It can effectively improve the problem of melting and forming a film of the first polymer with a low melting point during the hot pressing process of the battery cell, and improve the cycle performance of the battery cell.
[0049] The second polymer is spherical or quasi-spherical in the isolation membrane 10, and the sphericity R of the second polymer satisfies 0.7≤R≤1.0. Further, in some embodiments, the sphericity R of the second polymer satisfies 0.8≤R≤1.0. The high sphericity of the second polymer can make the amount of the second polymer in the organic coating 13 less and achieve better results, and the spherical or quasi-spherical second polymer has a low stacking density in the organic coating 13, which can increase the porosity of the organic coating and improve the cycle performance of the battery cell.
[0050] As the battery temperature rises, the first polymer is more likely to soften and lose its adhesiveness, while the second polymer, due to its relatively high melting point, does not soften and remains in its rigid granular form.
[0051] The higher the content of the first polymer is, the better the high-temperature failure effect is. However, if the content is too high, the isolation film 10 is prone to pore blockage, resulting in a decrease in the dynamics of the battery cell and a deterioration in the cycle performance.
[0052] The higher the content of the second polymer, the better the cycle performance of the battery cell, but if the content is too high, the adhesion of the isolation film at room temperature will be worse, which will easily lead to poor high-temperature storage performance and the risk of deformation during circulation.
[0053] Therefore, it is necessary to reasonably formulate the ratio of the first polymer and the second polymer in order to improve the hot box test window of the battery cell while ensuring the performance of the battery cell. In the present application, in the organic coating 13, the weight percentage of the first polymer is greater than or equal to 40% and less than or equal to 95%, and the weight percentage of the second polymer is less than or equal to 50%. Furthermore, in some embodiments, in the organic coating 13, the weight percentage of the first polymer is greater than or equal to 60% and less than or equal to 95%, and the weight percentage of the second polymer is less than or equal to 30%.
[0054] In the present application, in the organic coating 13, the weight percentage of the second polymer is greater than or equal to 10%.
[0055] In addition, the higher the content of linear carboxylic acid ester in the electrolyte, the better the performance of the battery cell, but if the content is too high, the polymer will swell too much, blocking the pores of the isolation membrane, resulting in poor performance of the battery cell. When the isolation membrane is applied to the battery cell, the weight percentage of linear carboxylic acid ester in the electrolyte is H, where 10%≤H≤50%.
[0056] In the present application, the swelling degree D of the second polymer and the content H of the linear carboxylic acid ester in the electrolyte satisfy D=K*H+0.1, wherein 0.01≤K≤0.08.
[0057] In this way, by adjusting the ratio of the first polymer to the second polymer and the linear carboxylate content of the electrolyte, the upper limit window of the hot box test can be improved while ensuring the performance of the battery cell.
[0058] The first polymer has a Dv10 that satisfies 0.1 μm≤Dv10≤0.7 μm, and a Dv90 that satisfies 2 μm≤Dv90≤5 μm.
[0059] The Dv10 of the second polymer satisfies 0.1 μm≤Dv10≤0.5 μm, the Dv50 satisfies 0.5 μm≤Dv50≤2 μm, and the Dv90 satisfies 2 μm≤Dv90≤5 μm. The ratio S of the Dv90 of the second polymer to the Dv90 of the first polymer satisfies 0.6≤S≤1.0.
[0060] In some embodiments, the first polymer includes a polymer of at least one monomer selected from the group consisting of ethylene, propylene, vinylidene fluoride, acrylic acid, acrylic ester, styrene, acrylonitrile, maleic anhydride, vinyl chloride and allyl chloride. The first polymer is at least one selected from the group consisting of a homopolymer, a copolymer and a blended polymer.
[0061] In some embodiments, the first polymer includes a grafted copolymer, the monomer of the polymer body in the grafted copolymer includes at least one of ethylene, propylene, vinylidene fluoride, acrylic acid, acrylate, styrene, acrylonitrile, maleic anhydride, vinyl chloride and allyl chloride, and the monomer used for grafting includes at least one of maleic anhydride, acrylate and acrylic acid.
[0062] In some embodiments, when the first polymer contains a graft copolymer, the weight percentage of the graft copolymer in the first polymer is greater than or equal to 3% and less than or equal to 10%.
[0063] In some embodiments, the second polymer includes a polymer of at least one monomer selected from vinylidene fluoride, hexafluoropropylene, propylene, vinyl chloride, styrene, butadiene, acrylate, and acrylic acid, and the second polymer is at least one of a homopolymer, a copolymer, and a blended polymer.
[0064] In some embodiments, the average molecular weight of the first polymer is greater than or equal to 300,000 and less than or equal to 1,000,000. The average molecular weight of the second polymer is greater than or equal to 800,000 and less than or equal to 2,000,000.
[0065] It is understood that, optionally, the organic coating contains, in addition to the first polymer and the second polymer, an auxiliary component, and the weight percentage of the auxiliary component in the organic coating does not exceed 10%. The auxiliary component may include conventional thickeners and wetting agents, etc. The thickener may be sodium carboxymethyl cellulose or lithium carboxymethyl cellulose, and the weight percentage in the organic coating may be 0.5% to 1.5%. The wetting agent includes sulfonate and dimethyl silane, and the weight percentage in the organic coating may be 1% to 10%.
[0066] In some embodiments, the coating weight of the organic coating on the base film is greater than or equal to 0.5 mg / 5000 mm 2 And less than or equal to 3mg / 5000mm 2 The coating thickness of the organic coating is greater than or equal to 0.5 μm and less than or equal to 5 μm. Furthermore, in some embodiments, the coating weight of the organic coating on the base film is greater than or equal to 0.5 mg / 5000 mm 2 And less than or equal to 1.5mg / 5000mm 2 .
[0067] Optionally, in some embodiments, such as Figure 1As shown, the isolation film 10 further includes an inorganic coating 15 disposed between the base film 11 and the organic coating 13. The inorganic coating 15 is used to improve the heat resistance and mechanical strength of the isolation film 10. The inorganic coating 15 includes ceramics, and the ceramics include at least one of aluminum oxide, boehmite, titanium dioxide, silicon dioxide, zirconium dioxide, tin dioxide, magnesium hydroxide, magnesium oxide, zinc oxide, barium sulfate, boron nitride or aluminum nitride.
[0068] Understandable, such as Figure 1 and Figure 2 As shown, the isolation film 10 also includes another organic coating 17 disposed on the other surface of the base film 11. The other organic coating 17 and the above-mentioned organic coating 13 are respectively disposed on the opposite surface of the base film 11, that is, the other organic coating 17 is disposed on the surface of the base film 11 facing the negative electrode plate 30. The present application has no particular restrictions on the type of the other organic coating 17, as long as it can play the role of bonding the isolation film and the negative electrode. In some embodiments, the other organic coating 17 mainly contains a binder and a thickener.
[0069] See also Figure 2 The present application also provides an electrochemical device, comprising a positive electrode sheet 20, a negative electrode sheet 30, an electrolyte, and the above-mentioned separator 10 disposed between the positive electrode sheet 20 and the negative electrode sheet 30. The organic coating 13 is disposed on the surface of the base film 11 facing the positive electrode sheet 20, that is, between the positive electrode sheet 20 and the base film 11, and can be used to bond the positive electrode sheet 20 and the separator 10. The electrochemical device can be a secondary battery. The electrolyte penetrates into the separator 10. Figure 2 As an illustration, the separator 10 is not in a state of bonding the positive electrode sheet 20 and the negative electrode sheet 30. The positive electrode sheet, the negative electrode sheet, and the electrolyte of the electrochemical device can all be of types known in the art.
[0070] [Positive electrode]
[0071] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector. As an example, the positive electrode current collector has two opposite surfaces along its own thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector. The positive electrode film layer includes a positive electrode active material.
[0072] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0073] In some embodiments, the positive electrode active material may adopt a positive electrode active material for a battery that is well known in the art. As an example, the positive electrode active material may include one or more of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, one or more of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0074] In some embodiments, the positive electrode film layer may also optionally include a binder. As an example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0075] In some embodiments, the positive electrode film layer may further include a conductive agent, which may include, for example, one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0076] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0077] [Negative electrode]
[0078] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0079] As an example, the negative electrode current collector has two opposite surfaces in its own thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0080] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0081] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include one or more of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from one or more of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0082] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0083] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0084] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0085] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0086] [Electrolyte]
[0087] The electrolyte plays a role in conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs, including electrolyte salts and solvents.
[0088] In some embodiments, the electrolyte salt can be selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethanesulfonyl imide), lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0089] In some embodiments, the solvent can be selected from one or more of ethylene carbonate, ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, propylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0090] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0091] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0092] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0093] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0094] The present application also provides a secondary battery, which includes a positive electrode sheet, a negative electrode sheet, and a separator disposed between the positive electrode sheet and the negative electrode sheet. Furthermore, the present application also provides an electrochemical device, which includes a positive electrode sheet, a negative electrode sheet, and a separator disposed between the positive electrode sheet and the negative electrode sheet.
[0095] The present application also provides an electric device using the above electrochemical device (secondary battery) as a power source, and the electric device may be, but is not limited to, a mobile phone, a tablet, a laptop, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, etc. Among them, the electric toy may include a fixed or mobile electric toy, for example, a game console, an electric car toy, an electric ship toy, an electric airplane toy, etc., and the spacecraft may include an airplane, a rocket, a space shuttle, a spacecraft, etc.
[0096] The technical solution of the embodiment of the present application is further explained below through specific examples.
[0097] Inorganic coating preparation
[0098] Inorganic boehmite particles with a Dv50 of 1 μm and polyacrylate are mixed in a mass ratio of 90:10 and dissolved in deionized water to form an inorganic coating slurry with a solid content of 50%. The resulting inorganic coating slurry is then evenly coated on one side of a PE base film using a micro-concave coating method to obtain a heat-resistant layer, which is then dried in an oven.
[0099] First Group of Examples: Preparation of Organic Coatings
[0100] First Group of Examples An organic coating was prepared according to the parameters of the first polymer and the second polymer in each example in Table 1 below and auxiliary components (the thickener is sodium carboxymethyl cellulose, and the wetting agent is sulfonate and dimethyl silane), wherein the first polymer, the second polymer, and the auxiliary components totaled 100 parts by weight, and then deionized water was added for stirring, and the viscosity of the slurry was adjusted to 50 mPa·s and the solid content was 5%, to obtain slurry A. The above slurry A was evenly coated on the surface of the inorganic coating of the PE base film to obtain a first coating, and the coating weight of the first coating was 0.2 g / m 2 , and complete drying in an oven.
[0101] Comparative Example Diaphragm Coating Preparation
[0102] According to the parameters of each comparative example in Table 1 below and adding auxiliary components (the thickener is sodium carboxymethyl cellulose, and the wetting agent is sulfonate and dimethyl silane), the comparative organic coating is prepared. 1-4 only adds the first polymer and the auxiliary component, and the first polymer and the auxiliary component are 100 parts by weight in total; Comparative Examples 1-1 to Comparative Examples 1-3 add the first polymer, the second polymer and the auxiliary component, and the first polymer, the second polymer, and the auxiliary component are 100 parts by weight in total. The swelling degree of the second polymer added in Comparative Examples 1-3 is greater than 30%; then deionized water is added for stirring, and the viscosity of the slurry is adjusted to 50mPa·s and the solid content is 5% to obtain comparative slurry A. The comparative slurry A is evenly coated on the surface of the inorganic coating of the PE base film to obtain the first coating of the comparative example. The coating weight of the first coating of the comparative example is 0.2g / m 2 , and complete drying in an oven.
[0103] High adhesion coating preparation
[0104] 90g of high molecular polymer binder was added to a stirrer, and then 0.5g of sodium carboxymethyl cellulose was added, and the mixture was stirred and mixed evenly; 8.5g of dimethylsiloxane as a wetting agent was added, and then deionized water was added and stirred, and the viscosity of the slurry was adjusted to 40mPa·s and the solid content was 5%, thereby obtaining slurry B. The slurry B was evenly coated on the other surface of the PE base film to obtain a second coating layer, and the coating weight of the second coating layer was 0.5g / m 2 , and complete drying in an oven.
[0105] Preparation of positive electrode
[0106] The positive electrode active materials lithium cobalt oxide, acetylene black, and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then N-methylpyrrolidone (NMP) is added as a solvent to prepare a slurry with a solid content of 75%, and stirred evenly. The slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, dried at 90°C, and cold pressed to obtain a positive electrode sheet with a positive electrode active material layer thickness of 100μm, and then the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet coated with a positive electrode active material layer on both sides. The positive electrode sheet is cut into a specification of 74mm×867mm and welded to the pole ear for standby use.
[0107] Preparation of negative electrode
[0108] The negative electrode active material artificial graphite, acetylene black, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in a mass ratio of 96:1:1.5:1.5, and then deionized water is added as a solvent to prepare a slurry with a solid content of 70% (mass content), and stirred evenly. The slurry is evenly coated on one surface of a copper foil with a thickness of 8 μm, dried at 110°C, and cold pressed to obtain a negative electrode sheet with a single-sided negative electrode active material layer coated with a negative electrode active material layer with a thickness of 150 μm, and then the above coating steps are repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet with a double-sided negative electrode active material layer coated. The negative electrode sheet is cut into a specification of 74 mm × 867 mm and welded to the pole ear for standby use.
[0109] Preparation of electrolyte
[0110] In an environment with a water content of less than 10 ppm, non-aqueous organic solvents of ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), and propyl propionate (PP) are mixed in a mass ratio of 2:3:2:3, and then lithium hexafluorophosphate (LiPF6) is added to the non-aqueous organic solvent to dissolve and mix evenly to obtain an electrolyte, wherein the ratio of LiPF6 to EC, DEC, PC, and PP is 8.7:20:30:20:30.
[0111] Preparation of lithium-ion batteries
[0112] The positive electrode sheet, separator, and negative electrode sheet prepared above are stacked in order, the side of the separator with the first coating is in contact with the positive electrode sheet, and the side of the separator with the second coating is in contact with the negative electrode sheet, and they are wound to obtain an electrode assembly. The electrode assembly is packed into an aluminum-plastic film packaging bag, and the moisture is removed at 80°C, and the prepared electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, forming, shaping, and other processes.
[0113] Adhesion test between separator and electrode
[0114] The national standard GB / T 2790-1995, that is, the 180° peel test standard is adopted to test the adhesion between the separator and the positive electrode sheet or the negative electrode sheet. The separator and the positive electrode sheet are cut into 54.2mm×72.5mm samples, the separator and the positive electrode sheet are compounded, and hot pressing is performed using a hot press. The hot pressing conditions are: temperature 85°C, pressure 1Mpa, hot pressing time 85s (seconds), the compounded samples are cut into 15mm×54.2mm strips, and the adhesion between the separator and the positive electrode sheet at room temperature (25°C) is tested according to the 180° peel test standard.
[0115] Hot Box Window Test
[0116] 1. Pre-treatment of battery cell full charging process
[0117] 1) The test temperature is 25°C;
[0118] 2) Sleep for 30 minutes;
[0119] 3) 0.2C constant current charging to 4.5V, 4.5V constant voltage charging to a cut-off current of 0.025C.
[0120] 2. Testing process:
[0121] ① Check the appearance and take photos before and after the test;
[0122] ②Thermosensitive line attachment position;
[0123] ③ Place the sample vertically in the box and heat it to 130℃ at a rate of 6℃ and keep it for 60min;
[0124] ④ Measurement frequency: The voltage internal resistance measurement uses the 1KHz specification, and is measured after pretreatment and testing;
[0125] ⑤Judgment criteria: no fire, no explosion, no smoke.
[0126] Cyclic performance test Preparation process before cycling: stand for 30 minutes at a test temperature of 25°C, then discharge to 3V at a current density of 0.2C;
[0127] Let it stand for another 30 minutes, charge to 4.48V at 0.5C constant current, charge to 0.02C at constant voltage; let it stand for 30 minutes; discharge to 3V at 0.2C current density, and finally let it stand for 30 minutes.
[0128] Cycle flow test process: let stand for 30 minutes under the test temperature of 25℃, then charge at a constant current of 12.4A to 4.22V, and charge at a constant voltage to 1.8C; then charge at a constant current of 1.8C to 4.3V, and charge at a constant voltage to 1.5C; charge at a constant current of 1.5C to 4.48V, and charge at a constant voltage to 1.2C; charge at a constant current of 1.2C to 4.53V, and charge at a constant voltage to 0.26C; let stand for 5 minutes, discharge to 3.2V at a current density of 0.7C; let stand for 5 minutes, and cycle 800 times from step 3 to step 9.
[0129] The high temperature cycle test was performed as above, except that the temperature condition was set to 45°C.
[0130] Swelling test method Preparation of film: disassemble the battery cell, take out the diaphragm, and dissolve it in the organic solvent NMP with a solvent-solution ratio of 1:9. Place the beaker containing the above suspension on a disperser and stir it for 1.5 hours. Let the stirred solution stand for 30 minutes to eliminate bubbles. Use a filter to filter to remove insoluble impurities and base film. Pour this solution into the film preparation mold, and remove any bubbles in advance. Put the mold in an oven, set the temperature to 60°C, and the time to 12 hours.
[0131] Cut the prepared film into strips of about 2g with scissors, and make 2-3 parallel samples for each film; weigh the strips separately, record the initial weight M1, put them in a vial, label the sample name, add electrolyte to 2-3cm above the film, seal the vial, put it in an oven, set the temperature to 60℃ and test the swelling time for 24h. During the test, take out the film, wipe it clean with dust-free paper, and record the film weight M2 at each time.
[0132] Swelling degree = (M2-M1) / M1
[0133] Table 1
[0134]
[0135]
[0136] According to the test results in Table 1, the hot box test pass rates of the batteries of Examples 1-1 to 1-21 can reach 80% or more and are significantly higher than the hot box test pass rates of the batteries of Comparative Examples 1-2 to 1-4. The capacity retention rates of the batteries of Examples 1-1 to 1-21 in the normal temperature cycle test at 25°C 4C for 800 cycles can reach 80% or more. It can be seen that by adopting the organic coating containing the first polymer with a low melting point and the second polymer with a low swelling degree in the present application, the hot box test pass rate of the battery can be effectively improved on the basis of ensuring the normal temperature cycle performance of the battery.
[0137] Second Group of Examples: Preparation of Organic Coatings
[0138] The second group of examples is to prepare an organic coating according to the parameters of the first polymer and the second polymer in Table 2 below and add auxiliary components (the thickener is sodium carboxymethyl cellulose, and the wetting agent is sulfonate and dimethyl silane) in a proportion, wherein the first polymer is 65 parts by weight, the second polymer is 30 parts by weight, and the auxiliary components are 5 parts by weight, and then deionized water is added for stirring, and the viscosity of the slurry is adjusted to 50mPa·s and the solid content is 5%, to obtain slurry A. The above slurry A is evenly coated on the surface of the inorganic coating of the PE base film to obtain a first coating, and the coating weight of the first coating is 0.2g / m 2 , and dried in an oven. The proportion of cyclic carboxylic acid ester (such as EC) in the electrolyte is increased accordingly to meet the regulation of the linear carboxylic acid ester content described below.
[0139] For other steps and parameters of the second group of embodiments, please refer to the steps and parameters of the first group of embodiments, and finally a lithium-ion battery is obtained.
[0140] Table 2
[0141]
[0142] According to the test results in Table 2, the swelling degree D of the second polymer and the content H of the linear carboxylate in the electrolyte satisfy the formula D=K*H+0.1, where 0.01≤K≤0.08; by controlling the reasonable content of the linear carboxylate in the electrolyte and matching the swelling degree of the second polymer, the high temperature cycle performance of the battery can be improved.
[0143] The third group of examples of organic coating preparation
[0144] The third group of examples is to prepare an organic coating according to the parameters of the first polymer and the second polymer in Table 3 below and add auxiliary components (the thickener is sodium carboxymethyl cellulose, and the wetting agent is sulfonate and dimethyl silane) in a proportion, wherein the first polymer is 65 parts by weight, the second polymer is 30 parts by weight, and the auxiliary components are 5 parts by weight, and then deionized water is added for stirring, and the viscosity of the slurry is adjusted to 50mPa·s and the solid content is 5%, to obtain slurry A. The above slurry A is evenly coated on the surface of the inorganic coating of the PE base film to obtain a first coating, and the coating weight of the first coating is 0.2g / m 2 , and complete drying in an oven.
[0145] For other steps and parameters of the third group of embodiments, please refer to the steps and parameters of the first group of embodiments, and finally a lithium-ion battery is obtained.
[0146] Table 3
[0147]
[0148] According to the test results in Table 3, it can be seen that by setting the second polymer to have a higher sphericity and a lower swelling degree (85° C.), the rate performance of the battery is improved.
[0149] It should be noted that the above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application; the implementation methods of the present application and the features in the implementation methods can be combined with each other without conflict. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A separation film, characterized in that: include: Basement membrane; An organic coating layer disposed on a surface of the base film, the organic coating layer comprising a first polymer and a second polymer; The melting point T of the first polymer satisfies 60°C≤T≤100°C; The swelling degree D of the second polymer when placed in a solution at 60° C. for 24 hours is ≤30%. The mass ratio of lithium hexafluorophosphate, ethylene carbonate, diethyl carbonate, propylene carbonate and propyl propionate in the solution is 8.7:20:30:20:
30.
2. The isolation film according to claim 1, characterized in that: The median particle size Dv50 of the first polymer satisfies 0.5 μm<Dv50<2 μm.
3. The isolation film according to claim 1, characterized in that: In the organic coating, the weight percentage of the first polymer is greater than or equal to 40% and less than or equal to 95%, and the weight percentage of the second polymer is less than or equal to 50%.
4. The isolation film according to claim 1, characterized in that: In the organic coating, the weight percentage of the first polymer is greater than or equal to 60% and less than or equal to 95%, and the weight percentage of the second polymer is less than or equal to 30%.
5. The isolation film according to claim 1, characterized in that: When the isolation membrane is applied to an electrochemical battery cell, the swelling degree D of the second polymer and the content H of the linear carboxylic acid ester in the electrolyte satisfy D=K*H+0.1, wherein 0.01≤K≤0.
08.
6. The isolation film according to claim 5, characterized in that: 10%≤H≤50%。 7. The isolation film according to claim 1, characterized in that: The median particle size Dv50 of the first polymer satisfies 1.0 μm≤Dv50≤2 μm.
8. The isolation film according to claim 1, characterized in that: The melting point T of the first polymer satisfies 60°C≤T≤85°C.
9. The isolation film according to claim 1, characterized in that: The second polymer is spherical or quasi-spherical, and the sphericity R of the second polymer satisfies 0.7≤R<1.
10. The isolation film according to claim 1, characterized in that: The second polymer is spherical or quasi-spherical, and the sphericity R of the second polymer satisfies 0.8≤R<1.
11. The isolation film according to claim 1, characterized in that: The swelling degree D of the second polymer when placed in an electrolyte at 85° C. for 24 hours satisfies 10%≤D≤50%.
12. The isolation film according to claim 1, characterized in that: The first polymer includes a graft copolymer, the monomer of the polymer main body in the graft copolymer includes at least one of ethylene, propylene, vinylidene fluoride, acrylic acid, acrylate, styrene, acrylonitrile, maleic anhydride, vinyl chloride and allyl chloride, and the monomer used for grafting includes at least one of maleic anhydride, acrylate and acrylic acid; the weight percentage of the graft copolymer in the first polymer is greater than or equal to 3% and less than or equal to 10%.
13. The isolation film according to claim 1, characterized in that: The second polymer includes a polymer of at least one monomer selected from vinylidene fluoride, hexafluoropropylene, propylene, vinyl chloride, styrene, butadiene, acrylate, and acrylic acid, and the second polymer is at least one selected from homopolymers, copolymers, and blended polymers.
14. A secondary battery comprising a positive electrode sheet, a negative electrode sheet and a separator disposed between the positive electrode sheet and the negative electrode sheet, characterized in that: The separator is the separator according to any one of claims 1 to 13, wherein the organic coating is located between the positive electrode sheet and the base film.
15. An electrochemical device comprising a positive electrode sheet, a negative electrode sheet, and a separator disposed between the positive electrode sheet and the negative electrode sheet, characterized in that: The separator is the separator according to any one of claims 1 to 13, wherein the organic coating is located between the positive electrode sheet and the base film.
16. An electrical device, characterized in that: The electrochemical device according to claim 15 or the secondary battery according to claim 14 is included.
Citation Information
Patent Citations
Organic functional porous isolating membrane, preparation method and lithium ion battery
CN107123767A
Coating diaphragm for lithium ion battery, preparation method and lithium ion battery
CN110729440A
Isolating membrane as well as electrochemical device and electronic device comprising isolating membrane
CN114175387A
Porous membrane with liner, method of manufacturing porous membrane, and method of manufacturing lithium secondary battery
JP2008027839A
Process for producing polymeric film fluorescing in ultraviolet light
SU960200A1