Bulk acoustic wave resonator, preparation method thereof and electronic equipment

CN119072849APending Publication Date: 2024-12-03BOE TECHNOLOGY GROUP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380008401.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing bulk acoustic resonators are prone to frequency drift when the temperature changes, resulting in unstable performance and failing to meet the high-performance requirements of filters in mobile communications.

Method used

A temperature drift compensation layer is set on the side of the piezoelectric layer of the bulk acoustic resonator that is close to or away from the substrate. The temperature drift is suppressed by using a material with thermal expansion and contraction properties. The lattice constant of the piezoelectric layer can be flexibly adjusted by adjusting the material and thickness of the temperature drift compensation layer, so as to achieve a resonant frequency with positive, negative or zero temperature coefficient.

Benefits of technology

It effectively suppresses temperature drift, improves the frequency stability and performance of the bulk acoustic resonator, and meets the high-performance requirements of filters in mobile communications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072849A_ABST
    Figure CN119072849A_ABST
Patent Text Reader

Abstract

The invention provides a bulk acoustic wave resonator, a preparation method thereof and electronic equipment, and belongs to the technical field of communication. The bulk acoustic wave resonator disclosed by the invention comprises a substrate, a first electrode, a piezoelectric layer and a second electrode, the first electrode is arranged on a substrate, the second electrode is arranged on the side, away from the substrate, of the first electrode, and the piezoelectric layer is arranged between the first electrode and the second electrode. Orthographic projections of any two of the first electrode, the piezoelectric layer and the second electrode on the substrate are at least partially overlapped; wherein one side, close to the substrate, of the piezoelectric layer, and / or one side, away from the substrate, of the piezoelectric layer is provided with a temperature drift compensation layer; the material of the temperature drift compensation layer has the property of thermal expansion and cold contraction, and is configured to suppress the temperature drift of the bulk acoustic wave resonator.
Need to check novelty before this filing date? Find Prior Art

Description

Bulk acoustic wave resonator, preparation method thereof, and electronic device Technical Field

[0001] The present disclosure belongs to the field of communication technology, and particularly relates to a bulk acoustic wave resonator, a preparation method thereof, and an electronic device. Background Art

[0002] In the field of mobile communications, because the total available frequency range is relatively narrow and there are many frequency bands used for mobile communications, the spacing between adjacent frequency bands is very narrow (approximately a few MHz to tens of MHz), and the bandwidth of a single frequency band is very narrow (tens of MHz), the filters used in mobile phones must have the performance characteristics of small in-band ripple, large out-of-band suppression, and good rectangularity. Conventional microstrip filters are large in size, have insufficient out-of-band suppression, and poor rectangularity, making them unsuitable. Cavity filters are also large in size and cannot be matched. Dielectric filters have large in-band insertion loss and poor rectangularity, making them unsuitable. IPD filters have large in-band ripple and poor rectangularity, making them unsuitable.

[0003] BAW resonators, the basic structural unit of BAW filters, currently use a silicon wafer as the substrate material, with a sandwich structure consisting of a first electrode, a piezoelectric material, and a second electrode from bottom to top. The operating principle is that a radio frequency signal is transmitted through the electrode at one end of the resonator. It is then converted into a mechanical vibration acoustic wave signal through the inverse piezoelectric effect at the interface between the piezoelectric material and the metal electrode. This acoustic wave signal forms a resonant standing wave with a certain frequency in the sandwich structure of the first electrode, piezoelectric material, and second electrode. The frequency of the radio frequency signal is equal to the resonant frequency of the resonator. The acoustic wave signal is then transmitted to the electrode at the other end of the resonator, where it is converted into a radio frequency signal through the piezoelectric effect at the interface between the metal electrode and the piezoelectric material. The resonator has a fixed resonant frequency. When the frequency of the RF signal is equal to the resonant frequency of the resonator, the conversion efficiency of RF signal → acoustic wave signal → RF signal is high; when the frequency of the RF signal is not equal to the resonant frequency of the resonator, the conversion efficiency of RF signal → acoustic wave signal → RF signal is very low, and most of the RF signals cannot be transmitted from the resonator. That is, the resonator is equivalent to the function of a filter to filter the RF signal.

[0004] Summary of the Invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art and provides a bulk acoustic wave resonator, a preparation method thereof, and an electronic device.

[0006] An embodiment of the present disclosure provides a bulk acoustic wave resonator, comprising: a substrate, a first electrode, a piezoelectric layer, and a second electrode; the first electrode is disposed on the substrate, the second electrode is disposed on a side of the first electrode facing away from the substrate, the piezoelectric layer is disposed between the first electrode and the second electrode, and the orthographic projections of any two of the first electrode, the piezoelectric layer, and the second electrode on the substrate at least partially overlap; wherein,

[0007] A temperature drift compensation layer is provided on a side of the piezoelectric layer close to the substrate and / or on a side of the piezoelectric layer away from the substrate; the material of the temperature drift compensation layer has the property of thermal expansion and contraction, and is configured to suppress the temperature drift of the bulk acoustic wave resonator.

[0008] The material of the temperature drift compensation layer is ZrW2O8, Zn2GeO4, HfW2O8, ZrMo2O8, HfMo2O8, ZrV2O7, HfV2O7, ZrV 1.7 Mo 0.3 O 7+δ 、ZrV 1.5 Mo 0.5 O 7+δ 、Cu2V2O7、Cu 2-x Zn x V2O7、Cu 2-y M y V2O7、Cu 1.5 Mg 0.5 V2O7, Cu2P2O7, Cu2PVO7, HfMgW3O 12 、HfMgMo3O 12 、ZrMgMo3O 12 、ZrMgW3O 12 、ZrMnMo3O 12 、HfMnMo3O 12 、AScY2XO 12 , TaVO5, NbVO5, Ag2O, Th2O(PO4)2, U2O(PO4)2, Zr2O(PO4)2, ScF3, CaZrF6, CaHfF6, MgZrF6, CaNbF6, CaTiF6, Z n(CN)2, Cd(CN)2, AgB(CN)4, CuB(CN)4, ScCo(CN)6, Si(NCN)2, Mn3AN(A=Zn,Ga), GdInO3, PbTiO3, PbVO3, PbVO 2.79 F 0.21 , PbV 1-x Cr x O3、Bi 0.5 Na 0.5VO3, GeTe, LaCu3Fe4O 12 , BiNiO3, V2OPO4, Ca2RuO4, Sr2IrO4, Sr2RhO4, Ca2MnO4, Ca2GeO4, Ca3Mn2O7, Ga3Ti2O7;

[0009] For Cu 2-x Zn x V2O7, where x is 0.1 or 0.2; Cu 2-y M y V2O7, where M is any one of Yb, Sm, and Ce, and y is 0.05; AScY2XO 12 , wherein A is Zr or Hf, Y is W or Mo, and X is V or P.

[0010] Wherein, the thickness of the temperature drift compensation layer is 1 nm-100 μm.

[0011] Wherein, the temperature drift compensation layer has a hollow pattern.

[0012] Wherein, when the temperature drift compensation layer is located on a side of the piezoelectric layer close to the base substrate, the temperature drift compensation layer is located on a side of the first electrode away from the piezoelectric layer.

[0013] When the temperature drift compensation layer is located on a side of the piezoelectric layer away from the base substrate, the temperature drift compensation layer is located on a side of the second electrode away from the piezoelectric layer.

[0014] The first electrode includes a first sub-electrode and a second sub-electrode arranged in sequence along a direction away from the base substrate. When the temperature drift compensation layer is located on the side of the piezoelectric layer close to the base substrate, the temperature drift compensation layer is located between the first sub-electrode and the second sub-electrode.

[0015] Among them, the first electrode includes a third sub-electrode and a fourth sub-electrode arranged in sequence along a direction away from the base substrate. When the temperature drift compensation layer is located on the side of the piezoelectric layer close to the base substrate, the temperature drift compensation layer is located between the third sub-electrode and the fourth sub-electrode.

[0016] The base substrate has a first groove portion penetrating a portion of the base substrate along a thickness direction thereof; an isolation layer is provided on a side of the opening of the first groove portion facing the first electrode.

[0017] The BAW resonator further includes an isolation layer provided between the base substrate and the first electrode; a certain space is defined between the isolation layer and the base substrate.

[0018] The base substrate has a first cavity penetrating along its thickness direction; and an isolation layer is provided on a side of the base substrate close to the first electrode.

[0019] An embodiment of the present disclosure also provides a method for preparing a bulk acoustic wave resonator, comprising: forming a first electrode, a piezoelectric layer, and a second electrode in sequence on a substrate, wherein the orthographic projections of any two of the first electrode, the piezoelectric layer, and the second electrode on the substrate at least partially overlap; wherein the preparation method further comprises: forming a temperature drift compensation layer on a side of the piezoelectric layer close to the first substrate, and / or forming the temperature drift compensation layer on a side of the voltage component away from the first substrate; the material of the temperature drift compensation layer has the property of thermal expansion and contraction, and is configured to suppress temperature drift of the bulk acoustic wave resonator.

[0020] The material of the temperature drift compensation layer is ZrW2O8, Zn2GeO4, HfW2O8, ZrMo2O8, HfMo2O8, ZrV2O7, HfV2O7, ZrV 1.7 Mo 0.3 O 7+δ 、ZrV 1.5 Mo 0.5 O 7+δ 、Cu2V2O7、Cu 2-x Zn x V2O7、Cu 2-y M y V2O7、Cu 1.5 Mg 0.5 V2O7, Cu2P2O7, Cu2PVO7, HfMgW3O 12 、HfMgMo3O 12 、ZrMgMo3O 12 、ZrMgW3O 12 、ZrMnMo3O 12 、HfMnMo3O 12 、AScY2XO 12 , TaVO5, NbVO5, Ag2O, Th2O(PO4)2, U2O(PO4)2, Zr2O(PO4)2, ScF3, CaZrF6, CaHfF6, MgZrF6, CaNbF6, CaTiF6, Z n(CN)2, Cd(CN)2, AgB(CN)4, CuB(CN)4, ScCo(CN)6, Si(NCN)2, Mn3AN(A=Zn,Ga), GdInO3, PbTiO3, PbVO3, PbVO 2.79 F 0.21 , PbV 1-x Cr x O3、Bi0.5 Na 0.5 VO3, GeTe, LaCu3Fe4O 12 , BiNiO3, V2OPO4, Ca2RuO4, Sr2IrO4, Sr2RhO4, Ca2MnO4, Ca2GeO4, Ca3Mn2O7, Ga3Ti2O7;

[0021] For Cu 2-x Zn x V2O7, where x is 0.1 or 0.2; Cu 2-y M y V2O7, where M is any one of Yb, Sm, and Ce, and y is 0.05; AScY2XO 12 , wherein A is Zr or Hf, Y is W or Mo, and X is V or P.

[0022] Wherein, the thickness of the temperature drift compensation layer is 1 nm-100 μm.

[0023] Wherein, the temperature drift compensation layer has a hollow pattern.

[0024] Wherein, when the preparation method includes forming the temperature drift compensation layer on a side of the piezoelectric layer close to the base substrate, the step of forming the temperature drift compensation layer is before the step of forming the first electrode.

[0025] Wherein, when the preparation method includes forming the temperature drift compensation layer on a side of the piezoelectric layer facing away from the base substrate, the step of forming the temperature drift compensation layer is after the step of forming the second electrode.

[0026] The step of forming the first electrode includes: forming a first sub-electrode and a second sub-electrode in sequence along a direction away from the substrate;

[0027] When the preparation method includes forming the temperature drift compensation layer on a side of the piezoelectric layer close to the base substrate, the step of forming the temperature drift compensation layer is between the step of forming the first sub-electrode and the step of forming the second sub-electrode.

[0028] The step of forming the second electrode includes: forming a third sub-electrode and a fourth sub-electrode in sequence along a direction away from the substrate;

[0029] When the preparation method includes forming the temperature drift compensation layer on a side of the piezoelectric layer facing away from the substrate, the step of forming the temperature drift compensation layer is between the step of forming the third sub-electrode and the step of forming the fourth sub-electrode.

[0030] The preparation method further includes: processing the base substrate to form a first groove portion penetrating a portion of the base substrate along its thickness direction; and providing an isolation layer on a side of the opening of the first groove portion facing the first electrode.

[0031] The preparation method further includes: forming an isolation layer before forming the first electrode; and defining a certain space between the isolation layer and the base substrate.

[0032] The preparation method further includes: processing the base substrate to form a first cavity penetrating along the thickness direction of the base substrate; and forming an isolation layer on a side of the base substrate close to the first electrode.

[0033] An embodiment of the present disclosure provides an electronic device, comprising any of the above-mentioned bulk acoustic wave resonators. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] FIG1 is a schematic structural diagram of a back-etched bulk acoustic wave resonator.

[0035] FIG2 is a schematic structural diagram of a thin film bulk acoustic wave resonator.

[0036] FIG3 is a schematic structural diagram of another thin film bulk acoustic wave resonator.

[0037] FIG4 is a schematic structural diagram of a solid-state assembled bulk acoustic wave resonator.

[0038] FIG5 is a schematic structural diagram of a first exemplary BAW resonator implemented in the present disclosure.

[0039] FIG6 is a flow chart of the preparation process of the BAW resonator shown in FIG5 .

[0040] FIG7 is a schematic structural diagram of a second exemplary BAW resonator implemented in the present disclosure.

[0041] FIG8 is a flow chart of the preparation process of the BAW resonator shown in FIG7 .

[0042] FIG9 is a schematic structural diagram of a third exemplary BAW resonator implemented in the present disclosure.

[0043] FIG10 is a schematic structural diagram of a fourth example of a bulk acoustic wave resonator implemented in the present disclosure.

[0044] FIG. 11 is a flow chart of the preparation process of the BAW resonator shown in FIG. 10 .

[0045] FIG12 is a schematic structural diagram of a fifth exemplary BAW resonator implemented in the present disclosure.

[0046] FIG13 is a flow chart of the preparation process of the BAW resonator shown in FIG12 .

[0047] FIG14 is a schematic structural diagram of a sixth exemplary BAW resonator implemented in the present disclosure.

[0048] FIG15 is a schematic structural diagram of a seventh exemplary BAW resonator implemented in the present disclosure.

[0049] FIG. 16 is a flow chart of the preparation process of the BAW resonator shown in FIG. 15 .

[0050] FIG17 is a schematic structural diagram of an eighth exemplary BAW resonator implemented in the present disclosure.

[0051] FIG18 is a flowchart of the preparation process of the BAW resonator shown in FIG17 .

[0052] FIG19 is a schematic structural diagram of a ninth exemplary BAW resonator implemented in the present disclosure.

[0053] FIG20 is a schematic structural diagram of a tenth example of a bulk acoustic wave resonator implemented in the present disclosure.

[0054] FIG. 21 is a flow chart of the preparation process of the BAW resonator shown in FIG. 20 .

[0055] FIG22 is a schematic structural diagram of an eleventh exemplary BAW resonator implemented in the present disclosure.

[0056] FIG23 is a schematic structural diagram of a twelfth example of a bulk acoustic wave resonator implemented in the present disclosure.

[0057] FIG. 24 is a flow chart of the preparation process of the BAW resonator shown in FIG. 23 .

[0058] FIG25 is a schematic structural diagram of a BAW resonator according to a thirteenth example of an embodiment of the present disclosure.

[0059] FIG26 is a schematic structural diagram of a BAW resonator according to a fourteenth example of an embodiment of the present disclosure.

[0060] FIG27 is a schematic structural diagram of a fifteenth example of a bulk acoustic wave resonator implemented in the present disclosure. DETAILED DESCRIPTION

[0061] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings and specific implementation methods.

[0062] Unless otherwise defined, the technical or scientific terms used in this disclosure should have the usual meanings understood by people with ordinary skills in the field to which this disclosure belongs. The words "first", "second" and similar words used in this disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one", "an" or "the" do not indicate a quantity limitation, but rather indicate the existence of at least one. Words such as "include" or "comprise" mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. Words such as "connect" or "connected" are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.

[0063] [Corrected 03.04.2023 according to Rule 91] As shown in Figures 1-4, to reduce insertion loss during filtering, a BAW resonator needs to confine the acoustic signal as much as possible within the piezoelectric layer 12 between the first electrode 11 and the second electrode 13 to prevent it from spreading outward. Therefore, acoustic reflectors are typically constructed on the upper and lower surfaces of the resonator. The upper surface generally uses a low-acoustic-impedance air medium as a reflector. Depending on the construction of the acoustic reflector on the lower surface, BAW resonators are divided into three major categories: back-etched BAW resonators (as shown in Figure 1); film bulk acoustic resonators (FBARs), as shown in Figures 2 and 3; and solid mounted resonators (SMRs), as shown in Figure 4. FBARs feature a first groove 102 etched into a first substrate 10 below the first electrode, serving as an air gap. The first electrode is then supported by an isolation layer 14, as shown in Figure 2. Alternatively, a first groove 102 is formed as an air gap through an isolation layer 14, as shown in FIG3 . The SMR method constructs an acoustic reflector structure 15 below the first electrode 11, which is formed by alternating and repeating high acoustic impedance layers 151 and low acoustic impedance material layers 152. The back-etch type constructs a first cavity 101 as an air layer on the first substrate 10 below the first electrode 11 by deeply etching the back side of the silicon substrate to form a cavity.

[0064] The inventors have discovered that in any of the aforementioned BAW resonators, the material of the piezoelectric layer 12 is C-axis oriented crystallized AlN. As the temperature rises, the in-plane lattice constant of this material increases, while the out-of-plane lattice constant decreases, resulting in a decrease in the speed of acoustic wave propagation. From the qualitative formula, it can be seen that the resonant frequency of the BAW resonator will decrease, that is, a temperature drift (abbreviated as: temperature drift) phenomenon will occur.

[0065] In response to the above technical problems, a temperature drift compensation layer is provided on the side of the piezoelectric layer 12 of the bulk acoustic wave resonator of the present embodiment close to the base substrate 10, and / or on the side of the piezoelectric layer 12 away from the base substrate 10, for resisting temperature drift. The material of the temperature drift compensation layer has the property of thermal expansion and contraction. Specifically, the temperature drift compensation layer can suppress the increase of the out-of-plane lattice constant of the thin film material of the piezoelectric layer 12 as the temperature rises, and the degree of suppression can be adjusted according to the specific material and thickness of the set temperature drift compensation layer. Therefore, the out-of-plane lattice constant of the thin film material of the piezoelectric layer 12 can become smaller, larger, or remain unchanged as the ambient temperature rises, that is, it can be flexibly adjusted, thereby obtaining a bulk acoustic wave resonator with a positive temperature coefficient, a negative temperature coefficient, or even a zero temperature coefficient.

[0066] It should be noted that to ensure the normal operation of the bulk acoustic wave resonator, when the temperature drift compensation layer is located on the side of the piezoelectric layer 12 close to the base substrate 10, the voltage layer still needs to maintain electrical connection with the first electrode 11; when the temperature drift compensation layer is located on the side of the piezoelectric layer 12 away from the base substrate 10, the voltage layer still needs to maintain electrical connection with the second electrode 13.

[0067] In addition, since back-etched BAW resonators and thin-film BAW resonators are prone to temperature drift problems, temperature drift compensation layers are mainly added to back-etched BAW resonators and thin-film BAW resonators. However, it is also feasible to add temperature drift compensation layers to solid-state assembled BAW resonators. The following only illustrates some situations in which a temperature drift compensation layer is added to the thin-film BAW resonator shown in FIG2 . In order to more clearly introduce the BAW resonator in the embodiment of the present disclosure, the temperature drift compensation layer located on the side of the piezoelectric layer 12 close to the base substrate 10 is referred to as the first temperature drift compensation layer 21, and the temperature drift compensation layer located on the side of the piezoelectric layer 12 away from the base substrate 10 is referred to as the second temperature drift compensation layer 22.

[0068] First example: FIG5 is a schematic structural diagram of a BAW resonator according to the first example of the present disclosure. As shown in FIG5 , the BAW resonator includes a base substrate 10, an isolation layer 14, a first temperature drift compensation layer 21, a first electrode 11, a piezoelectric layer 12, and a second electrode 13 sequentially arranged on the base substrate 10. The base substrate 10 has a first groove 102 that penetrates a portion of the base substrate 10 along its thickness direction, i.e., an air gap is formed below the isolation layer 14. The release hole 30 that penetrates the first electrode 11, the first temperature drift compensation layer 21, and the isolation layer 14 is used to release the sacrificial layer formed in the first groove 102 during the preparation of the BAW resonator (detailed description will be given in the preparation method).

[0069] Continuing with Figure 5 , an RF signal enters the upper left corner of Figure 5 , is converted into an acoustic wave signal through the inverse piezoelectric effect at the interface between second electrode 13 and piezoelectric layer 12, propagates longitudinally through piezoelectric layer 12, and upon reaching the interface between first electrode 11 and piezoelectric layer 12, is converted back into an RF signal through the piezoelectric effect and then transmitted outward. The air gap below the BAW resonator and the air layer above it act as acoustic reflectors, confining the acoustic signal within the resonator structure rather than dissipating it, thereby reducing the resonator's insertion loss. The first temperature-drift compensation layer 21 in the disclosed embodiment is different from general materials. Its temperature-drift compensation layer material has the property of thermal contraction and thermal expansion. When the ambient temperature rises, the increase in the in-plane lattice constant of the piezoelectric layer 12 material connected to the first temperature-drift compensation layer 21 via the first electrode 11 is suppressed. The degree of suppression can be adjusted by factors such as the selection of different types of temperature-drift compensation layer thin film materials and the thickness of the temperature-drift compensation layer. Therefore, the out-of-plane lattice constant of the piezoelectric layer 12 can decrease, increase, or remain unchanged as the ambient temperature rises. In other words, it can be flexibly adjusted, thereby obtaining a bulk acoustic wave resonator with a positive temperature coefficient, a negative temperature coefficient, or even a zero temperature coefficient.

[0070] In some examples, the material of the base substrate 10 is preferably glass, but Si, sapphire, SiC, GaAs, GaN, InP, BN, ZnO, etc. can also be selected. The thickness of the base substrate 10 ranges from 0.1 μm to 10 mm. The thickness of the air gap on the base substrate 10 ranges from 0.1 μm to 50 μm.

[0071] In some examples, the first electrode 11 is made of a metal material, such as Mo. Alternatively, the first electrode 11 may be made of Cu, Al, Co, Ag, Ti, Pt, Ru, W, or Au, or an alloy formed by any combination of the above metals. The thickness of the first electrode 11 ranges from about 1 nm to about 10 μm.

[0072] In some examples, the material of the piezoelectric layer 12 is preferably hBN, and cBN and wBN can also be selected. Of course, the material of the piezoelectric layer 12 can also be selected from AlN, ZnO, PZT, GaN, InN, CdS, CdSe, ZnS, CdTe, ZnTe, GaAs, GaSb, InAs, InSb, GaSe, GaP, AlP, quartz crystal, LiTaO3, LiNbO3, La3Ga5SiO14, BaTiO3, PbNb2O6, PBLN, LiGaO3, LiGeO3, TiGeO3, PbTiO3, PbZrO3, PVDF and other materials. The piezoelectric layer 12 in this embodiment can be one of the above-mentioned piezoelectric materials, or it can be a stack of the above-mentioned various piezoelectric materials. The thickness of the piezoelectric layer 12 ranges from 10nm to 100μm.

[0073] In some examples, the second electrode 13 may be made of Cu, Al, Mo, Co, Ag, Ti, Pt, Ru, W, or Au, or may be an alloy of the above metals. The thickness of the second electrode 13 ranges from 1 nm to 10 μm.

[0074] In some examples, the isolation layer 14 is used to electrically isolate the air gap from the BAW resonator and provide structural support. The isolation layer 14 may be made of insulating materials such as SiO2, Si3N4, Al2O3, and combinations thereof. The thickness ranges from 1 nm to 100 μm.

[0075] In some examples, the first temperature drift compensation layer 21 is a thin film composed of a material having the property of thermal contraction and cold expansion. The optional materials include ZrW2O8, Zn2GeO4, HfW2O8, ZrMo2O8, HfMo2O8, ZrV2O7, HfV2O7, ZrV 1.7 Mo 0.3 O 7+δ 、ZrV 1.5 Mo 0.5 O 7+δ 、Cu2V2O7、Cu 2-x Zn x V2O7 (x is 0.1 or 0.2), Cu 2-y M y V2O7 (M is any one of Yb, Sm, Ce, y is 0.05), Cu 1.5 Mg 0.5 V2O7, Cu2P2O7, Cu2PVO7, HfMgW3O 12 、HfMgMo3O 12 、ZrMgMo3O 12 、ZrMgW3O 12、ZrMnMo3O 12 、HfMnMo3O 12 、AScY2XO 12 (A is Zr or Hf, Y is W or Mo, X is V or P), TaVO5, NbVO5, Ag2O, Th2O(PO4)2, U2O(PO4)2, Zr2O(PO4)2, ScF3, CaZrF6, CaHfF6, MgZrF6, CaNbF6, CaTiF6, Zn(CN)2, Cd(CN)2, AgB(CN)4, CuB(CN)4, ScCo(CN)6, Si(NCN)2, Mn3AN(A=Zn,Ga), GdInO3, PbTiO3, PbVO3, PbVO 2.79 F 0.21 , PbV 1-x Cr x O3、Bi 0.5 Na 0.5 VO3, GeTe, LaCu3Fe4O 12 , BiNiO3, V2OPO4, Ca2RuO4, Sr2IrO4, Sr2RhO4, Ca2MnO4, Ca2GeO4, Ca3Mn2O7, Ga3Ti2O7. The thickness of the first temperature drift compensation layer 21 ranges from 1nm to 100um.

[0076] In some examples, referring to FIG5 , an encapsulation layer 16 is provided on the side of the second electrode 13 facing away from the substrate 10. The material of the encapsulation layer 16 is preferably an organic compound that can isolate water vapor and oxygen, such as polyimide, epoxy resin, etc., or an inorganic material such as SiN x , Al2O3, etc. The encapsulation layer 16 can be a single layer of a single material, or a stacked configuration of multiple materials.

[0077] Next, the preparation method of the BAW resonator in the first example is described. FIG6 is a flow chart of the preparation of the BAW resonator shown in FIG5 ; as shown in FIG6 , the preparation method specifically includes the following steps.

[0078] S11 , providing a base substrate 10 .

[0079] In some examples, taking the substrate 10 as an example of a single crystal silicon substrate, step S11 can specifically include: first, ultrasonically cleaning the single crystal silicon substrate with deionized water; then placing it in a H2SO4:H2O=3:1 mixed solution, heating it to 250°C and washing it for 15 minutes; then placing it in deionized water and ultrasonically cleaning it; then placing it in a NH4OH:H2O=1:6 mixed solution, heating it to 80°C and washing it for 15 minutes; taking it out and placing it in deionized water for rinsing; next, placing it in a HCl:H2O2:H2O=1:1:5 mixed solution, heating it to 85°C and washing it for 15 minutes, taking it out and placing it in a HF:H2O=1:20 dilute hydrofluoric acid and rinsing it for 10 seconds to remove the surface oxide layer; finally, placing it in deionized water for ultrasonic cleaning for 20 minutes, blow-drying it with an air knife, and completing the entire substrate 10 cleaning process.

[0080] S12 , forming a first groove portion 102 on the base substrate 10 .

[0081] In some examples, step S12 may specifically include: preparing a mask pattern on the substrate 10, performing a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Then, performing an etching process to form the first groove 102. The etching process may be either wet etching or dry etching, with wet etching being preferred. Finally, performing a resist stripping process to complete the preparation of the first groove 102.

[0082] S13 , forming a sacrificial layer in the first groove 102 .

[0083] In some examples, the material of the sacrificial layer can be loose amorphous silicon dioxide doped with boron and phosphorus. Step S13 can specifically include forming a slurry containing loose silicon dioxide doped with boron and phosphorus using any of the processes of plasma enhanced chemical vapor deposition (PECVD), subatmospheric pressure chemical vapor deposition (SACVD), and screen printing, and then performing thermal annealing at 700-900°C for 15-30 minutes in a vacuum chamber to liquefy and flow the loose amorphous silicon dioxide film doped with boron and phosphorus, completely filling the pores in the first groove portion 102, leveling it, and then cooling and solidifying it. Finally, chemical mechanical polishing is performed, where the base substrate 10 is pressed against a rough polishing pad using a polishing head. By means of the coupled effects of polishing liquid corrosion, particle friction, and polishing pad friction, the surface of the base substrate 10 is flattened after a certain period of time, and the surface of the material overflowing from the surface of the first groove portion 102 is polished to a height equivalent to the surface height of the base substrate 10.

[0084] S14 , forming an isolation layer 14 on the base substrate 10 .

[0085] In some examples, step S14 may specifically include: preparing an isolation layer 14 thin film on the substrate 10, first depositing an electrically insulating material, the deposition method of which may be radio frequency magnetron sputtering, pulsed laser sputtering (PLD), atomic layer deposition (ALD), or plasma chemical vapor deposition (PECVD). The isolation layer 14 is subjected to a photolithography process to form a pattern including the isolation layer 14, the photolithography process including coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably a wet etching process, but a dry etching process may also be selected.

[0086] S15 , forming a first temperature drift compensation layer 21 on a side of the isolation layer 14 facing away from the base substrate 10 .

[0087] In some examples, step S15 may specifically include: first depositing a thin film of the first temperature drift compensation layer 21, preferably using radio frequency magnetron sputtering, but also alternatively using pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), sol-gel method (preparing a slurry containing the temperature drift compensation layer material and then heating and sintering it), thermal evaporation, electron beam evaporation, and the like. The temperature drift compensation layer thin film then undergoes a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably using a wet etching process, but also using a dry etching process, to form a pattern of the first temperature drift compensation layer 21.

[0088] S16 , forming a first electrode 11 on a side of the first temperature drift compensation layer 21 facing away from the base substrate 10 .

[0089] In some examples, when the first electrode 11 is made of a metal material, step S16 may include depositing a first metal film on the side of the first temperature drift compensation layer 21 away from the base substrate 10. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. A copper foil attachment method can also be used. Thereafter, the first metal film is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Next, etching is performed to form a pattern including the first electrode 11. The etching process preferably adopts a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the first electrode 11.

[0090] S17 , forming a release hole 30 penetrating the first electrode 11 , the isolation layer 14 and the first temperature drift compensation layer 21 .

[0091] In some examples, step S17 may include performing a photolithography process on the side of the first electrode 11 facing away from the substrate 10, including resist coating (or spraying), pre-baking, exposure, development, and post-baking to expose the hole. A dry etching process is then performed to etch the first electrode 11. The etching gas is then changed to etch the first temperature drift compensation layer 21. Finally, the etching gas is changed to etch the isolation layer 14 until the sacrificial layer is etched. Finally, a resist stripping process is performed to form the release hole 30.

[0092] S18 , forming a piezoelectric layer 12 on a side of the first electrode 11 facing away from the substrate 10 .

[0093] In some examples, taking the piezoelectric layer 12 as an example of an AlN single-layer structure, step S18 may include forming a piezoelectric material layer on the side of the first electrode 11 away from the substrate 10, and performing oriented growth of the piezoelectric material layer. The piezoelectric material layer is preferably formed by radio frequency magnetron sputtering (DC measurement and control sputtering is also possible). For AlN piezoelectric material, the target material is Al. By controlling the Ar and N2 gas pressures and temperatures during the deposition process and the post-annealing time and temperature, an AlN C-axis oriented piezoelectric material layer is formed, and the preferred growth orientation is (001). The deposition method of the piezoelectric material layer can also be selected from pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), etc. Next, the piezoelectric layer 12 is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Etching is then performed to form a pattern including the piezoelectric layer 12. A wet etching process is preferably used, but a dry etching process can also be used. Finally, a debonding process is performed to complete the preparation of the piezoelectric layer 12 .

[0094] S19 . Form a second electrode 13 on a side of the piezoelectric layer 12 facing away from the first electrode 11 .

[0095] In some examples, when the second electrode 13 is made of a metal material, step S19 may specifically include first depositing a third metal film on the side of the piezoelectric layer 12 away from the first electrode 11. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Next, the third metal film is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Thereafter, etching is performed to form a pattern including the second electrode 13. The etching process is preferably a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the second electrode 13.

[0096] S110 , removing the sacrificial layer.

[0097] In some examples, step S110 may include etching the sacrificial layer, preferably using a wet etching process. Immersion etching is performed using a mixture of hydrofluoric acid, dilute nitric acid, and deionized water (the etching temperature may be appropriately increased to increase the wet etching rate) for a sufficient period of time to ensure that the boron- and phosphorus-doped silicon dioxide filling material in the first groove portion 102 is completely dissolved. Finally, the first groove portion 102 is ultrasonically cleaned multiple times with deionized water and dried to form the first groove portion 102.

[0098] S111 , forming an encapsulation layer 16 on a side of the second electrode 13 facing away from the base substrate 10 .

[0099] In some examples, taking the encapsulation layer 16 as an example using an organic compound material, step S111 may specifically include first coating the organic material liquid, which may be done by spin coating, spraying, inkjet printing, transfer, etc., and then heating and curing to form a pattern of the encapsulation layer 16.

[0100] Of course, if multiple BAW resonators are prepared together, the preparation method provided in the embodiment of the present disclosure may further include a step of device cutting.

[0101] Second Example: FIG7 is a schematic structural diagram of a BAW resonator according to the second example of the present disclosure. As shown in FIG7 , the BAW resonator includes a base substrate 10, an isolation layer 14, a first temperature drift compensation layer 21, a first electrode 11, a piezoelectric layer 12, and a second electrode 13 disposed on the base substrate 10. The first electrode 11 includes a first sub-electrode 111 and a second sub-electrode 112. In the BAW resonator, the isolation layer 14, the first sub-electrode 111, the first temperature drift compensation layer 21, the second sub-electrode 112, the piezoelectric layer 12, and the second electrode 13 are sequentially disposed in a direction away from the base substrate 10. The base substrate 10 has a first groove 102 extending through a portion of the base substrate 10 along its thickness, forming an air gap below the isolation layer 14. The release hole 30 that passes through the first sub-electrode 111, the second sub-electrode 112, the first temperature drift compensation layer 21 and the isolation layer 14 is used to release the sacrificial layer formed in the first groove 102 during the preparation of the bulk acoustic wave resonator (specific details are described in detail in the preparation method).

[0102] Continuing with Figure 7 , an RF signal enters the upper left corner of Figure 7 , is converted into an acoustic wave signal through the inverse piezoelectric effect at the interface between second electrode 13 and piezoelectric layer 12, propagates longitudinally through piezoelectric layer 12, and is converted back into an RF signal through the piezoelectric effect at the interface between second sub-electrode 112 and piezoelectric layer 12 before being transmitted outward. The air gap below the BAW resonator and the air layer above it act as acoustic reflectors, confining the acoustic signal within the resonator structure rather than dissipating it, thereby reducing the resonator's insertion loss. The first temperature-drift compensation layer 21 in the disclosed embodiment is different from general materials. Its temperature-drift compensation layer material has the property of thermal contraction and thermal expansion. When the ambient temperature rises, the increase in the in-plane lattice constant of the piezoelectric layer 12 material connected to the first temperature-drift compensation layer 21 via the first electrode 11 is suppressed. The degree of suppression can be adjusted by factors such as the selection of different types of temperature-drift compensation layer thin film materials and the thickness of the temperature-drift compensation layer. Therefore, the out-of-plane lattice constant of the piezoelectric layer 12 can decrease, increase, or remain unchanged as the ambient temperature rises. In other words, it can be flexibly adjusted, thereby obtaining a bulk acoustic wave resonator with a positive temperature coefficient, a negative temperature coefficient, or even a zero temperature coefficient.

[0103] In some examples, the material of the base substrate 10 is preferably glass, but Si, sapphire, SiC, GaAs, GaN, InP, BN, ZnO, etc. can also be selected. The thickness of the base substrate 10 ranges from 0.1 μm to 10 mm. The thickness of the air gap on the base substrate 10 ranges from 0.1 μm to 50 μm.

[0104] In some examples, the first sub-electrode 111 and the second sub-electrode 112 are made of a metal material, such as Mo. Alternatively, the first sub-electrode 111 and the second sub-electrode 112 may be made of Cu, Al, Co, Ag, Ti, Pt, Ru, W, or Au, or may be alloys formed by any combination of the above metals. The thickness of the first electrode 11, formed by the first sub-electrode 111 and the second sub-electrode 112, ranges from approximately 1 nm to 10 μm.

[0105] In some examples, the material of the piezoelectric layer 12 is preferably hBN, and cBN and wBN can also be selected. Of course, the material of the piezoelectric layer 12 can also be selected from AlN, ZnO, PZT, GaN, InN, CdS, CdSe, ZnS, CdTe, ZnTe, GaAs, GaSb, InAs, InSb, GaSe, GaP, AlP, quartz crystal, LiTaO3, LiNbO3, La3Ga5SiO14, BaTiO3, PbNb2O6, PBLN, LiGaO3, LiGeO3, TiGeO3, PbTiO3, PbZrO3, PVDF and other materials. The piezoelectric layer 12 in this embodiment can be one of the above-mentioned piezoelectric materials, or it can be a stack of the above-mentioned various piezoelectric materials. The thickness of the piezoelectric layer 12 ranges from 10nm to 100μm.

[0106] In some examples, the second electrode 13 may be made of Cu, Al, Mo, Co, Ag, Ti, Pt, Ru, W, or Au, or may be an alloy of the above metals. The thickness of the second electrode 13 ranges from 1 nm to 10 μm.

[0107] In some examples, the isolation layer 14 is used to electrically isolate the air gap from the BAW resonator and provide structural support. The isolation layer 14 may be made of insulating materials such as SiO2, Si3N4, Al2O3, and combinations thereof. The thickness ranges from 1 nm to 100 μm.

[0108] In some examples, the first temperature drift compensation layer 21 is a thin film composed of a material having the property of thermal contraction and cold expansion. The optional materials include ZrW2O8, Zn2GeO4, HfW2O8, ZrMo2O8, HfMo2O8, ZrV2O7, HfV2O7, ZrV 1.7 Mo 0.3 O 7+δ 、ZrV 1.5 Mo 0.5 O 7+δ 、Cu2V2O7、Cu 2-x Zn x V2O7 (x is 0.1 or 0.2), Cu 2-y M y V2O7 (M is any one of Yb, Sm, Ce, y is 0.05), Cu 1.5 Mg 0.5 V2O7, Cu2P2O7, Cu2PVO7, HfMgW3O 12 、HfMgMo3O 12 、ZrMgMo3O 12 、ZrMgW3O 12、ZrMnMo3O 12 、HfMnMo3O 12 、AScY2XO 12 (A is Zr or Hf, Y is W or Mo, X is V or P), TaVO5, NbVO5, Ag2O, Th2O(PO4)2, U2O(PO4)2, Zr2O(PO4)2, ScF3, CaZrF6, CaHfF6, MgZrF6, CaNbF6, CaTiF6, Zn(CN)2, Cd(CN)2, AgB(CN)4, CuB(CN)4, ScCo(CN)6, Si(NCN)2, Mn3AN(A=Zn,Ga), GdInO3, PbTiO3, PbVO3, PbVO 2.79 F 0.21 , PbV 1-x Cr x O3、Bi 0.5 Na 0.5 VO3, GeTe, LaCu3Fe4O 12 , BiNiO3, V2OPO4, Ca2RuO4, Sr2IrO4, Sr2RhO4, Ca2MnO4, Ca2GeO4, Ca3Mn2O7, Ga3Ti2O7. The thickness of the first temperature drift compensation layer 21 ranges from 1nm to 100um.

[0109] In some examples, referring to FIG7 , an encapsulation layer 16 is provided on the side of the second electrode 13 facing away from the substrate 10. The material of the encapsulation layer 16 is preferably an organic compound that can isolate water vapor and oxygen, such as polyimide, epoxy resin, etc., or an inorganic material such as SiN x , Al2O3, etc. The encapsulation layer 16 can be a single layer of a single material, or a stacked configuration of multiple materials.

[0110] Next, the preparation method of the BAW resonator in the second example is described. FIG8 is a flow chart of the preparation of the BAW resonator shown in FIG7 ; as shown in FIG8 , the preparation method specifically includes the following steps.

[0111] S21 , providing a base substrate 10 .

[0112] In some examples, taking the substrate 10 as an example of a single crystal silicon substrate, step S21 can specifically include: first, ultrasonically cleaning the single crystal silicon substrate with deionized water; then placing it in a H2SO4:H2O=3:1 mixed solution, heating it to 250°C and washing it for 15 minutes; then placing it in deionized water and ultrasonically cleaning it; then placing it in a NH4OH:H2O=1:6 mixed solution, heating it to 80°C and washing it for 15 minutes; taking it out and placing it in deionized water for rinsing; next, placing it in a HCl:H2O2:H2O=1:1:5 mixed solution, heating it to 85°C and washing it for 15 minutes, taking it out and placing it in a HF:H2O=1:20 dilute hydrofluoric acid and rinsing it for 10 seconds to remove the surface oxide layer; finally, placing it in deionized water for ultrasonic cleaning for 20 minutes, blow-drying it with an air knife, and completing the entire substrate 10 cleaning process.

[0113] S22 , forming a first groove portion 102 on the base substrate 10 .

[0114] In some examples, step S22 may specifically include: preparing a mask pattern on the substrate 10, performing a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Then, performing an etching process to form the first groove 102. The etching process may be either wet etching or dry etching, with wet etching being preferred. Finally, performing a resist stripping process to complete the preparation of the first groove 102.

[0115] S23 , forming a sacrificial layer in the first groove 102 .

[0116] In some examples, the material of the sacrificial layer can be loose amorphous silicon dioxide doped with boron and phosphorus. Step S23 can specifically include forming a slurry containing loose silicon dioxide doped with boron and phosphorus using any of the processes of plasma enhanced chemical vapor deposition (PECVD), sub-atmospheric pressure chemical vapor deposition (SACVD), and screen printing, and then performing thermal annealing at 700-900°C for 15-30 minutes in a vacuum chamber to liquefy and flow the loose amorphous silicon dioxide film doped with boron and phosphorus, completely filling the pores in the first groove portion 102, leveling it, and then cooling and solidifying it. Finally, chemical mechanical polishing is performed, where the base substrate 10 is pressed against a rough polishing pad using a polishing head. By means of the coupled effects of polishing liquid corrosion, particle friction, and polishing pad friction, the surface of the base substrate 10 is flattened after a certain period of time, and the surface of the material overflowing from the surface of the first groove portion 102 is polished to a height equivalent to the surface height of the base substrate 10.

[0117] S24 , forming an isolation layer 14 on the base substrate 10 .

[0118] In some examples, step S24 may specifically include: preparing an isolation layer 14 thin film on the substrate 10, first depositing an electrically insulating material, the deposition method of which may be radio frequency magnetron sputtering, pulsed laser sputtering (PLD), atomic layer deposition (ALD), or plasma chemical vapor deposition (PECVD). The isolation layer 14 is subjected to a photolithography process to form a pattern including the isolation layer 14, the photolithography process including coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably a wet etching process, but a dry etching process may also be selected.

[0119] S25 , forming a first sub-electrode 111 on a side of the isolation layer 14 facing away from the base substrate 10 .

[0120] In some examples, when the first electrode 11 is made of a metal material, step S25 may include depositing a first metal film on the side of the isolation layer 14 away from the base substrate 10. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. The copper foil attachment method can also be used. Thereafter, the second metal film is subjected to a photolithography process, including glue coating (or glue spraying), pre-baking, exposure, development, and post-baking. Next, etching is performed to form a pattern including the first sub-electrode 111. The etching process preferably adopts a wet etching process, and a dry etching process can also be selected. Finally, a de-gumming process is performed to complete the preparation of the first sub-electrode 111.

[0121] S26 , forming a first temperature drift compensation layer 21 on a side of the first sub-electrode 111 facing away from the base substrate 10 .

[0122] In some examples, step S26 may specifically include: first depositing a thin film of the first temperature drift compensation layer 21, preferably using radio frequency magnetron sputtering, but also alternatively using pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), sol-gel method (preparing a slurry containing the temperature drift compensation layer material and then heating and sintering it), thermal evaporation, electron beam evaporation, and the like. The temperature drift compensation layer thin film then undergoes a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably using a wet etching process, but also using a dry etching process, to form a pattern of the first temperature drift compensation layer 21.

[0123] S27 , forming a second sub-electrode 112 on a side of the first temperature drift compensation layer 21 facing away from the base substrate 10 .

[0124] In some examples, when the second sub-electrode 112 is made of a metal material, step S27 may include depositing a second metal film on the side of the first temperature drift compensation layer 21 facing away from the base substrate 10. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Copper foil can also be attached. The second metal film is then subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Next, etching is performed to form a pattern including the second sub-electrode 112. The etching process preferably uses a wet etching process, but a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the second sub-electrode 112.

[0125] S28 , forming a release hole 30 penetrating the first sub-electrode 111 , the second sub-electrode 112 , the isolation layer 14 and the first temperature drift compensation layer 21 .

[0126] In some examples, step S28 may include performing a photolithography process on the side of the second sub-electrode 112 facing away from the substrate 10, including resist coating (or spraying), pre-baking, exposure, development, and post-baking, to expose the hole. A dry etching process is then performed to etch the second sub-electrode 112. The etching gas is then changed to etch the first drift compensation layer 21. The etching gas is then changed to etch the first sub-electrode 111. Finally, the etching gas is changed to etch the isolation layer 14 until the sacrificial layer is etched. Finally, a resist stripping process is performed to form the release hole 30.

[0127] S29 , forming a piezoelectric layer 12 on a side of the first electrode 11 facing away from the substrate 10 .

[0128] In some examples, taking the piezoelectric layer 12 as an example of an AlN single-layer structure, step S29 may include forming a piezoelectric material layer on the side of the first electrode 11 away from the substrate 10, and performing oriented growth of the piezoelectric material layer. The piezoelectric material layer is preferably formed by radio frequency magnetron sputtering (DC measurement and control sputtering is also possible). For AlN piezoelectric material, the target material is Al. By controlling the Ar and N2 gas pressures and temperatures during the deposition process and the post-annealing time and temperature, an AlN C-axis oriented piezoelectric material layer is formed, and the preferred growth orientation is (001). The deposition method of the piezoelectric material layer can also be selected from pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), etc. Next, the piezoelectric layer 12 is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Etching is then performed to form a pattern including the piezoelectric layer 12. A wet etching process is preferably used, but a dry etching process can also be used. Finally, a debonding process is performed to complete the preparation of the piezoelectric layer 12 .

[0129] S210 , forming a second electrode 13 on a side of the piezoelectric layer 12 facing away from the first electrode 11 .

[0130] In some examples, when the second electrode 13 is made of a metal material, step S210 may specifically include first depositing a third metal film on the side of the piezoelectric layer 12 away from the first electrode 11. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Next, the third metal film is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Thereafter, etching is performed to form a pattern including the second electrode 13. The etching process is preferably a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the second electrode 13.

[0131] S211 , removing the sacrificial layer.

[0132] In some examples, step S211 may include etching the sacrificial layer, preferably using a wet etching process. Immersion etching is performed using a mixture of hydrofluoric acid, dilute nitric acid, and deionized water (the etching temperature may be appropriately increased to increase the wet etching rate) for a sufficient period of time to ensure that the boron- and phosphorus-doped silicon dioxide filling material in the first groove portion 102 is completely dissolved. Finally, the first groove portion 102 is ultrasonically cleaned multiple times with deionized water and dried to form the first groove portion 102.

[0133] S212 , forming an encapsulation layer 16 on a side of the second electrode 13 facing away from the base substrate 10 .

[0134] In some examples, taking the encapsulation layer 16 as an example using an organic compound material, step S212 may specifically include first coating the organic material liquid, which may be done by spin coating, spraying, inkjet printing, transfer, etc., and then heating and curing to form a pattern of the encapsulation layer 16.

[0135] Of course, if multiple BAW resonators are prepared together, the preparation method provided in the embodiment of the present disclosure may further include a step of device cutting.

[0136] Third Example: FIG9 is a schematic diagram of the structure of the BAW resonator of the third example implemented in the present disclosure; as shown in FIG9 , the structure of the BAW resonator of this example is substantially the same as that of the BAW resonator in the second example, with the only difference being that in this example, the first temperature drift compensation layer 21 has a hollow pattern, and the first temperature drift compensation layer 21 also has a through hole extending through its thickness. In this case, the first sub-electrode 111 and the second sub-electrode 112 of the first electrode 11 can be electrically connected through the through hole extending through the first temperature drift compensation layer 21, thereby reducing the resistance of the first electrode 11 and, in turn, reducing the in-band insertion loss of the BAW resonator. The remaining structures in this BAW resonator can adopt the same structure as in the second example, so they will not be described in detail here.

[0137] The preparation method of the bulk acoustic wave resonator in the third example can be prepared using the same method as in the second example. The only difference from the second example is that when forming the first temperature drift compensation layer 21, a through hole is formed that penetrates along its thickness direction, that is, a hollow pattern is formed. The remaining steps are the same as those in the second example, so they will not be repeated here.

[0138] Fourth Example: FIG10 is a schematic structural diagram of a BAW resonator according to the fourth example of the present disclosure. As shown in FIG10 , the BAW resonator includes a substrate 10, an isolation layer 14, a first electrode 11, a piezoelectric layer 12, a second electrode 13, and a second temperature drift compensation layer 22 sequentially arranged on the substrate 10. The substrate 10 has a first groove 102 that penetrates a portion of the substrate 10 along its thickness, forming an air gap below the isolation layer 14. A release hole 30 that penetrates the first electrode 11 and the isolation layer 14 is used to release the sacrificial layer formed in the first groove 102 during the preparation of the BAW resonator (details are described in detail in the preparation method).

[0139] Continuing with Figure 10 , an RF signal enters from the upper left corner of Figure 10 . It is then converted into an acoustic wave signal through the inverse piezoelectric effect at the interface between second electrode 13 and piezoelectric layer 12. This acoustic wave propagates longitudinally through piezoelectric layer 12, and upon reaching the interface between first electrode 11 and piezoelectric layer 12, it is converted back into an RF signal through the piezoelectric effect and then transmitted outward. The air gap below the BAW resonator and the air layer above it act as acoustic reflectors, confining the acoustic signal within the resonator structure rather than dissipating it, thereby reducing the resonator's insertion loss. The second temperature drift compensation layer 22 in the disclosed embodiment is different from general materials. The material of the second temperature drift compensation layer 22 has the property of thermal contraction and thermal expansion. When the ambient temperature rises, the increase in the in-plane lattice constant of the piezoelectric layer 12 material connected to the second temperature drift compensation layer 22 via the second electrode 13 is suppressed. The degree of suppression can be adjusted by factors such as the selection of different types of temperature drift compensation layer thin film materials and the thickness of the temperature drift compensation layer. Therefore, the out-of-plane lattice constant of the piezoelectric layer 12 can decrease, increase, or remain unchanged as the ambient temperature rises. In other words, it can be flexibly adjusted to obtain a bulk acoustic wave resonator with a positive temperature coefficient, a negative temperature coefficient, or even a zero temperature coefficient.

[0140] In some examples, the material of the base substrate 10 is preferably glass, but Si, sapphire, SiC, GaAs, GaN, InP, BN, ZnO, etc. can also be selected. The thickness of the base substrate 10 ranges from 0.1 μm to 10 mm. The thickness of the air gap on the base substrate 10 ranges from 0.1 μm to 50 μm.

[0141] In some examples, the first electrode 11 is made of a metal material, such as Mo. Alternatively, the first electrode 11 may be made of Cu, Al, Co, Ag, Ti, Pt, Ru, W, or Au, or an alloy formed by any combination of the above metals. The thickness of the first electrode 11 ranges from about 1 nm to about 10 μm.

[0142] In some examples, the material of the piezoelectric layer 12 is preferably hBN, and cBN and wBN can also be selected. Of course, the material of the piezoelectric layer 12 can also be selected from AlN, ZnO, PZT, GaN, InN, CdS, CdSe, ZnS, CdTe, ZnTe, GaAs, GaSb, InAs, InSb, GaSe, GaP, AlP, quartz crystal, LiTaO3, LiNbO3, La3Ga5SiO14, BaTiO3, PbNb2O6, PBLN, LiGaO3, LiGeO3, TiGeO3, PbTiO3, PbZrO3, PVDF and other materials. The piezoelectric layer 12 in this embodiment can be one of the above-mentioned piezoelectric materials, or it can be a stack of the above-mentioned various piezoelectric materials. The thickness of the piezoelectric layer 12 ranges from 10nm to 100μm.

[0143] In some examples, the second electrode 13 may be made of Cu, Al, Mo, Co, Ag, Ti, Pt, Ru, W, or Au, or may be an alloy of the above metals. The thickness of the second electrode 13 ranges from 1 nm to 10 μm.

[0144] In some examples, the isolation layer 14 is used to electrically isolate the air gap from the BAW resonator and provide structural support. The isolation layer 14 may be made of insulating materials such as SiO2, Si3N4, Al2O3, and combinations thereof. The thickness ranges from 1 nm to 100 μm.

[0145] In some examples, the second temperature drift compensation layer 22 is a thin film composed of a material having the property of thermal contraction and cold expansion. The optional materials include ZrW2O8, Zn2GeO4, HfW2O8, ZrMo2O8, HfMo2O8, ZrV2O7, HfV2O7, ZrV 1.7 Mo 0.3 O 7+δ 、ZrV 1.5 Mo 0.5 O 7+δ 、Cu2V2O7、Cu 2-x Zn x V2O7 (x is 0.1 or 0.2), Cu 2-y M y V2O7 (M is any one of Yb, Sm, Ce, y is 0.05), Cu 1.5 Mg 0.5 V2O7, Cu2P2O7, Cu2PVO7, HfMgW3O 12 、HfMgMo3O 12 、ZrMgMo3O 12 、ZrMgW3O 12 、ZrMnMo3O 12 、HfMnMo3O 12 、AScY2XO 12 (A is Zr or Hf, Y is W or Mo, X is V or P), TaVO5, NbVO5, Ag2O, Th2O(PO4)2, U2O(PO4)2, Zr2O(PO4)2, ScF3, CaZrF6, CaHfF6, MgZrF6, CaNbF6, CaTiF6, Zn(CN)2, Cd(CN)2, AgB(CN)4, CuB(CN)4, ScCo(CN)6, Si(NCN)2, Mn3AN(A=Zn,Ga), GdInO3, PbTiO3, PbVO3, PbVO 2.79 F 0.21 , PbV 1-xCr x O3、Bi 0.5 Na 0.5 VO3, GeTe, LaCu3Fe4O 12 , BiNiO3, V2OPO4, Ca2RuO4, Sr2IrO4, Sr2RhO4, Ca2MnO4, Ca2GeO4, Ca3Mn2O7, Ga3Ti2O7. The thickness of the first temperature drift compensation layer 21 ranges from 1nm to 100um.

[0146] In some examples, referring to FIG10 , a packaging layer 16 is provided on the side of the second temperature drift compensation layer 22 facing away from the substrate 10. The material of the packaging layer 16 is preferably an organic compound that can isolate water vapor and oxygen, such as polyimide, epoxy resin, etc., or an inorganic material such as SiN x , Al2O3, etc. The encapsulation layer 16 can be a single layer of a single material, or a stacked configuration of multiple materials.

[0147] Next, the preparation method of the BAW resonator in the fourth example is described. FIG11 is a flow chart of the preparation of the BAW resonator shown in FIG10 ; as shown in FIG11 , the preparation method specifically includes the following steps.

[0148] S41 , providing a base substrate 10 .

[0149] In some examples, taking the substrate 10 as an example of a single crystal silicon substrate, step S41 may specifically include: first, ultrasonically cleaning the single crystal silicon substrate with deionized water; then placing it in a H2SO4:H2O=3:1 mixed solution, heating it to 250°C and washing it for 15 minutes; then placing it in deionized water and ultrasonically cleaning it; then placing it in a NH4OH:H2O=1:6 mixed solution, heating it to 80°C and washing it for 15 minutes; taking it out and placing it in deionized water for rinsing; next, placing it in a HCl:H2O2:H2O=1:1:5 mixed solution, heating it to 85°C and washing it for 15 minutes, taking it out and placing it in a HF:H2O=1:20 dilute hydrofluoric acid and rinsing it for 10 seconds to remove the surface oxide layer; finally, placing it in deionized water for ultrasonic cleaning for 20 minutes, blow-drying it with an air knife, and completing the entire substrate 10 cleaning process.

[0150] S42 , forming a first groove portion 102 on the base substrate 10 .

[0151] In some examples, step S42 may specifically include: preparing a mask pattern on the base substrate 10, performing a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Then, performing an etching process to form the first groove 102. The etching process may be either wet etching or dry etching, with wet etching being preferred. Finally, performing a resist stripping process to complete the preparation of the first groove 102.

[0152] S43 , forming a sacrificial layer in the first groove 102 .

[0153] In some examples, the material of the sacrificial layer can be loose amorphous silicon dioxide doped with boron and phosphorus. Step S43 can specifically include forming a slurry containing loose silicon dioxide doped with boron and phosphorus using any of the processes selected from plasma enhanced chemical vapor deposition (PECVD), subatmospheric pressure chemical vapor deposition (SACVD), and screen printing, and then performing a thermal annealing at 700-900°C for 15-30 minutes in a vacuum chamber to liquefy and flow the loose amorphous silicon dioxide film doped with boron and phosphorus, completely filling the pores in the first groove 102 and leveling it, and then cooling and solidifying it. Finally, chemical mechanical polishing is performed, where the base substrate 10 is pressed against a rough polishing pad using a polishing head. Through the coupled effects of polishing liquid corrosion, particle friction, and polishing pad friction, the surface of the base substrate 10 is flattened over a certain period of time, and the surface of the material overflowing from the surface of the first groove 102 is polished to a height equivalent to that of the base substrate 10 surface.

[0154] S44 , forming an isolation layer 14 on the base substrate 10 .

[0155] In some examples, step S44 may specifically include: preparing an isolation layer 14 thin film on the substrate 10, first depositing an electrically insulating material, the deposition method of which may be radio frequency magnetron sputtering, pulsed laser sputtering (PLD), atomic layer deposition (ALD), or plasma chemical vapor deposition (PECVD). The isolation layer 14 is subjected to a photolithography process to form a pattern including the isolation layer 14, the photolithography process including coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably a wet etching process, but a dry etching process may also be selected.

[0156] S45 , forming a first electrode 11 on a side of the isolation layer 14 facing away from the base substrate 10 .

[0157] In some examples, when the first electrode 11 is made of a metal material, step S45 may include depositing a first metal film on the side of the first temperature drift compensation layer 21 away from the base substrate 10. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. A copper foil attachment method can also be used. Thereafter, the first metal film is subjected to a photolithography process, including glue coating (or glue spraying), pre-baking, exposure, development, and post-baking. Next, etching is performed to form a pattern including the first electrode 11. The etching process preferably adopts a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the first electrode 11.

[0158] S46 , forming a release hole 30 penetrating the first electrode 11 and the isolation layer 14 .

[0159] In some examples, step S46 may include performing a photolithography process on the side of the first electrode 11 facing away from the substrate 10, including resist coating (or spraying), pre-baking, exposure, development, and post-baking to expose the hole. A dry etching process is then performed to etch the first electrode 11. The etching gas is then changed to etch the isolation layer 14 until the sacrificial layer is reached. Finally, a resist stripping process is performed to form the release hole 30.

[0160] S47 , forming a piezoelectric layer 12 on a side of the first electrode 11 facing away from the base substrate 10 .

[0161] In some examples, taking the piezoelectric layer 12 as an example of an AlN single-layer structure, step S47 may include forming a piezoelectric material layer on the side of the first electrode 11 away from the substrate 10, and performing oriented growth of the piezoelectric material layer. The piezoelectric material layer is preferably formed by radio frequency magnetron sputtering (DC measurement and control sputtering is also possible). For AlN piezoelectric material, the target material is Al. By controlling the Ar and N2 gas pressures and temperatures during the deposition process and the post-annealing time and temperature, an AlN C-axis oriented piezoelectric material layer is formed, and the preferred growth orientation is (001). The deposition method of the piezoelectric material layer can also be selected from pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), etc. Next, the piezoelectric layer 12 is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Etching is then performed to form a pattern including the piezoelectric layer 12. A wet etching process is preferably used, but a dry etching process can also be used. Finally, a debonding process is performed to complete the preparation of the piezoelectric layer 12 .

[0162] S48 . Form a second electrode 13 on a side of the piezoelectric layer 12 facing away from the first electrode 11 .

[0163] In some examples, when the second electrode 13 is made of a metal material, step S48 may specifically include first depositing a second metal film on the side of the piezoelectric layer 12 away from the first electrode 11. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Next, the third metal film is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Thereafter, etching is performed to form a pattern including the second electrode 13. The etching process is preferably a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the second electrode 13.

[0164] S49 , forming a second temperature drift compensation layer 22 on a side of the second electrode 13 facing away from the base substrate 10 .

[0165] In some examples, step S49 may specifically include: first depositing a thin film of the second temperature drift compensation layer 22, preferably using radio frequency magnetron sputtering, but also including pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), sol-gel method (preparing a slurry containing the temperature drift compensation layer material and then heating and sintering it), thermal evaporation, electron beam evaporation, and the like. The temperature drift compensation layer thin film then undergoes a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably using a wet etching process, but also using a dry etching process, to form a pattern of the second temperature drift compensation layer 22.

[0166] S410 , removing the sacrificial layer.

[0167] In some examples, step S410 may include etching the sacrificial layer, preferably using a wet etching process. Immersion etching is performed using a mixture of hydrofluoric acid, dilute nitric acid, and deionized water (the etching temperature may be appropriately increased to increase the wet etching rate) for a sufficient period of time to ensure that the boron- and phosphorus-doped silicon dioxide filling material in the first groove portion 102 is completely dissolved. Finally, the first groove portion 102 is ultrasonically cleaned multiple times with deionized water and dried to form the first groove portion 102.

[0168] S411 , forming an encapsulation layer 16 on a side of the second electrode 13 facing away from the base substrate 10 .

[0169] In some examples, taking the encapsulation layer 16 as an example using an organic compound material, step S111 may specifically include first coating the organic material liquid, which may be done by spin coating, spraying, inkjet printing, transfer, etc., and then heating and curing to form a pattern of the encapsulation layer 16.

[0170] Of course, if multiple BAW resonators are prepared together, the preparation method provided in the embodiment of the present disclosure may further include a step of device cutting.

[0171] Fifth Example: Figure 12 is a schematic structural diagram of a BAW resonator according to the fifth example of the present disclosure. As shown in Figure 12, the BAW resonator includes a base substrate 10, an isolation layer 14, a first electrode 11, a piezoelectric layer 12, a second electrode 13, and a second temperature drift compensation layer 22 disposed on the base substrate 10. The second electrode 13 includes a third sub-electrode 131 and a fourth sub-electrode 132. In the BAW resonator, the isolation layer 14, the first electrode 11, the piezoelectric layer 12, the third sub-electrode 131, the second temperature drift compensation layer 22, and the fourth sub-electrode 132 are sequentially arranged in a direction away from the base substrate 10. The base substrate 10 has a first groove 102 extending through a portion of the base substrate 10 along its thickness, forming an air gap below the isolation layer 14. A release hole 30 extending through the first electrode 11 and the isolation layer 14 is used to release the sacrificial layer formed within the first groove 102 during the fabrication of the BAW resonator (details are described in detail in the fabrication method).

[0172] Continuing with Figure 12 , an RF signal enters the upper left corner of Figure 12 . It is then converted into an acoustic wave signal through the inverse piezoelectric effect at the interface between third sub-electrode 131 and piezoelectric layer 12. This acoustic wave propagates longitudinally through piezoelectric layer 12, and upon reaching the interface between first electrode 11 and piezoelectric layer 12, it is converted back into an RF signal through the piezoelectric effect and then transmitted outward. The air gap below the BAW resonator and the air layer above it act as acoustic reflectors, confining the acoustic signal within the resonator structure rather than dissipating it, thereby reducing the resonator's insertion loss. The second temperature-drift compensation layer 22 in the disclosed embodiment is different from general materials. The material of the second temperature-drift compensation layer 22 has the property of shrinking when heated and expanding when cooled. When the ambient temperature rises, the increase in the in-plane lattice constant of the piezoelectric layer 12 material connected to the second temperature-drift compensation layer 22 via the fourth sub-electrode 132 is suppressed. The degree of suppression can be adjusted by factors such as the selection of different types of temperature-drift compensation layer thin film materials and the thickness of the temperature-drift compensation layer. Therefore, the out-of-plane lattice constant of the piezoelectric layer 12 can decrease, increase, or remain unchanged as the ambient temperature increases. In other words, it can be flexibly adjusted, thereby obtaining a bulk acoustic wave resonator with a positive temperature coefficient, a negative temperature coefficient, or even a zero temperature coefficient.

[0173] In some examples, the material of the base substrate 10 is preferably glass, but Si, sapphire, SiC, GaAs, GaN, InP, BN, ZnO, etc. can also be selected. The thickness of the base substrate 10 ranges from 0.1 μm to 10 mm. The thickness of the air gap on the base substrate 10 ranges from 0.1 μm to 50 μm.

[0174] In some examples, the material of the first electrode 11 is a metal material, such as Mo. The materials of the first sub-electrode 111 and the second sub-electrode 112 can also be Cu, Al, Co, Ag, Ti, Pt, Ru, W, Au, or alloys formed by any combination of the above metals. The thickness of the first electrode 11, composed of the first sub-electrode 111 and the second sub-electrode 112, ranges from approximately 1 nm to 10 μm.

[0175] In some examples, the material of the piezoelectric layer 12 is preferably hBN, and cBN and wBN can also be selected. Of course, the material of the piezoelectric layer 12 can also be selected from AlN, ZnO, PZT, GaN, InN, CdS, CdSe, ZnS, CdTe, ZnTe, GaAs, GaSb, InAs, InSb, GaSe, GaP, AlP, quartz crystal, LiTaO3, LiNbO3, La3Ga5SiO14, BaTiO3, PbNb2O6, PBLN, LiGaO3, LiGeO3, TiGeO3, PbTiO3, PbZrO3, PVDF and other materials. The piezoelectric layer 12 in this embodiment can be one of the above-mentioned piezoelectric materials, or it can be a stack of the above-mentioned various piezoelectric materials. The thickness of the piezoelectric layer 12 ranges from 10nm to 100μm.

[0176] In some examples, the third sub-electrode 131 and the fourth sub-electrode 132 may be made of Cu, Al, Mo, Co, Ag, Ti, Pt, Ru, W, Au, or alloys thereof. The thickness of the second electrode 13 is in the range of 1 nm to 10 μm.

[0177] In some examples, the isolation layer 14 is used to electrically isolate the air gap from the BAW resonator and provide structural support. The isolation layer 14 may be made of insulating materials such as SiO2, Si3N4, Al2O3, and combinations thereof. The thickness ranges from 1 nm to 100 μm.

[0178] In some examples, the second temperature drift compensation layer 22 is a thin film composed of a material having the property of thermal contraction and cold expansion. The optional materials include ZrW2O8, Zn2GeO4, HfW2O8, ZrMo2O8, HfMo2O8, ZrV2O7, HfV2O7, ZrV 1.7 Mo 0.3 O 7+δ 、ZrV 1.5 Mo 0.5 O 7+δ 、Cu2V2O7、Cu 2-x Zn x V2O7 (x is 0.1 or 0.2), Cu 2-yM y V2O7 (M is any one of Yb, Sm, Ce, y is 0.05), Cu 1.5 Mg 0.5 V2O7, Cu2P2O7, Cu2PVO7, HfMgW3O 12 、HfMgMo3O 12 、ZrMgMo3O 12 、ZrMgW3O 12 、ZrMnMo3O 12 、HfMnMo3O 12 、AScY2XO 12 (A is Zr or Hf, Y is W or Mo, X is V or P), TaVO5, NbVO5, Ag2O, Th2O(PO4)2, U2O(PO4)2, Zr2O(PO4)2, ScF3, CaZrF6, CaHfF6, MgZrF6, CaNbF6, CaTiF6, Zn(CN)2, Cd(CN)2, AgB(CN)4, CuB(CN)4, ScCo(CN)6, Si(NCN)2, Mn3AN(A=Zn,Ga), GdInO3, PbTiO3, PbVO3, PbVO 2.79 F 0.21 , PbV 1-x Cr x O3、Bi 0.5 Na 0.5 VO3, GeTe, LaCu3Fe4O 12 , BiNiO3, V2OPO4, Ca2RuO4, Sr2IrO4, Sr2RhO4, Ca2MnO4, Ca2GeO4, Ca3Mn2O7, Ga3Ti2O7. The thickness of the second temperature drift compensation layer 22 ranges from 1nm to 100um.

[0179] In some examples, referring to FIG12 , an encapsulation layer 16 is provided on the side of the second electrode 13 facing away from the substrate 10. The material of the encapsulation layer 16 is preferably an organic compound that can isolate water vapor and oxygen, such as polyimide, epoxy resin, etc., or an inorganic material such as SiN x , Al2O3, etc. The encapsulation layer 16 can be a single layer of a single material, or a stacked configuration of multiple materials.

[0180] Next, the preparation method of the BAW resonator in the fifth example is described. FIG13 is a flow chart of the preparation of the BAW resonator shown in FIG12. As shown in FIG13, the preparation method specifically includes the following steps.

[0181] S51 , providing a base substrate 10 .

[0182] In some examples, taking the substrate 10 as an example of a single crystal silicon substrate, step S51 may specifically include: first, ultrasonically cleaning the single crystal silicon substrate with deionized water; then placing it in a H2SO4:H2O=3:1 mixed solution, heating it to 250°C and washing it for 15 minutes; then placing it in deionized water and ultrasonically cleaning it; then placing it in a NH4OH:H2O=1:6 mixed solution, heating it to 80°C and washing it for 15 minutes; taking it out and placing it in deionized water for rinsing; next, placing it in a HCl:H2O2:H2O=1:1:5 mixed solution, heating it to 85°C and washing it for 15 minutes, taking it out and placing it in a HF:H2O=1:20 dilute hydrofluoric acid and rinsing it for 10 seconds to remove the surface oxide layer; finally, placing it in deionized water for ultrasonic cleaning for 20 minutes, blow-drying it with an air knife, and completing the entire substrate 10 cleaning process.

[0183] S52 , forming a first groove portion 102 on the base substrate 10 .

[0184] In some examples, step S52 may specifically include: preparing a mask pattern on the base substrate 10, performing a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Then, performing an etching process to form the first groove 102. The etching process may be either wet etching or dry etching, with wet etching being preferred. Finally, performing a resist stripping process to complete the preparation of the first groove 102.

[0185] S53 , forming a sacrificial layer in the first groove 102 .

[0186] In some examples, the sacrificial layer can be made of loose amorphous silicon dioxide doped with boron and phosphorus. Step S53 can specifically include forming a slurry containing loose silicon dioxide doped with boron and phosphorus using any of the processes selected from plasma enhanced chemical vapor deposition (PECVD), subatmospheric pressure chemical vapor deposition (SACVD), and screen printing, followed by thermal annealing at 700-900°C for 15-30 minutes in a vacuum chamber to liquefy and flow the loose amorphous silicon dioxide film doped with boron and phosphorus, completely filling the pores in the first groove 102 and leveling it, and then cooling and solidifying it. Finally, chemical mechanical polishing is performed, where a polishing head is used to press the substrate 10 against a rough polishing pad. The surface of the substrate 10 is flattened over a period of time by the coupled effects of polishing liquid corrosion, particle friction, and polishing pad friction, and the material overflowing from the surface of the first groove 102 is polished to a height equivalent to that of the substrate 10 surface.

[0187] S54 , forming an isolation layer 14 on the base substrate 10 .

[0188] In some examples, step S54 may specifically include: preparing an isolation layer 14 thin film on the substrate 10, first depositing an electrically insulating material, wherein the deposition method may be radio frequency magnetron sputtering, pulsed laser sputtering (PLD), atomic layer deposition (ALD), or plasma chemical vapor deposition (PECVD). The isolation layer 14 is subjected to a photolithography process to form a pattern including the isolation layer 14, wherein the photolithography process includes coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably a wet etching process, but a dry etching process may also be selected.

[0189] S55 , forming a first electrode 11 on a side of the isolation layer 14 facing away from the base substrate 10 .

[0190] In some examples, when the first electrode 11 is made of a metal material, step S55 may include depositing a first metal film on the side of the first temperature drift compensation layer 21 facing away from the base substrate 10. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Copper foil can also be attached. Thereafter, the first metal film is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Next, etching is performed to form a pattern including the first electrode 11. The etching process preferably uses a wet etching process, but a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the first electrode 11.

[0191] S56 , forming a release hole 30 penetrating the first electrode 11 and the isolation layer 14 .

[0192] In some examples, step S56 may include performing a photolithography process on the side of the first electrode 11 facing away from the substrate 10, including resist coating (or spraying), pre-baking, exposure, development, and post-baking to expose the hole. A dry etching process is then performed to etch the first electrode 11. The etching gas is then changed to etch the isolation layer 14 until the sacrificial layer is reached. Finally, a resist stripping process is performed to form the release hole 30.

[0193] S57 , forming a piezoelectric layer 12 on a side of the first electrode 11 facing away from the base substrate 10 .

[0194] In some examples, taking the piezoelectric layer 12 as an example of an AlN single-layer structure, step S57 may include forming a piezoelectric material layer on the side of the first electrode 11 away from the substrate 10, and performing oriented growth of the piezoelectric material layer. The piezoelectric material layer is preferably formed by radio frequency magnetron sputtering (DC measurement and control sputtering is also possible). For AlN piezoelectric material, the target material is Al. By controlling the Ar and N2 gas pressures and temperatures during the deposition process and the post-annealing time and temperature, an AlN C-axis oriented piezoelectric material layer is formed, and the preferred growth orientation is (001). The deposition method of the piezoelectric material layer can also be selected from pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), etc. Next, the piezoelectric layer 12 is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Etching is then performed to form a pattern including the piezoelectric layer 12. A wet etching process is preferably used, but a dry etching process can also be used. Finally, a debonding process is performed to complete the preparation of the piezoelectric layer 12 .

[0195] S58 . Form a third sub-electrode 131 on a side of the piezoelectric layer 12 facing away from the first electrode 11 .

[0196] In some examples, when the third sub-electrode 131 is made of a metal material, step S58 may specifically include first depositing a second metal film on the side of the piezoelectric layer 12 facing away from the first electrode 11. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Next, the third metal film is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Thereafter, etching is performed to form a pattern including the third sub-electrode 131. The etching process is preferably a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the third sub-electrode 131.

[0197] S59 , forming a second temperature drift compensation layer 22 on a side of the third sub-electrode 131 facing away from the base substrate 10 .

[0198] In some examples, step S59 may specifically include: first depositing a thin film of the second temperature drift compensation layer 22, preferably using radio frequency magnetron sputtering, but also including pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), sol-gel method (preparing a slurry containing the temperature drift compensation layer material and then heating and sintering it), thermal evaporation, electron beam evaporation, and the like. The temperature drift compensation layer thin film then undergoes a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably using a wet etching process, but also using a dry etching process, to form a pattern of the second temperature drift compensation layer 22.

[0199] S510 , forming a fourth sub-electrode 132 on a side of the second temperature drift compensation layer 22 away from the third sub-electrode 131 .

[0200] In some examples, when the fourth sub-electrode 132 is made of a metal material, step S510 may specifically include first depositing a third metal film on the side of the piezoelectric layer 12 facing away from the first electrode 11. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Next, the third metal film is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Thereafter, etching is performed to form a pattern including the fourth sub-electrode 132. The etching process is preferably a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the fourth sub-electrode 132.

[0201] S511 , removing the sacrificial layer.

[0202] In some examples, step S511 may include etching the sacrificial layer, preferably using a wet etching process. Immersion etching is performed using a mixture of hydrofluoric acid, dilute nitric acid, and deionized water (the etching temperature may be appropriately increased to increase the wet etching rate) for a sufficient period of time to ensure that the boron- and phosphorus-doped silicon dioxide filling material in the first groove portion 102 is completely dissolved. Finally, the first groove portion 102 is ultrasonically cleaned multiple times with deionized water and dried to form the first groove portion 102.

[0203] S512 , forming an encapsulation layer 16 on a side of the fourth sub-electrode 132 facing away from the base substrate 10 .

[0204] In some examples, taking the encapsulation layer 16 as an example using an organic compound material, step S512 may specifically include first coating the organic material liquid, which may be done by spin coating, spraying, inkjet printing, transfer, etc., and then heating and curing to form a pattern of the encapsulation layer 16.

[0205] Of course, if multiple BAW resonators are prepared together, the preparation method provided in the embodiment of the present disclosure may further include a step of device cutting.

[0206] Sixth Example: FIG14 is a schematic diagram of the structure of a BAW resonator according to the sixth example of the present disclosure. As shown in FIG14 , the structure of the BAW resonator according to this example is substantially the same as that of the BAW resonator according to the fifth example, with the only difference being that, in this example, the second temperature drift compensation layer 22 has a hollow pattern and a through hole extending through the second temperature drift compensation layer 22 along its thickness. In this case, the third sub-electrode 131 and the fourth sub-electrode 132 of the second electrode 13 can be electrically connected via the through hole extending through the second temperature drift compensation layer 22, thereby reducing the resistance of the second electrode 13 and, in turn, the in-band insertion loss of the BAW resonator. The remaining structures in this BAW resonator can adopt the same structures as those in the fifth example, so they will not be described in detail here.

[0207] The preparation method of the bulk acoustic wave resonator in the sixth example can be prepared by the same method as in the fifth example. The only difference from the fifth example is that when forming the second temperature drift compensation layer 22, a through hole is formed along its thickness direction, that is, a hollow pattern is formed. The remaining steps are the same as those in the fifth example, so they will not be repeated here.

[0208] Seventh example: FIG15 is a schematic structural diagram of a BAW resonator of the seventh example implemented in the present disclosure; as shown in FIG15 , the BAW resonator includes a base substrate 10, an isolation layer 14, a first temperature drift compensation layer 21, a first electrode 11, a piezoelectric layer 12, a second electrode 13, and a second temperature drift compensation layer 22 sequentially arranged on the base substrate 10. The base substrate 10 has a first groove 102 that penetrates a portion of the base substrate 10 along its thickness direction, i.e., an air gap is formed under the isolation layer 14. The release hole 30 that penetrates the first electrode 11, the first temperature drift compensation layer 21, and the isolation layer 14 is used to release the sacrificial layer formed in the first groove 102 during the preparation of the BAW resonator (detailed description is provided in the preparation method).

[0209] Continuing with Figure 15 , an RF signal enters from the upper left corner of Figure 15 . It is then converted into an acoustic wave signal through the inverse piezoelectric effect at the interface between second electrode 13 and piezoelectric layer 12. This acoustic wave propagates longitudinally through piezoelectric layer 12, and upon reaching the interface between first electrode 11 and piezoelectric layer 12, it is converted back into an RF signal through the piezoelectric effect and then transmitted outward. The air gap below the BAW resonator and the air layer above it act as acoustic reflectors, confining the acoustic signal within the resonator structure rather than dissipating it, thereby reducing the resonator's insertion loss. The first temperature-drift compensation layer 21 in the disclosed embodiment is different from general materials. Its temperature-drift compensation layer material has the property of thermal contraction and thermal expansion. When the ambient temperature rises, the increase in the in-plane lattice constant of the piezoelectric layer 12 material connected to the first temperature-drift compensation layer 21 via the first electrode 11 and to the second temperature-drift compensation layer 22 via the second electrode 13 is suppressed. The degree of suppression can be adjusted by factors such as the selection of different types of temperature-drift compensation layer thin film materials and the thickness of the temperature-drift compensation layers. Therefore, the out-of-plane lattice constant of the piezoelectric layer 12 can decrease, increase, or remain unchanged as the ambient temperature rises. In other words, it can be flexibly adjusted, thereby obtaining a bulk acoustic wave resonator with a positive temperature coefficient, a negative temperature coefficient, or even a zero temperature coefficient.

[0210] In some examples, the material of the base substrate 10 is preferably glass, but Si, sapphire, SiC, GaAs, GaN, InP, BN, ZnO, etc. can also be selected. The thickness of the base substrate 10 ranges from 0.1 μm to 10 mm. The thickness of the air gap on the base substrate 10 ranges from 0.1 μm to 50 μm.

[0211] In some examples, the first electrode 11 is made of a metal material, such as Mo. Alternatively, the first electrode 11 may be made of Cu, Al, Co, Ag, Ti, Pt, Ru, W, or Au, or an alloy formed by any combination of the above metals. The thickness of the first electrode 11 ranges from about 1 nm to about 10 μm.

[0212] In some examples, the material of the piezoelectric layer 12 is preferably hBN, and cBN and wBN can also be selected. Of course, the material of the piezoelectric layer 12 can also be selected from AlN, ZnO, PZT, GaN, InN, CdS, CdSe, ZnS, CdTe, ZnTe, GaAs, GaSb, InAs, InSb, GaSe, GaP, AlP, quartz crystal, LiTaO3, LiNbO3, La3Ga5SiO14, BaTiO3, PbNb2O6, PBLN, LiGaO3, LiGeO3, TiGeO3, PbTiO3, PbZrO3, PVDF and other materials. The piezoelectric layer 12 in this embodiment can be one of the above-mentioned piezoelectric materials, or it can be a stack of the above-mentioned various piezoelectric materials. The thickness of the piezoelectric layer 12 ranges from 10nm to 100μm.

[0213] In some examples, the second electrode 13 may be made of Cu, Al, Mo, Co, Ag, Ti, Pt, Ru, W, or Au, or may be an alloy of the above metals. The thickness of the second electrode 13 ranges from 1 nm to 10 μm.

[0214] In some examples, the isolation layer 14 is used to electrically isolate the air gap from the BAW resonator and provide structural support. The isolation layer 14 may be made of insulating materials such as SiO2, Si3N4, Al2O3, and combinations thereof. The thickness ranges from 1 nm to 100 μm.

[0215] In some examples, the first temperature drift compensation layer 21 and the second temperature drift compensation layer 22 are both thin films made of materials with thermal contraction and cold expansion properties. The materials that can be selected include ZrW2O8, Zn2GeO4, HfW2O8, ZrMo2O8, HfMo2O8, ZrV2O7, HfV2O7, ZrV 1.7 Mo 0.3 O 7+δ 、ZrV 1.5 Mo 0.5 O 7+δ 、Cu2V2O7、Cu 2-x Zn x V2O7 (x is 0.1 or 0.2), Cu 2-y M y V2O7 (M is any one of Yb, Sm, Ce, y is 0.05), Cu 1.5 Mg 0.5 V2O7, Cu2P2O7, Cu2PVO7, HfMgW3O 12 、HfMgMo3O 12 、ZrMgMo3O 12 、ZrMgW3O 12 、ZrMnMo3O 12 、HfMnMo3O 12 、AScY2XO 12 (A is Zr or Hf, Y is W or Mo, X is V or P), TaVO5, NbVO5, Ag2O, Th2O(PO4)2, U2O(PO4)2, Zr2O(PO4)2, ScF3, CaZrF6, CaHfF6, MgZrF6, CaNbF6, CaTiF6, Zn(CN)2, Cd(CN)2, AgB(CN)4, CuB(CN)4, ScCo(CN)6, Si(NCN)2, Mn3AN(A=Zn,Ga), GdInO3, PbTiO3, PbVO3, PbVO2.79 F 0.21 , PbV 1-x Cr x O3、Bi 0.5 Na 0.5 VO3, GeTe, LaCu3Fe4O 12 , BiNiO3, V2OPO4, Ca2RuO4, Sr2IrO4, Sr2RhO4, Ca2MnO4, Ca2GeO4, Ca3Mn2O7, Ga3Ti2O7. The thickness of the first temperature drift compensation layer 21 and the second temperature drift compensation layer 22 are both in the range of 1nm to 100um.

[0216] In some examples, referring to FIG15 , a packaging layer 16 is provided on the side of the second temperature drift compensation layer 22 facing away from the substrate 10. The material of the packaging layer 16 is preferably an organic compound that can isolate water vapor and oxygen, such as polyimide, epoxy resin, etc., or an inorganic material such as SiN x , Al2O3, etc. The encapsulation layer 16 can be a single layer of a single material, or a stacked configuration of multiple materials.

[0217] Next, the preparation method of the BAW resonator in the seventh example is described. FIG16 is a flow chart of the preparation of the BAW resonator shown in FIG15. As shown in FIG16, the preparation method specifically includes the following steps.

[0218] S71 , providing a base substrate 10 .

[0219] In some examples, taking the substrate 10 as an example of a single crystal silicon substrate, step S71 may specifically include: first, ultrasonically cleaning the single crystal silicon substrate with deionized water; then placing it in a H2SO4:H2O=3:1 mixed solution, heating it to 250°C and washing it for 15 minutes; then placing it in deionized water and ultrasonically cleaning it; then placing it in a NH4OH:H2O=1:6 mixed solution, heating it to 80°C and washing it for 15 minutes; taking it out and placing it in deionized water for rinsing; next, placing it in a HCl:H2O2:H2O=1:1:5 mixed solution, heating it to 85°C and washing it for 15 minutes, taking it out and placing it in a HF:H2O=1:20 dilute hydrofluoric acid and rinsing it for 10 seconds to remove the surface oxide layer; finally, placing it in deionized water for ultrasonic cleaning for 20 minutes, blow-drying it with an air knife, and completing the entire substrate 10 cleaning process.

[0220] S72 , forming a first groove portion 102 on the base substrate 10 .

[0221] In some examples, step S72 may specifically include: preparing a mask pattern on the base substrate 10, performing a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Then, performing an etching process to form the first groove 102. The etching process may be either wet etching or dry etching, with wet etching being preferred. Finally, performing a resist stripping process to complete the preparation of the first groove 102.

[0222] S73 , forming a sacrificial layer in the first groove 102 .

[0223] In some examples, the sacrificial layer can be made of loose amorphous silicon dioxide doped with boron and phosphorus. Step S73 can specifically include forming a slurry containing loose silicon dioxide doped with boron and phosphorus using any of the processes selected from plasma enhanced chemical vapor deposition (PECVD), subatmospheric pressure chemical vapor deposition (SACVD), and screen printing, followed by thermal annealing at 700-900°C for 15-30 minutes in a vacuum chamber. This slurry is used to liquefy and flow the loose amorphous silicon dioxide film doped with boron and phosphorus, completely filling the pores in the first groove 102 and leveling the surface, and then cooling and solidifying the film. Finally, chemical mechanical polishing is performed, where a polishing head is used to press the substrate 10 against a rough polishing pad. The surface of the substrate 10 is flattened over a period of time by the coupled effects of polishing liquid corrosion, particle friction, and polishing pad friction. The material overflowing from the surface of the first groove 102 is polished to a height equivalent to that of the substrate 10 surface.

[0224] S74 , forming an isolation layer 14 on the base substrate 10 .

[0225] In some examples, step S74 may specifically include: preparing an isolation layer 14 thin film on the substrate 10, first depositing an electrically insulating material, the deposition method of which may be radio frequency magnetron sputtering, pulsed laser sputtering (PLD), atomic layer deposition (ALD), or plasma chemical vapor deposition (PECVD). The isolation layer 14 is subjected to a photolithography process to form a pattern including the isolation layer 14, the photolithography process including coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably a wet etching process, but a dry etching process may also be selected.

[0226] S75 , forming a first temperature drift compensation layer 21 on a side of the isolation layer 14 facing away from the base substrate 10 .

[0227] In some examples, step S75 may specifically include: first depositing a thin film of the first temperature drift compensation layer 21, preferably using radio frequency magnetron sputtering, but also alternative methods include pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), sol-gel method (preparing a slurry containing the temperature drift compensation layer material and then heating and sintering it), thermal evaporation, electron beam evaporation, etc. The temperature drift compensation layer thin film then undergoes a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably using a wet etching process, but also using a dry etching process, to form a pattern of the first temperature drift compensation layer 21.

[0228] S76 , forming a first electrode 11 on a side of the first temperature drift compensation layer 21 facing away from the base substrate 10 .

[0229] In some examples, when the first electrode 11 is made of a metal material, step S76 may include depositing a first metal film on the side of the first temperature drift compensation layer 21 facing away from the base substrate 10. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. A copper foil attachment method can also be used. Thereafter, the first metal film is subjected to a photolithography process, including glue coating (or glue spraying), pre-baking, exposure, development, and post-baking. Next, etching is performed to form a pattern including the first electrode 11. The etching process preferably adopts a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the first electrode 11.

[0230] S77 , forming a release hole 30 penetrating the first electrode 11 , the isolation layer 14 and the first temperature drift compensation layer 21 .

[0231] In some examples, step S77 may include performing a photolithography process on the side of the first electrode 11 facing away from the substrate 10, including resist coating (or spraying), pre-baking, exposure, development, and post-baking to expose the hole. A dry etching process is then performed to etch the first electrode 11. The etching gas is then changed to etch the first temperature drift compensation layer 21. Finally, the etching gas is changed to etch the isolation layer 14 until the sacrificial layer is etched. Finally, a resist stripping process is performed to form the release hole 30.

[0232] S78 , forming a piezoelectric layer 12 on a side of the first electrode 11 facing away from the base substrate 10 .

[0233] In some examples, taking the piezoelectric layer 12 as an example of an AlN single-layer structure, step S78 may include forming a piezoelectric material layer on the side of the first electrode 11 away from the substrate 10, and performing oriented growth of the piezoelectric material layer. The piezoelectric material layer is preferably formed by radio frequency magnetron sputtering (DC measurement and control sputtering is also possible). For AlN piezoelectric material, the target material is Al. By controlling the Ar and N2 gas pressures and temperatures during the deposition process and the post-annealing time and temperature, an AlN C-axis oriented piezoelectric material layer is formed, and the preferred growth orientation is (001). The deposition method of the piezoelectric material layer can also be selected from pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), etc. Next, the piezoelectric layer 12 is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Etching is then performed to form a pattern including the piezoelectric layer 12. A wet etching process is preferably used, but a dry etching process can also be used. Finally, a debonding process is performed to complete the preparation of the piezoelectric layer 12 .

[0234] S79 . Form a second electrode 13 on a side of the piezoelectric layer 12 facing away from the first electrode 11 .

[0235] In some examples, when the second electrode 13 is made of a metal material, step S79 may specifically include first depositing a third metal film on the side of the piezoelectric layer 12 away from the first electrode 11. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Next, the third metal film is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Thereafter, etching is performed to form a pattern including the second electrode 13. The etching process is preferably a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the second electrode 13.

[0236] S710 , forming a second temperature drift compensation layer 22 on a side of the second electrode 13 facing away from the base substrate 10 .

[0237] In some examples, step S710 may specifically include: first depositing a thin film of the second temperature drift compensation layer 22, preferably using radio frequency magnetron sputtering, but also alternatively using pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), sol-gel method (preparing a slurry containing the temperature drift compensation layer material and then heating and sintering it), thermal evaporation, electron beam evaporation, and the like. The temperature drift compensation layer thin film then undergoes a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably using a wet etching process, but also using a dry etching process, to form a pattern of the second temperature drift compensation layer 22.

[0238] S711 , removing the sacrificial layer.

[0239] In some examples, step S711 may include etching the sacrificial layer, preferably using a wet etching process. Immersion etching is performed using a mixture of hydrofluoric acid, dilute nitric acid, and deionized water (the etching temperature may be appropriately increased to increase the wet etching rate) for a sufficient period of time to ensure that the boron- and phosphorus-doped silicon dioxide filling material in the first groove portion 102 is completely dissolved. Finally, the first groove portion 102 is ultrasonically cleaned multiple times with deionized water and dried to form the first groove portion 102.

[0240] S712 , forming an encapsulation layer 16 on a side of the second electrode 13 facing away from the base substrate 10 .

[0241] In some examples, taking the encapsulation layer 16 as an example using an organic compound material, step S712 may specifically include first coating the organic material liquid, which may be done by spin coating, spraying, inkjet printing, transfer, etc., and then heating and curing to form a pattern of the encapsulation layer 16.

[0242] Of course, if multiple BAW resonators are prepared together, the preparation method provided in the embodiment of the present disclosure may further include a step of device cutting.

[0243] Example 8: FIG17 is a schematic structural diagram of a BAW resonator according to the eighth example of the present disclosure. As shown in FIG17 , the BAW resonator includes a base substrate 10, an isolation layer 14, a first temperature drift compensation layer 21, a first electrode 11, a piezoelectric layer 12, a second electrode 13, and a second temperature drift compensation layer 22 disposed on the base substrate 10. The second electrode 13 includes a third sub-electrode 131 and a fourth sub-electrode 132. In the BAW resonator, the isolation layer 14, the first temperature drift compensation layer 21, the first electrode 11, the piezoelectric layer 12, the third sub-electrode 131, the second temperature drift compensation layer 22, and the fourth sub-electrode 132 are sequentially disposed in a direction away from the base substrate 10. The base substrate 10 has a first groove 102 extending through a portion of the base substrate 10 along its thickness, forming an air gap below the isolation layer 14. The release hole 30 penetrating the first electrode 11 and the isolation layer 14 is used to release the sacrificial layer formed in the first groove 102 during the process of manufacturing the BAW resonator (detailed description will be given in the manufacturing method).

[0244] Continuing with Figure 17 , an RF signal enters from the upper left corner of Figure 17 . It is then converted into an acoustic wave signal through the inverse piezoelectric effect at the interface between third sub-electrode 131 and piezoelectric layer 12. This acoustic wave propagates longitudinally through piezoelectric layer 12, and upon reaching the interface between first electrode 11 and piezoelectric layer 12, it is converted back into an RF signal through the piezoelectric effect and then transmitted outward. The air gap below the BAW resonator and the air layer above it act as acoustic reflectors, confining the acoustic signal within the resonator structure rather than dissipating it, thereby reducing the resonator's insertion loss. The second temperature-drift compensation layer 22 in the disclosed embodiment is different from general materials. The materials of the first temperature-drift compensation layer 21 and the second temperature-drift compensation layer 22 have the property of shrinking when heated and expanding when cooled. When the ambient temperature rises, the increase in the in-plane lattice constant of the piezoelectric layer 12 material connected to the first temperature-drift compensation layer 21 via the first electrode 11 and to the second temperature-drift compensation layer 22 via the fourth sub-electrode 132 is suppressed. The degree of suppression can be adjusted by factors such as the selection of different types of temperature-drift compensation layer thin film materials and the thickness of the temperature-drift compensation layers. Therefore, the out-of-plane lattice constant of the piezoelectric layer 12 can decrease, increase, or remain unchanged as the ambient temperature increases. In other words, it can be flexibly adjusted, thereby obtaining a bulk acoustic wave resonator with a positive temperature coefficient, a negative temperature coefficient, or even a zero temperature coefficient.

[0245] In some examples, the material of the base substrate 10 is preferably glass, but Si, sapphire, SiC, GaAs, GaN, InP, BN, ZnO, etc. can also be selected. The thickness of the base substrate 10 ranges from 0.1 μm to 10 mm. The thickness of the air gap on the base substrate 10 ranges from 0.1 μm to 50 μm.

[0246] In some examples, the material of the first electrode 11 is a metal material, such as Mo. The materials of the first sub-electrode 111 and the second sub-electrode 112 can also be Cu, Al, Co, Ag, Ti, Pt, Ru, W, Au, or alloys formed by any combination of the above metals. The thickness of the first electrode 11, composed of the first sub-electrode 111 and the second sub-electrode 112, ranges from approximately 1 nm to 10 μm.

[0247] In some examples, the material of the piezoelectric layer 12 is preferably hBN, and cBN and wBN can also be selected. Of course, the material of the piezoelectric layer 12 can also be selected from AlN, ZnO, PZT, GaN, InN, CdS, CdSe, ZnS, CdTe, ZnTe, GaAs, GaSb, InAs, InSb, GaSe, GaP, AlP, quartz crystal, LiTaO3, LiNbO3, La3Ga5SiO14, BaTiO3, PbNb2O6, PBLN, LiGaO3, LiGeO3, TiGeO3, PbTiO3, PbZrO3, PVDF and other materials. The piezoelectric layer 12 in this embodiment can be one of the above-mentioned piezoelectric materials, or it can be a stack of the above-mentioned various piezoelectric materials. The thickness of the piezoelectric layer 12 ranges from 10nm to 100μm.

[0248] In some examples, the third sub-electrode 131 and the fourth sub-electrode 132 may be made of Cu, Al, Mo, Co, Ag, Ti, Pt, Ru, W, Au, or alloys thereof. The thickness of the second electrode 13 is in the range of 1 nm to 10 μm.

[0249] In some examples, the isolation layer 14 is used to electrically isolate the air gap from the BAW resonator and provide structural support. The isolation layer 14 may be made of insulating materials such as SiO2, Si3N4, Al2O3, and combinations thereof. The thickness ranges from 1 nm to 100 μm.

[0250] In some examples, the first temperature drift compensation layer 21 and the second temperature drift compensation layer 22 are thin films made of materials with thermal contraction and cold expansion properties. The materials that can be selected include ZrW2O8, Zn2GeO4, HfW2O8, ZrMo2O8, HfMo2O8, ZrV2O7, HfV2O7, ZrV 1.7 Mo 0.3 O 7+δ 、ZrV 1.5 Mo 0.5 O 7+δ 、Cu2V2O7、Cu 2-x Zn x V2O7 (x is 0.1 or 0.2), Cu2-y M y V2O7 (M is any one of Yb, Sm, Ce, y is 0.05), Cu 1.5 Mg 0.5 V2O7, Cu2P2O7, Cu2PVO7, HfMgW3O 12 、HfMgMo3O 12 、ZrMgMo3O 12 、ZrMgW3O 12 、ZrMnMo3O 12 、HfMnMo3O 12 、AScY2XO 12 (A is Zr or Hf, Y is W or Mo, X is V or P), TaVO5, NbVO5, Ag2O, Th2O(PO4)2, U2O(PO4)2, Zr2O(PO4)2, ScF3, CaZrF6, CaHfF6, MgZrF6, CaNbF6, CaTiF6, Zn(CN)2, Cd(CN)2, AgB(CN)4, CuB(CN)4, ScCo(CN)6, Si(NCN)2, Mn3AN(A=Zn,Ga), GdInO3, PbTiO3, PbVO3, PbVO 2.79 F 0.21 , PbV 1-x Cr x O3、Bi 0.5 Na 0.5 VO3, GeTe, LaCu3Fe4O 12 , BiNiO3, V2OPO4, Ca2RuO4, Sr2IrO4, Sr2RhO4, Ca2MnO4, Ca2GeO4, Ca3Mn2O7, Ga3Ti2O7. The thickness of the first temperature drift compensation layer 21 and the second temperature drift compensation layer 22 are both in the range of 1nm to 100um.

[0251] In some examples, referring to FIG17 , an encapsulation layer 16 is provided on the side of the second electrode 13 facing away from the substrate 10. The material of the encapsulation layer 16 is preferably an organic compound that can isolate water vapor and oxygen, such as polyimide, epoxy resin, etc., or an inorganic material such as SiN x , Al2O3, etc. The encapsulation layer 16 can be a single layer of a single material, or a stacked configuration of multiple materials.

[0252] Next, the preparation method of the BAW resonator in the eighth example is described. FIG18 is a flow chart of the preparation of the BAW resonator shown in FIG17 ; as shown in FIG18 , the preparation method specifically includes the following steps.

[0253] S81, providing a base substrate 10.

[0254] In some examples, taking the substrate 10 as an example of a single crystal silicon substrate, step S81 may specifically include: first, ultrasonically cleaning the single crystal silicon substrate with deionized water; then placing it in a H2SO4:H2O=3:1 mixed solution, heating it to 250°C and washing it for 15 minutes; then placing it in deionized water and ultrasonically cleaning it; then placing it in a NH4OH:H2O=1:6 mixed solution, heating it to 80°C and washing it for 15 minutes; taking it out and placing it in deionized water for rinsing; next, placing it in a HCl:H2O2:H2O=1:1:5 mixed solution, heating it to 85°C and washing it for 15 minutes, taking it out and placing it in a HF:H2O=1:20 dilute hydrofluoric acid and rinsing it for 10 seconds to remove the surface oxide layer; finally, placing it in deionized water for ultrasonic cleaning for 20 minutes, blow-drying it with an air knife, and completing the entire substrate 10 cleaning process.

[0255] S82 , forming a first groove portion 102 on the base substrate 10 .

[0256] In some examples, step S82 may specifically include: preparing a mask pattern on the base substrate 10, performing a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Then, performing an etching process to form the first groove 102. The etching process may be either wet etching or dry etching, with wet etching being preferred. Finally, performing a resist stripping process to complete the preparation of the first groove 102.

[0257] S83 , forming a sacrificial layer in the first groove 102 .

[0258] In some examples, the sacrificial layer can be made of loose amorphous silicon dioxide doped with boron and phosphorus. Step S83 can specifically include forming a slurry containing loose silicon dioxide doped with boron and phosphorus using any of the processes selected from plasma enhanced chemical vapor deposition (PECVD), subatmospheric pressure chemical vapor deposition (SACVD), and screen printing. The slurry is then thermally annealed at 700-900°C for 15-30 minutes in a vacuum chamber to liquefy and flow the loose amorphous silicon dioxide film doped with boron and phosphorus, completely filling the pores in the first groove 102 and leveling the pores. The slurry is then cooled and solidified. Finally, chemical mechanical polishing is performed, where a polishing head is used to press the substrate 10 against a rough polishing pad. The surface of the substrate 10 is flattened over a period of time by the coupled effects of polishing liquid corrosion, particle friction, and polishing pad friction. The material overflowing from the surface of the first groove 102 is polished to a height equivalent to that of the substrate 10 surface.

[0259] S84 , forming an isolation layer 14 on the base substrate 10 .

[0260] In some examples, step S84 may specifically include: preparing an isolation layer 14 thin film on the substrate 10, first depositing an electrically insulating material, where the deposition method may be radio frequency magnetron sputtering, pulsed laser sputtering (PLD), atomic layer deposition (ALD), or plasma chemical vapor deposition (PECVD). The isolation layer 14 is subjected to a photolithography process to form a pattern including the isolation layer 14, where the photolithography process includes coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably a wet etching process, but a dry etching process may also be selected.

[0261] S55 , forming a first temperature drift compensation layer 21 on a side of the isolation layer 14 facing away from the base substrate 10 .

[0262] In some examples, step S55 may specifically include: first depositing a thin film of the first temperature drift compensation layer 21, preferably using radio frequency magnetron sputtering; alternative deposition methods include pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), sol-gel method (preparing a slurry containing the temperature drift compensation layer material followed by heating and sintering), thermal evaporation, electron beam evaporation, and the like. The temperature drift compensation layer thin film then undergoes a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably using a wet etching process, but also a dry etching process, to form a pattern of the first temperature drift compensation layer 21.

[0263] S86 , forming a first electrode 11 on a side of the isolation layer 14 facing away from the base substrate 10 .

[0264] In some examples, when the first electrode 11 is made of a metal material, step 86 may include depositing a first metal film on the side of the first temperature drift compensation layer 21 facing away from the base substrate 10. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Copper foil can also be attached. Thereafter, the first metal film is subjected to a photolithography process, including glue coating (or glue spraying), pre-baking, exposure, development, and post-baking. Next, etching is performed to form a pattern including the first electrode 11. The etching process preferably adopts a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the first electrode 11.

[0265] S87 , forming a release hole 30 penetrating the first electrode 11 , the first temperature drift compensation layer 21 and the isolation layer 14 .

[0266] In some examples, step S87 may include performing a photolithography process on the side of the first electrode 11 facing away from the substrate 10, including resist coating (or spraying), pre-baking, exposure, development, and post-baking to expose the hole. A dry etching process is then performed to etch the first electrode 11. The etching gas is then changed to etch the first temperature drift compensation layer 21. Finally, the etching gas is changed to etch the isolation layer 14 until the sacrificial layer is etched. Finally, a resist stripping process is performed to form the release hole 30.

[0267] S88 , forming a piezoelectric layer 12 on a side of the first electrode 11 facing away from the base substrate 10 .

[0268] In some examples, taking the piezoelectric layer 12 as an example of an AlN single-layer structure, step S57 may include forming a piezoelectric material layer on the side of the first electrode 11 away from the substrate 10, and performing oriented growth of the piezoelectric material layer. The piezoelectric material layer is preferably formed by radio frequency magnetron sputtering (DC measurement and control sputtering is also possible). For AlN piezoelectric material, the target material is Al. By controlling the Ar and N2 gas pressures and temperatures during the deposition process and the post-annealing time and temperature, an AlN C-axis oriented piezoelectric material layer is formed, and the preferred growth orientation is (001). The deposition method of the piezoelectric material layer can also be selected from pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), etc. Next, the piezoelectric layer 12 is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Etching is then performed to form a pattern including the piezoelectric layer 12. A wet etching process is preferably used, but a dry etching process can also be used. Finally, a debonding process is performed to complete the preparation of the piezoelectric layer 12 .

[0269] S89 . Form a third sub-electrode 131 on a side of the piezoelectric layer 12 facing away from the first electrode 11 .

[0270] In some examples, when the third sub-electrode 131 is made of a metal material, step S89 may specifically include first depositing a second metal film on the side of the piezoelectric layer 12 facing away from the first electrode 11. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Next, the third metal film is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Thereafter, etching is performed to form a pattern including the third sub-electrode 131. The etching process is preferably a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the third sub-electrode 131.

[0271] S810 , forming a second temperature drift compensation layer 22 on a side of the third sub-electrode 131 facing away from the base substrate 10 .

[0272] In some examples, step S810 may specifically include: first depositing a thin film of the second temperature drift compensation layer 22, preferably using radio frequency magnetron sputtering; alternative deposition methods include pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), sol-gel method (preparing a slurry containing the temperature drift compensation layer material followed by heating and sintering), thermal evaporation, electron beam evaporation, and the like. The temperature drift compensation layer thin film then undergoes a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably using a wet etching process, but also a dry etching process, to form a pattern of the second temperature drift compensation layer 22.

[0273] S811 , forming a fourth sub-electrode 132 on a side of the second temperature drift compensation layer 22 away from the third sub-electrode 131 .

[0274] In some examples, when the fourth sub-electrode 132 is made of a metal material, step S811 may specifically include first depositing a third metal film on the side of the piezoelectric layer 12 facing away from the first electrode 11. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Next, the third metal film is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Thereafter, etching is performed to form a pattern including the fourth sub-electrode 132. The etching process is preferably a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the fourth sub-electrode 132.

[0275] S812: removing the sacrificial layer.

[0276] In some examples, step S812 may include etching the sacrificial layer, preferably using a wet etching process. Immersion etching is performed using a mixture of hydrofluoric acid, dilute nitric acid, and deionized water (the etching temperature may be appropriately increased to increase the wet etching rate) for a sufficient period of time to ensure that the boron- and phosphorus-doped silicon dioxide filling material in the first groove portion 102 is completely dissolved. Finally, the first groove portion 102 is ultrasonically cleaned multiple times with deionized water and dried to form the first groove portion 102.

[0277] S813 , forming an encapsulation layer 16 on a side of the fourth sub-electrode 132 facing away from the base substrate 10 .

[0278] In some examples, taking the encapsulation layer 16 as an example using an organic compound material, step S813 may specifically include first coating the organic material liquid, which may be done by spin coating, spraying, inkjet printing, transfer, etc., and then heating and curing to form a pattern of the encapsulation layer 16.

[0279] Of course, if multiple BAW resonators are prepared together, the preparation method provided in the embodiment of the present disclosure may further include a step of device cutting.

[0280] Ninth Example: FIG19 is a schematic structural diagram of a BAW resonator according to the ninth example of the present disclosure. As shown in FIG19 , the structure of the BAW resonator according to this example is substantially the same as that of the BAW resonator according to the eighth example, with the only difference being that, in this example, the second temperature drift compensation layer 22 has a hollow pattern and a through hole extending through the second temperature drift compensation layer 22 along its thickness. In this case, the third sub-electrode 131 and the fourth sub-electrode 132 of the second electrode 13 can be electrically connected via the through hole extending through the second temperature drift compensation layer 22, thereby reducing the resistance of the second electrode 13 and, in turn, the in-band insertion loss of the BAW resonator. The remaining structures in this BAW resonator can all adopt the same structure as in the eighth example, so they will not be described in detail here.

[0281] The preparation method of the bulk acoustic wave resonator in the ninth example can be prepared by the same method as in the eighth example. The only difference from the eighth example is that when forming the second temperature drift compensation layer 22, a through hole is formed along its thickness direction, that is, a hollow pattern is formed. The remaining steps are the same as those in the eighth example, so they will not be repeated here.

[0282] Tenth Example: FIG20 is a schematic structural diagram of a BAW resonator according to the tenth example of the present disclosure. As shown in FIG20 , the BAW resonator includes a base substrate 10, an isolation layer 14, a first temperature drift compensation layer 21, a first electrode 11, a piezoelectric layer 12, a second electrode 13, and a second temperature drift compensation layer 22 disposed on the base substrate 10. The first electrode 11 includes a first sub-electrode 111 and a second sub-electrode 112. In the BAW resonator, the isolation layer 14, the first sub-electrode 111, the first temperature drift compensation layer 21, the second sub-electrode 112, the piezoelectric layer 12, the second electrode 13, and the second temperature drift compensation layer 22 are sequentially disposed in a direction away from the base substrate 10. The base substrate 10 has a first groove 102 extending through a portion of the base substrate 10 along its thickness, forming an air gap below the isolation layer 14. The release hole 30 that passes through the first sub-electrode 111, the second sub-electrode 112, the first temperature drift compensation layer 21 and the isolation layer 14 is used to release the sacrificial layer formed in the first groove 102 during the preparation of the bulk acoustic wave resonator (specific details are described in detail in the preparation method).

[0283] Continuing with Figure 20 , an RF signal enters the upper left corner of Figure 20 . It is then converted into an acoustic wave signal through the inverse piezoelectric effect at the interface between second electrode 13 and piezoelectric layer 12. This acoustic wave propagates longitudinally through piezoelectric layer 12, and upon reaching the interface between second sub-electrode 112 and piezoelectric layer 12, it is converted back into an RF signal through the piezoelectric effect and then transmitted outward. The air gap below the BAW resonator and the air layer above it act as acoustic reflectors, confining the acoustic signal within the resonator structure rather than dissipating it, thereby reducing the resonator's insertion loss. The first temperature-drift compensation layer 21 in the disclosed embodiment is different from general materials. Its temperature-drift compensation layer material has the property of thermal contraction and thermal expansion. When the ambient temperature rises, the increase in the in-plane lattice constant of the piezoelectric layer 12 material connected to the first temperature-drift compensation layer 21 via the first electrode 11 is suppressed. The degree of suppression can be adjusted by factors such as the selection of different types of temperature-drift compensation layer thin film materials and the thickness of the temperature-drift compensation layer. Therefore, the out-of-plane lattice constant of the piezoelectric layer 12 can decrease, increase, or remain unchanged as the ambient temperature rises. In other words, it can be flexibly adjusted, thereby obtaining a bulk acoustic wave resonator with a positive temperature coefficient, a negative temperature coefficient, or even a zero temperature coefficient.

[0284] In some examples, the material of the base substrate 10 is preferably glass, but Si, sapphire, SiC, GaAs, GaN, InP, BN, ZnO, etc. can also be selected. The thickness of the base substrate 10 ranges from 0.1 μm to 10 mm. The thickness of the air gap on the base substrate 10 ranges from 0.1 μm to 50 μm.

[0285] In some examples, the first sub-electrode 111 and the second sub-electrode 112 are made of a metal material, such as Mo. Alternatively, the first sub-electrode 111 and the second sub-electrode 112 may be made of Cu, Al, Co, Ag, Ti, Pt, Ru, W, or Au, or may be alloys formed by any combination of the above metals. The thickness of the first electrode 11, formed by the first sub-electrode 111 and the second sub-electrode 112, ranges from approximately 1 nm to 10 μm.

[0286] In some examples, the material of the piezoelectric layer 12 is preferably hBN, and cBN and wBN can also be selected. Of course, the material of the piezoelectric layer 12 can also be selected from AlN, ZnO, PZT, GaN, InN, CdS, CdSe, ZnS, CdTe, ZnTe, GaAs, GaSb, InAs, InSb, GaSe, GaP, AlP, quartz crystal, LiTaO3, LiNbO3, La3Ga5SiO14, BaTiO3, PbNb2O6, PBLN, LiGaO3, LiGeO3, TiGeO3, PbTiO3, PbZrO3, PVDF and other materials. The piezoelectric layer 12 in this embodiment can be one of the above-mentioned piezoelectric materials, or it can be a stack of the above-mentioned various piezoelectric materials. The thickness of the piezoelectric layer 12 ranges from 10nm to 100μm.

[0287] In some examples, the second electrode 13 may be made of Cu, Al, Mo, Co, Ag, Ti, Pt, Ru, W, or Au, or may be an alloy of the above metals. The thickness of the second electrode 13 ranges from 1 nm to 10 μm.

[0288] In some examples, the isolation layer 14 is used to electrically isolate the air gap from the BAW resonator and provide structural support. The isolation layer 14 may be made of insulating materials such as SiO2, Si3N4, Al2O3, and combinations thereof. The thickness ranges from 1 nm to 100 μm.

[0289] In some examples, the first temperature drift compensation layer 21 and the second temperature drift compensation layer 22 are both thin films made of materials with thermal contraction and cold expansion properties. The materials that can be selected include ZrW2O8, Zn2GeO4, HfW2O8, ZrMo2O8, HfMo2O8, ZrV2O7, HfV2O7, ZrV 1.7 Mo 0.3 O 7+δ 、ZrV 1.5 Mo 0.5 O 7+δ 、Cu2V2O7、Cu 2-x Zn x V2O7 (x is 0.1 or 0.2), Cu 2-y M y V2O7 (M is any one of Yb, Sm, Ce, y is 0.05), Cu 1.5 Mg 0.5 V2O7, Cu2P2O7, Cu2PVO7, HfMgW3O 12 、HfMgMo3O 12 、ZrMgMo3O 12 、ZrMgW3O12 、ZrMnMo3O 12 、HfMnMo3O 12 、AScY2XO 12 (A is Zr or Hf, Y is W or Mo, X is V or P), TaVO5, NbVO5, Ag2O, Th2O(PO4)2, U2O(PO4)2, Zr2O(PO4)2, ScF3, CaZrF6, CaHfF6, MgZrF6, CaNbF6, CaTiF6, Zn(CN)2, Cd(CN)2, AgB(CN)4, CuB(CN)4, ScCo(CN)6, Si(NCN)2, Mn3AN(A=Zn,Ga), GdInO3, PbTiO3, PbVO3, PbVO 2.79 F 0.21 , PbV 1-x Cr x O3、Bi 0.5 Na 0.5 VO3, GeTe, LaCu3Fe4O 12 , BiNiO3, V2OPO4, Ca2RuO4, Sr2IrO4, Sr2RhO4, Ca2MnO4, Ca2GeO4, Ca3Mn2O7, Ga3Ti2O7. The thickness of the first temperature drift compensation layer 21 and the second temperature drift compensation layer 22 are both in the range of 1nm to 100um.

[0290] In some examples, referring to FIG20 , an encapsulation layer 16 is provided on the side of the second electrode 13 facing away from the substrate 10. The material of the encapsulation layer 16 is preferably an organic compound that can isolate water vapor and oxygen, such as polyimide, epoxy resin, etc., or an inorganic material such as SiN x , Al2O3, etc. The encapsulation layer 16 can be a single layer of a single material, or a stacked configuration of multiple materials.

[0291] Next, the preparation method of the BAW resonator in the tenth example is described. FIG21 is a flow chart of the preparation of the BAW resonator shown in FIG20 ; as shown in FIG21 , the preparation method specifically includes the following steps.

[0292] S101 , providing a base substrate 10 .

[0293] In some examples, taking the substrate 10 as an example of a single crystal silicon substrate, step S101 can specifically include: first, ultrasonically cleaning the single crystal silicon substrate with deionized water; then placing it in a H2SO4:H2O=3:1 mixed solution, heating it to 250°C and washing it for 15 minutes; then placing it in deionized water and ultrasonically cleaning it; then placing it in a NH4OH:H2O=1:6 mixed solution, heating it to 80°C and washing it for 15 minutes; taking it out and placing it in deionized water for rinsing; next, placing it in a HCl:H2O2:H2O=1:1:5 mixed solution, heating it to 85°C and washing it for 15 minutes, taking it out and placing it in a HF:H2O=1:20 dilute hydrofluoric acid and rinsing it for 10 seconds to remove the surface oxide layer; finally, placing it in deionized water for ultrasonic cleaning for 20 minutes, blow-drying it with an air knife, and completing the entire substrate 10 cleaning process.

[0294] S102 , forming a first groove portion 102 on the base substrate 10 .

[0295] In some examples, step S102 may specifically include: preparing a mask pattern on the substrate 10, performing a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Then, performing an etching process to form the first groove 102. The etching process may be either wet etching or dry etching, with wet etching being preferred. Finally, performing a resist stripping process to complete the preparation of the first groove 102.

[0296] S103 , forming a sacrificial layer in the first groove 102 .

[0297] In some examples, the sacrificial layer can be made of loose amorphous silicon dioxide doped with boron and phosphorus. Step S103 can specifically include forming a slurry containing loose silicon dioxide doped with boron and phosphorus using any of the processes selected from plasma enhanced chemical vapor deposition (PECVD), subatmospheric pressure chemical vapor deposition (SACVD), and screen printing, followed by thermal annealing at 700-900°C for 15-30 minutes in a vacuum chamber to liquefy and flow the loose amorphous silicon dioxide film doped with boron and phosphorus, completely filling the pores in the first groove 102 and leveling it, and then cooling and solidifying it. Finally, chemical mechanical polishing is performed, where a polishing head is used to press the substrate 10 against a rough polishing pad. The surface of the substrate 10 is flattened over a period of time by the coupled effects of polishing liquid corrosion, particle friction, and polishing pad friction, and the material overflowing from the surface of the first groove 102 is polished to a height equivalent to that of the substrate 10 surface.

[0298] S104 , forming an isolation layer 14 on the base substrate 10 .

[0299] In some examples, step S104 may specifically include: preparing an isolation layer 14 thin film on the substrate 10, first depositing an electrically insulating material, the deposition method of which may be radio frequency magnetron sputtering, pulsed laser sputtering (PLD), atomic layer deposition (ALD), or plasma chemical vapor deposition (PECVD). The isolation layer 14 is subjected to a photolithography process to form a pattern including the isolation layer 14, the photolithography process including coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably a wet etching process, but a dry etching process may also be selected.

[0300] S105 , forming a first sub-electrode 111 on a side of the isolation layer 14 facing away from the base substrate 10 .

[0301] In some examples, when the first electrode 11 is made of a metal material, step S105 may include depositing a first metal film on the side of the isolation layer 14 away from the base substrate 10. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. The copper foil attachment method can also be used. Thereafter, the second metal film is subjected to a photolithography process, including glue coating (or glue spraying), pre-baking, exposure, development, and post-baking. Next, etching is performed to form a pattern including the first sub-electrode 111. The etching process preferably adopts a wet etching process, and a dry etching process can also be selected. Finally, a de-gumming process is performed to complete the preparation of the first sub-electrode 111.

[0302] S106 , forming a first temperature drift compensation layer 21 on a side of the first sub-electrode 111 facing away from the base substrate 10 .

[0303] In some examples, step S106 may specifically include: first depositing a thin film of the first temperature drift compensation layer 21, preferably using radio frequency magnetron sputtering, but also alternative methods include pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), sol-gel method (preparing a slurry containing the temperature drift compensation layer material and then heating and sintering it), thermal evaporation, electron beam evaporation, etc. The temperature drift compensation layer thin film then undergoes a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably using a wet etching process, but also using a dry etching process, to form a pattern of the first temperature drift compensation layer 21.

[0304] S107 , forming a second sub-electrode 112 on a side of the first temperature drift compensation layer 21 facing away from the base substrate 10 .

[0305] In some examples, when the second sub-electrode 112 is made of a metal material, step S107 may include depositing a second metal film on the side of the first temperature drift compensation layer 21 facing away from the base substrate 10. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Copper foil can also be attached. The second metal film is then subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Next, etching is performed to form a pattern including the second sub-electrode 112. The etching process preferably uses a wet etching process, but a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the second sub-electrode 112.

[0306] S108 , forming a release hole 30 penetrating the first sub-electrode 111 , the second sub-electrode 112 , the isolation layer 14 and the first temperature drift compensation layer 21 .

[0307] In some examples, step S108 may specifically include performing a photolithography process on the side of the second sub-electrode 112 facing away from the substrate 10, including resist coating (or spraying), pre-baking, exposure, development, and post-baking, to expose the hole. A dry etching process is then performed to etch the second sub-electrode 112. The etching gas is then changed to etch the first temperature drift compensation layer 21. The etching gas is then changed to etch the first sub-electrode 111. Finally, the etching gas is changed to etch the isolation layer 14 until the sacrificial layer is etched. Finally, a resist stripping process is performed to form the release hole 30.

[0308] S109 , forming a piezoelectric layer 12 on a side of the first electrode 11 facing away from the base substrate 10 .

[0309] In some examples, taking the piezoelectric layer 12 as an example of an AlN single-layer structure, step S109 may include forming a piezoelectric material layer on the side of the first electrode 11 away from the substrate 10, and performing oriented growth of the piezoelectric material layer. The piezoelectric material layer is preferably formed by radio frequency magnetron sputtering (DC measurement and control sputtering is also possible). For AlN piezoelectric material, the target material is Al. By controlling the Ar and N2 gas pressures and temperatures during the deposition process and the post-annealing time and temperature, an AlN C-axis oriented piezoelectric material layer is formed, and the preferred growth orientation is (001). The deposition method of the piezoelectric material layer can also be selected from pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), etc. Next, the piezoelectric layer 12 is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Etching is then performed to form a pattern including the piezoelectric layer 12. A wet etching process is preferably used, but a dry etching process can also be used. Finally, a debonding process is performed to complete the preparation of the piezoelectric layer 12 .

[0310] S1010 , forming a second electrode 13 on a side of the piezoelectric layer 12 facing away from the first electrode 11 .

[0311] In some examples, when the second electrode 13 is made of a metal material, step S1010 may specifically include first depositing a third metal film on the side of the piezoelectric layer 12 facing away from the first electrode 11. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Next, the third metal film is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Thereafter, etching is performed to form a pattern including the second electrode 13. The etching process is preferably a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the second electrode 13.

[0312] S1011 , forming a second temperature drift compensation layer 22 on a side of the second electrode 13 facing away from the base substrate 10 .

[0313] In some examples, step S1011 may specifically include: first depositing a thin film of the second temperature drift compensation layer 22, preferably using radio frequency magnetron sputtering, but also including pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), sol-gel method (preparing a slurry containing the temperature drift compensation layer material and then heating and sintering it), thermal evaporation, electron beam evaporation, and the like. The temperature drift compensation layer thin film then undergoes a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably using a wet etching process, but also using a dry etching process, to form a pattern of the second temperature drift compensation layer 22.

[0314] S1012: removing the sacrificial layer.

[0315] In some examples, step S1012 may include etching the sacrificial layer, preferably using a wet etching process. Immersion etching is performed using a mixture of hydrofluoric acid, dilute nitric acid, and deionized water (the etching temperature may be appropriately increased to increase the wet etching rate) for a sufficient period of time to ensure that the boron- and phosphorus-doped silicon dioxide filling material in the first groove portion 102 is completely dissolved. Finally, the first groove portion 102 is ultrasonically cleaned multiple times with deionized water and dried to form the first groove portion 102.

[0316] S1013 , forming an encapsulation layer 16 on a side of the second electrode 13 facing away from the base substrate 10 .

[0317] In some examples, taking the encapsulation layer 16 as an example using an organic compound material, step S1013 may specifically include first coating the organic material liquid, which may be done by spin coating, spraying, inkjet printing, transfer, etc., and then heating and curing to form a pattern of the encapsulation layer 16.

[0318] Of course, if multiple BAW resonators are prepared together, the preparation method provided in the embodiment of the present disclosure may further include a step of device cutting.

[0319] Example 11: FIG22 is a schematic structural diagram of a BAW resonator according to the eleventh example implemented in the present disclosure. As shown in FIG11 , the structure of the BAW resonator according to this example is substantially the same as that of the BAW resonator according to the tenth example, with the only difference being that, in this example, the first temperature drift compensation layer 21 has a hollow pattern and a through hole extending through the first temperature drift compensation layer 21 along its thickness. In this case, the first sub-electrode 111 and the second sub-electrode 112 of the first electrode 11 can be electrically connected via the through hole extending through the first temperature drift compensation layer 21, thereby reducing the resistance of the first electrode 11 and, in turn, reducing the in-band insertion loss of the BAW resonator. The remaining structures in this BAW resonator can all adopt the same structure as in the tenth example, so they will not be described in detail here.

[0320] The preparation method of the bulk acoustic wave resonator in the eleventh example can be prepared by the same method as in the tenth example. The only difference from the tenth example is that when forming the first temperature drift compensation layer 21, a through hole is formed along its thickness direction, that is, a hollow pattern is formed. The remaining steps are the same as those in the tenth example, so they will not be repeated here.

[0321] Example 12: FIG23 is a schematic structural diagram of a BAW resonator according to the twelfth example of the present disclosure. As shown in FIG23 , the BAW resonator includes a base substrate 10, an isolation layer 14, a first temperature drift compensation layer 21, a first electrode 11, a piezoelectric layer 12, a second electrode 13, and a second temperature drift compensation layer 22 disposed on the base substrate 10. The first electrode 11 includes a first sub-electrode 111 and a second sub-electrode 112, and the second electrode 13 includes a third sub-electrode 131 and a fourth sub-electrode 132. In the BAW resonator, the isolation layer 14, the first sub-electrode 111, the first temperature drift compensation layer 21, the second sub-electrode 112, the piezoelectric layer 12, the third sub-electrode 131, and the fourth sub-electrode 132 of the second temperature drift compensation layer 22 are sequentially disposed in a direction away from the base substrate 10. The base substrate 10 has a first groove 102 extending through a portion of the base substrate 10 along its thickness, forming an air gap below the isolation layer 14. The release hole 30 that passes through the first sub-electrode 111, the second sub-electrode 112, the first temperature drift compensation layer 21 and the isolation layer 14 is used to release the sacrificial layer formed in the first groove 102 during the preparation of the bulk acoustic wave resonator (specific details are described in detail in the preparation method).

[0322] Continuing with Figure 23 , an RF signal enters the upper left corner of Figure 23 . It is then converted into an acoustic wave signal through the inverse piezoelectric effect at the interface between third sub-electrode 131 and piezoelectric layer 12. This acoustic wave propagates longitudinally through piezoelectric layer 12, and upon reaching the interface between second sub-electrode 112 and piezoelectric layer 12, it is converted back into an RF signal through the piezoelectric effect and then transmitted outward. The air gap below the BAW resonator and the air layer above it act as acoustic reflectors, confining the acoustic signal within the resonator structure rather than dissipating it, thereby reducing the resonator's insertion loss. The first temperature-drift compensation layer 21 in the disclosed embodiment is different from general materials. Its temperature-drift compensation layer material has the property of thermal contraction and thermal expansion. When the ambient temperature rises, the increase in the in-plane lattice constant of the piezoelectric layer 12 material connected to the first temperature-drift compensation layer 21 through the second sub-electrode 112, and to the second temperature-drift compensation layer 22 through the third sub-electrode 131, is suppressed. The degree of suppression can be adjusted by factors such as the selection of different types of temperature-drift compensation layer thin film materials and the thickness of the temperature-drift compensation layer. Therefore, the out-of-plane lattice constant of the piezoelectric layer 12 can decrease, increase, or remain unchanged as the ambient temperature increases. In other words, it can be flexibly adjusted, thereby obtaining a bulk acoustic wave resonator with a positive temperature coefficient, a negative temperature coefficient, or even a zero temperature coefficient.

[0323] In some examples, the material of the base substrate 10 is preferably glass, but Si, sapphire, SiC, GaAs, GaN, InP, BN, ZnO, etc. can also be selected. The thickness of the base substrate 10 ranges from 0.1 μm to 10 mm. The thickness of the air gap on the base substrate 10 ranges from 0.1 μm to 50 μm.

[0324] In some examples, the first sub-electrode 111 and the second sub-electrode 112 are made of a metal material, such as Mo. Alternatively, the first sub-electrode 111 and the second sub-electrode 112 may be made of Cu, Al, Co, Ag, Ti, Pt, Ru, W, or Au, or may be alloys formed by any combination of the above metals. The thickness of the first electrode 11, formed by the first sub-electrode 111 and the second sub-electrode 112, ranges from approximately 1 nm to 10 μm.

[0325] In some examples, the material of the piezoelectric layer 12 is preferably hBN, and cBN and wBN can also be selected. Of course, the material of the piezoelectric layer 12 can also be selected from AlN, ZnO, PZT, GaN, InN, CdS, CdSe, ZnS, CdTe, ZnTe, GaAs, GaSb, InAs, InSb, GaSe, GaP, AlP, quartz crystal, LiTaO3, LiNbO3, La3Ga5SiO14, BaTiO3, PbNb2O6, PBLN, LiGaO3, LiGeO3, TiGeO3, PbTiO3, PbZrO3, PVDF and other materials. The piezoelectric layer 12 in this embodiment can be one of the above-mentioned piezoelectric materials, or it can be a stack of the above-mentioned various piezoelectric materials. The thickness of the piezoelectric layer 12 ranges from 10nm to 100μm.

[0326] In some examples, the second electrode 13 may be made of Cu, Al, Mo, Co, Ag, Ti, Pt, Ru, W, or Au, or may be an alloy of the above metals. The thickness of the second electrode 13 ranges from 1 nm to 10 μm.

[0327] In some examples, the isolation layer 14 is used to electrically isolate the air gap from the BAW resonator and provide structural support. The isolation layer 14 may be made of insulating materials such as SiO2, Si3N4, Al2O3, and combinations thereof. The thickness ranges from 1 nm to 100 μm.

[0328] In some examples, the first temperature drift compensation layer 21 and the second temperature drift compensation layer 22 are both thin films made of materials with thermal contraction and cold expansion properties. The materials that can be selected include ZrW2O8, Zn2GeO4, HfW2O8, ZrMo2O8, HfMo2O8, ZrV2O7, HfV2O7, ZrV 1.7 Mo 0.3 O 7+δ 、ZrV 1.5 Mo 0.5 O 7+δ 、Cu2V2O7、Cu 2-x Zn xV2O7 (x is 0.1 or 0.2), Cu 2-y M y V2O7 (M is any one of Yb, Sm, Ce, y is 0.05), Cu 1.5 Mg 0.5 V2O7, Cu2P2O7, Cu2PVO7, HfMgW3O 12 、HfMgMo3O 12 、ZrMgMo3O 12 、ZrMgW3O 12 、ZrMnMo3O 12 、HfMnMo3O 12 、AScY2XO 12 (A is Zr or Hf, Y is W or Mo, X is V or P), TaVO5, NbVO5, Ag2O, Th2O(PO4)2, U2O(PO4)2, Zr2O(PO4)2, ScF3, CaZrF6, CaHfF6, MgZrF6, CaNbF6, CaTiF6, Zn(CN)2, Cd(CN)2, AgB(CN)4, CuB(CN)4, ScCo(CN)6, Si(NCN)2, Mn3AN(A=Zn,Ga), GdInO3, PbTiO3, PbVO3, PbVO 2.79 F 0.21 , PbV 1-x Cr x O3、Bi 0.5 Na 0.5 VO3, GeTe, LaCu3Fe4O 12 , BiNiO3, V2OPO4, Ca2RuO4, Sr2IrO4, Sr2RhO4, Ca2MnO4, Ca2GeO4, Ca3Mn2O7, Ga3Ti2O7. The thickness of the first temperature drift compensation layer 21 and the second temperature drift compensation layer 22 are both in the range of 1nm to 100um.

[0329] In some examples, referring to FIG23 , an encapsulation layer 16 is provided on the side of the second electrode 13 facing away from the substrate 10. The material of the encapsulation layer 16 is preferably an organic compound that can isolate water vapor and oxygen, such as polyimide, epoxy resin, etc., or an inorganic material such as SiN x , Al2O3, etc. The encapsulation layer 16 can be a single layer of a single material, or a stacked configuration of multiple materials.

[0330] Next, the preparation method of the BAW resonator in the twelfth example is described. FIG24 is a flow chart of the preparation of the BAW resonator shown in FIG23. As shown in FIG24, the preparation method specifically includes the following steps.

[0331] S121 , providing a base substrate 10 .

[0332] In some examples, taking the substrate 10 as an example of a single crystal silicon substrate, step S121 can specifically include: first, ultrasonically cleaning the single crystal silicon substrate with deionized water; then placing it in a H2SO4:H2O=3:1 mixed solution, heating it to 250°C and washing it for 15 minutes; then placing it in deionized water and ultrasonically cleaning it; then placing it in a NH4OH:H2O=1:6 mixed solution, heating it to 80°C and washing it for 15 minutes; taking it out and placing it in deionized water for rinsing; next, placing it in a HCl:H2O2:H2O=1:1:5 mixed solution, heating it to 85°C and washing it for 15 minutes, taking it out and placing it in a HF:H2O=1:20 dilute hydrofluoric acid and rinsing it for 10 seconds to remove the surface oxide layer; finally, placing it in deionized water for ultrasonic cleaning for 20 minutes, blow-drying it with an air knife, and completing the entire substrate 10 cleaning process.

[0333] S122 , forming a first groove portion 102 on the base substrate 10 .

[0334] In some examples, step S102 may specifically include: preparing a mask pattern on the substrate 10, performing a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Then, performing an etching process to form the first groove 102. The etching process may be either wet etching or dry etching, with wet etching being preferred. Finally, performing a resist stripping process to complete the preparation of the first groove 102.

[0335] S123 , forming a sacrificial layer in the first groove 102 .

[0336] In some examples, the sacrificial layer can be made of loose amorphous silicon dioxide doped with boron and phosphorus. Step S123 can specifically include forming a slurry containing loose silicon dioxide doped with boron and phosphorus using any of the processes selected from plasma enhanced chemical vapor deposition (PECVD), subatmospheric pressure chemical vapor deposition (SACVD), and screen printing, and then performing a thermal annealing process at 700-900°C for 15-30 minutes in a vacuum chamber to liquefy and flow the loose amorphous silicon dioxide film doped with boron and phosphorus, completely filling the pores in the first groove 102 and leveling it, and then cooling and solidifying it. Finally, chemical mechanical polishing is performed, where a polishing head is used to press the base substrate 10 against a rough polishing pad. Through the coupled effects of polishing liquid corrosion, particle friction, and polishing pad friction, the surface of the base substrate 10 is flattened over a period of time, and the surface of the material overflowing from the surface of the first groove 102 is polished to a height equivalent to that of the base substrate 10 surface.

[0337] S124 , forming an isolation layer 14 on the base substrate 10 .

[0338] In some examples, step S124 may specifically include: preparing an isolation layer 14 thin film on the substrate 10, first depositing an electrically insulating material, the deposition method of which may be radio frequency magnetron sputtering, pulsed laser sputtering (PLD), atomic layer deposition (ALD), or plasma chemical vapor deposition (PECVD). The isolation layer 14 is subjected to a photolithography process to form a pattern including the isolation layer 14, the photolithography process including coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably a wet etching process, but a dry etching process may also be selected.

[0339] S125 , forming a first sub-electrode 111 on a side of the isolation layer 14 facing away from the base substrate 10 .

[0340] In some examples, when the first electrode 11 is made of a metal material, step S125 may include depositing a first metal film on the side of the isolation layer 14 away from the base substrate 10. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. The copper foil attachment method can also be used. Thereafter, the second metal film is subjected to a photolithography process, including glue coating (or glue spraying), pre-baking, exposure, development, and post-baking. Next, etching is performed to form a pattern including the first sub-electrode 111. The etching process preferably adopts a wet etching process, and a dry etching process can also be selected. Finally, a de-gumming process is performed to complete the preparation of the first sub-electrode 111.

[0341] S126 , forming a first temperature drift compensation layer 21 on a side of the first sub-electrode 111 facing away from the base substrate 10 .

[0342] In some examples, step S126 may specifically include: first depositing a thin film of the first temperature drift compensation layer 21, preferably using radio frequency magnetron sputtering, but also alternatively using pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), sol-gel method (preparing a slurry containing the temperature drift compensation layer material and then heating and sintering it), thermal evaporation, electron beam evaporation, and the like. The temperature drift compensation layer thin film then undergoes a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably using a wet etching process, but also using a dry etching process, to form a pattern of the first temperature drift compensation layer 21.

[0343] S127 , forming a second sub-electrode 112 on a side of the first temperature drift compensation layer 21 facing away from the base substrate 10 .

[0344] In some examples, when the second sub-electrode 112 is made of a metal material, step S127 may include depositing a second metal film on the side of the first temperature drift compensation layer 21 facing away from the base substrate 10. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Copper foil can also be attached. The second metal film is then subjected to a photolithography process, including glue coating (or spraying), pre-baking, exposure, development, and post-baking. Next, etching is performed to form a pattern including the second sub-electrode 112. The etching process preferably uses a wet etching process, and a dry etching process can also be selected. Finally, a de-gumming process is performed to complete the preparation of the second sub-electrode 112.

[0345] S128 , forming a release hole 30 penetrating the first sub-electrode 111 , the second sub-electrode 112 , the isolation layer 14 , and the first temperature drift compensation layer 21 .

[0346] In some examples, step S128 may include performing a photolithography process on the side of the second sub-electrode 112 facing away from the substrate 10, including resist coating (or spraying), pre-baking, exposure, development, and post-baking, to expose the hole. A dry etching process is then performed to etch the second sub-electrode 112. The etching gas is then changed to etch the first temperature drift compensation layer 21. The etching gas is then changed to etch the first sub-electrode 111. Finally, the etching gas is changed to etch the isolation layer 14 until the sacrificial layer is etched. Finally, a resist stripping process is performed to form the release hole 30.

[0347] S129 , forming a piezoelectric layer 12 on a side of the first electrode 11 facing away from the base substrate 10 .

[0348] In some examples, taking the piezoelectric layer 12 as an example of an AlN single-layer structure, step S129 may include forming a piezoelectric material layer on the side of the first electrode 11 away from the substrate 10, and performing oriented growth of the piezoelectric material layer. The piezoelectric material layer is preferably formed by radio frequency magnetron sputtering (DC measurement and control sputtering is also possible). For AlN piezoelectric material, the target material is Al. By controlling the Ar and N2 gas pressures and temperatures during the deposition process and the post-annealing time and temperature, an AlN C-axis oriented piezoelectric material layer is formed, and the preferred growth orientation is (001). The deposition method of the piezoelectric material layer can also be selected from pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), etc. Next, the piezoelectric layer 12 is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Etching is then performed to form a pattern including the piezoelectric layer 12. A wet etching process is preferably used, but a dry etching process can also be used. Finally, a debonding process is performed to complete the preparation of the piezoelectric layer 12 .

[0349] S1210 , forming a third sub-electrode 131 on a side of the piezoelectric layer 12 facing away from the first electrode 11 .

[0350] In some examples, when the second electrode 13 is made of a metal material, step S1210 may specifically include first depositing a third metal film on the side of the piezoelectric layer 12 facing away from the first electrode 11. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be selected. Next, the third metal film is subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Thereafter, etching is performed to form a pattern including the third sub-electrode 131. The etching process is preferably a wet etching process, and a dry etching process can also be selected. Finally, a de-bonding process is performed to complete the preparation of the third sub-electrode 131.

[0351] S1211 , forming a second temperature drift compensation layer 22 on a side of the third group of electrodes facing away from the base substrate 10 .

[0352] In some examples, step S1211 may specifically include: first depositing a thin film of the second temperature drift compensation layer 22, preferably using radio frequency magnetron sputtering, but also including pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), metal organic chemical vapor deposition (MOCVD), plasma enhanced chemical vapor deposition (PECVD), sol-gel method (first applying a slurry containing the temperature drift compensation layer material, then heating and sintering), thermal evaporation, electron beam evaporation, etc. The temperature drift compensation layer thin film is then subjected to a photolithography process, including coating (or spraying), pre-baking, exposure, development, and post-baking. Finally, etching is performed, preferably using a wet etching process, but also using a dry etching process, to form a pattern of the second temperature drift compensation layer 22.

[0353] S1212 , forming a fourth sub-electrode 132 on a side of the second temperature drift compensation layer 22 away from the third sub-electrode 131 .

[0354] In some examples, when the fourth sub-electrode 132 is made of a metal material, step S1212 may specifically include first depositing a fourth metal film on the side of the second temperature drift compensation layer 22 facing away from the third sub-electrode 131. The deposition method is preferably DC magnetron sputtering (RF magnetron sputtering is also acceptable), and pulsed laser sputtering (PLD), molecular beam epitaxy (MBE), thermal evaporation, electron beam evaporation, etc. can also be used. Next, the third metal film is subjected to a photolithography process, including resist coating (or spraying), pre-baking, exposure, development, and post-baking. Etching is then performed to form a pattern including the fourth sub-electrode 132. The etching process is preferably a wet etching process, but a dry etching process can also be used. Finally, a resist stripping process is performed to complete the preparation of the fourth sub-electrode 132.

[0355] S1213. Remove the sacrificial layer.

[0356] In some examples, step S1213 may include etching the sacrificial layer, preferably using a wet etching process. Immersion etching is performed using a mixture of hydrofluoric acid, dilute nitric acid, and deionized water (the etching temperature may be appropriately increased to increase the wet etching rate) for a sufficient period of time to ensure that the boron- and phosphorus-doped silicon dioxide filling material in the first groove portion 102 is completely dissolved. Finally, the first groove portion 102 is ultrasonically cleaned multiple times with deionized water and dried to form the first groove portion 102.

[0357] S1214 , forming an encapsulation layer 16 on a side of the second electrode 13 facing away from the base substrate 10 .

[0358] In some examples, taking the encapsulation layer 16 as an example using an organic compound material, step S1214 may specifically include first coating the organic material liquid, which may be done by spin coating, spraying, inkjet printing, transfer, etc., and then heating and curing to form a pattern of the encapsulation layer 16.

[0359] Of course, if multiple BAW resonators are prepared together, the preparation method provided in the embodiment of the present disclosure may further include a step of device cutting.

[0360] Thirteenth Example: FIG25 is a schematic diagram of the structure of the BAW resonator of the thirteenth example implemented in the present disclosure; as shown in FIG25 , the structure of the BAW resonator of this example is substantially the same as that of the BAW resonator of the twelfth example, with the only difference being that in this example, the first temperature drift compensation layer 21 has a hollow pattern, and the first temperature drift compensation layer 21 also has a through hole extending through its thickness. In this case, the first sub-electrode 111 and the second sub-electrode 112 of the first electrode 11 can be electrically connected through the through hole extending through the first temperature drift compensation layer 21, thereby reducing the resistance of the first electrode 11 and, in turn, reducing the in-band insertion loss of the BAW resonator. The remaining structures in this BAW resonator can adopt the same structure as in the twelfth example, so they will not be described in detail here.

[0361] The preparation method of the bulk acoustic wave resonator in the thirteenth example can be prepared by the same method as in the twelfth example. The only difference from the twelfth example is that when forming the first temperature drift compensation layer 21, a through hole is formed along its thickness direction, that is, a hollow pattern is formed. The remaining steps are the same as in the twelfth example, so they will not be repeated here.

[0362] Fourteenth Example: FIG26 is a schematic structural diagram of a BAW resonator according to the fourteenth example implemented in the present disclosure. As shown in FIG26 , the structure of the BAW resonator in this example is substantially the same as that of the BAW resonator in the twelfth example, with the only difference being that in this example, the second temperature drift compensation layer 22 has a hollow pattern and a through hole extending through the second temperature drift compensation layer 22 along its thickness. In this case, the third sub-electrode 131 and the fourth sub-electrode 132 of the second electrode 13 can be electrically connected via the through hole extending through the second temperature drift compensation layer 22, thereby reducing the resistance of the second electrode 13 and, in turn, the in-band insertion loss of the BAW resonator. The remaining structures in this BAW resonator can adopt the same structures as those in the twelfth example, so they will not be described in detail here.

[0363] The preparation method of the bulk acoustic wave resonator in the fourteenth example can be prepared by the same method as in the twelfth example. The only difference from the twelfth example is that when forming the second temperature drift compensation layer 22, a through hole is formed along its thickness direction, that is, a hollow pattern is formed. The remaining steps are the same as in the twelfth example, so they will not be repeated here.

[0364] Fifteenth Example: FIG27 is a schematic structural diagram of a BAW resonator according to the fifteenth example of the present disclosure. As shown in FIG27 , the structure of the BAW resonator according to this example is substantially the same as that of the BAW resonator according to the twelfth example, with the only difference being that, in this example, the first temperature drift compensation layer 21 has a hollow pattern and a through hole extending through the thickness of the first temperature drift compensation layer 21, and the second temperature drift compensation layer 22 has a hollow pattern, i.e., the second temperature drift compensation layer 22 has a through hole extending through the thickness of the second temperature drift compensation layer 22. In this case, the first sub-electrode 111 and the second sub-electrode 112 of the first electrode 11 can be electrically connected via the through hole extending through the first temperature drift compensation layer 21, thereby reducing the resistance of the first electrode 11. The third sub-electrode 131 and the fourth sub-electrode 132 of the second electrode 13 can be connected via the through hole extending through the second temperature drift compensation layer 22, thereby reducing the resistance of the second electrode 13 and, in turn, reducing the in-band insertion loss of the BAW resonator. The remaining structures of this BAW resonator can adopt the same structures as those in the twelfth example, and therefore will not be described in detail here.

[0365] The preparation method of the bulk acoustic wave resonator in the fifteenth example can be prepared by the same method as in the twelfth example. The only difference from the twelfth example is that when forming the first temperature drift compensation layer 21, a through hole is formed along its thickness direction, that is, a hollow pattern is formed. The remaining steps are the same as in the twelfth example, so they will not be repeated here.

[0366] Only fifteen exemplary BAW resonators and methods for preparing some BAW resonators are given above. However, it should be understood that providing a temperature drift compensation layer for the BAW resonators of Figures 1 and 3 in the manner described above is also within the scope of protection of the embodiments of the present disclosure and will not be described in detail here.

[0367] An embodiment of the present disclosure further provides an electronic device, which may include any of the above-mentioned bulk acoustic wave resonators.

[0368] It will be understood that the above embodiments are merely exemplary embodiments for illustrating the principles of the present invention, and the present invention is not limited thereto. Those skilled in the art will appreciate that various modifications and improvements can be made without departing from the spirit and substance of the present invention, and such modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. A bulk acoustic wave resonator, comprising: A substrate, a first electrode, a piezoelectric layer, and a second electrode; The first electrode is arranged on the substrate, the second electrode is arranged on the side of the first electrode away from the substrate, the piezoelectric layer is arranged between the first electrode and the second electrode, and the orthographic projections of any two of the first electrode, the piezoelectric layer and the second electrode on the substrate at least partially overlap; wherein, A temperature drift compensation layer is provided on a side of the piezoelectric layer close to the substrate and / or a side of the piezoelectric layer away from the substrate; The material of the temperature drift compensation layer has a property of thermal expansion and contraction, and is configured to suppress the temperature drift of the BAW resonator.

2. The BAW resonator according to claim 1, wherein: Temperature drifting materials ZrW2O8, Zn2GeO4, HfW2O8, ZrMo2O8, HfMo2O8, ZrV2O7, HfV2O7, ZrV 1.7 Mo 0.3 O 7+δ , ZrV 1.5 Mo 0.5 O 7+δ , Cu2V2O7, Cu 2-x Zinc x V2O7, Cu 2-y M y V2O7, Cu 1.5 Mg 0.5 V2O7, Cu2P2O7, Cu2PVO7, HfMgW3O 12 , HfMgMoO 12 , ZrMgMoO 12 , ZrMgWO 12 , ZrMnMoO 12 , HfMnMoO 12 , AScY2XO 12 , TaVO5, NbVO5, Ag2O, Th2O(PO4)2, U2O(PO4)2, Zr2O(PO4)2, ScF3, CaZrF6, CaHfF6, MgZrF6, CaNbF6, CaTiF6, Z n(CN)2, Cd(CN)2, AgB(CN)4, CuB(CN)4, ScCo(CN)6, Si(NCN)2, Mn3AN(A=Zn,Ga), GdInO3, PbTiO3, PbVO3, PbVO 2.79 F 0.21 , PbV 1-x Cr x O3, Bi 0.5 Na 0.5 VO3, GeTe, LaCu3Fe4O 12 , BiNiO3, V2OPO4, Ca2RuO4, Sr2IrO4, Sr2RhO4, Ca2MnO4, Ca2GeO4, Ca3Mn2O7, Ga3Ti2O7; For Cu 2-x Zn x V2O7, where x is 0.1 or 0.2; Cu 2-y M y V2O7, where M is any one of Yb, Sm, and Ce, and y is 0.05; AScY2XO 12 , wherein A is Zr or Hf, Y is W or Mo, and X is V or P.

3. The BAW resonator according to claim 1, wherein: The thickness of the temperature drift compensation layer is 1 nm-100 μm.

4. The BAW resonator according to claim 1, wherein: The temperature drift compensation layer has a hollow pattern.

5. The BAW resonator according to claim 1, wherein: When the temperature drift compensation layer is located on a side of the piezoelectric layer close to the substrate, the temperature drift compensation layer is located on a side of the first electrode away from the piezoelectric layer.

6. The BAW resonator according to claim 1, wherein: When the temperature drift compensation layer is located at a side of the piezoelectric layer away from the substrate, the temperature drift compensation layer is located at a side of the second electrode away from the piezoelectric layer.

7. The BAW resonator according to claim 1, wherein: The first electrode includes a first sub-electrode and a second sub-electrode arranged in sequence along a direction away from the base substrate. When the temperature drift compensation layer is located on a side of the piezoelectric layer close to the base substrate, the temperature drift compensation layer is located between the first sub-electrode and the second sub-electrode.

8. The BAW resonator according to claim 1, wherein: The first electrode includes a third sub-electrode and a fourth sub-electrode arranged in sequence along a direction away from the substrate. When the temperature drift compensation layer is located on a side of the piezoelectric layer close to the substrate, the temperature drift compensation layer is located between the third sub-electrode and the fourth sub-electrode.

9. The BAW resonator according to any one of claims 1 to 8, wherein: The base substrate has a first groove portion penetrating a portion of the base substrate along a thickness direction thereof; an isolation layer is provided on a side of the opening of the first groove portion facing the first electrode.

10. The BAW resonator according to any one of claims 1 to 8, wherein: It also includes an isolation layer arranged between the base substrate and the first electrode; a certain space is defined between the isolation layer and the base substrate.

11. The BAW resonator according to any one of claims 1 to 8, wherein: The base substrate has a first cavity penetrating along the thickness direction thereof; an isolation layer is arranged on a side of the base substrate close to the first electrode.

12. A method for preparing a bulk acoustic wave resonator, comprising: The steps of sequentially forming a first electrode, a piezoelectric layer and a second electrode on a substrate, wherein the orthographic projections of any two of the first electrode, the piezoelectric layer and the second electrode on the substrate at least partially overlap; wherein the preparation method further comprises: forming a temperature drift compensation layer on a side of the piezoelectric layer close to the first substrate, and / or forming the temperature drift compensation layer on a side of the voltage component away from the first substrate; the material of the temperature drift compensation layer has the property of thermal expansion and contraction, and is configured to suppress the temperature drift of the BAW resonator.

13. The method for preparing a bulk acoustic wave resonator according to claim 12, wherein: Temperature drifting materials ZrW2O8, Zn2GeO4, HfW2O8, ZrMo2O8, HfMo2O8, ZrV2O7, HfV2O7, ZrV 1.7 Mo 0.3 O 7+δ , ZrV 1.5 Mo 0.5 O 7+δ , Cu2V2O7, Cu 2-x Zinc x V2O7, Cu 2-y M y V2O7, Cu 1.5 Mg 0.5 V2O7, Cu2P2O7, Cu2PVO7, HfMgW3O 12 , HfMgMoO 12 , ZrMgMoO 12 , ZrMgWO 12 , ZrMnMoO 12 , HfMnMoO 12 , AScY2XO 12 , TaVO5, NbVO5, Ag2O, Th2O(PO4)2, U2O(PO4)2, Zr2O(PO4)2, ScF3, CaZrF6, CaHfF6, MgZrF6, CaNbF6, CaTiF6, Z n(CN)2, Cd(CN)2, AgB(CN)4, CuB(CN)4, ScCo(CN)6, Si(NCN)2, Mn3AN(A=Zn,Ga), GdInO3, PbTiO3, PbVO3, PbVO 2.79 F 0.21 , PbV 1-x Cr x O3, Bi 0.5 Na 0.5 VO3, GeTe, LaCu3Fe4O 12 , BiNiO3, V2OPO4, Ca2RuO4, Sr2IrO4, Sr2RhO4, Ca2MnO4, Ca2GeO4, Ca3Mn2O7, Ga3Ti2O7; For Cu 2-x Zn x V2O7, where x is 0.1 or 0.2; Cu 2-y M y V2O7, where M is any one of Yb, Sm, and Ce, and y is 0.05; AScY2XO 12 , wherein A is Zr or Hf, Y is W or Mo, and X is V or P.

14. The method for preparing a bulk acoustic wave resonator according to claim 12, wherein: The thickness of the temperature drift compensation layer is 1 nm-100 μm.

15. The method for preparing a bulk acoustic wave resonator according to claim 12, wherein: The temperature drift compensation layer has a hollow pattern.

16. The method for preparing a bulk acoustic wave resonator according to claim 12, wherein: When the preparation method includes forming the temperature drift compensation layer on a side of the piezoelectric layer close to the base substrate, the step of forming the temperature drift compensation layer is prior to the step of forming the first electrode.

17. The method for preparing a bulk acoustic wave resonator according to claim 12, wherein: When the preparation method includes forming the temperature drift compensation layer on a side of the piezoelectric layer facing away from the substrate, the step of forming the temperature drift compensation layer is after the step of forming the second electrode.

18. The method for preparing a bulk acoustic wave resonator according to claim 12, wherein: The step of forming the first electrode comprises: forming a first sub-electrode and a second sub-electrode in sequence along a direction away from the substrate; When the preparation method includes forming the temperature drift compensation layer on a side of the piezoelectric layer close to the base substrate, the step of forming the temperature drift compensation layer is between the step of forming the first sub-electrode and the step of forming the second sub-electrode.

19. The method for preparing a bulk acoustic wave resonator according to claim 12, wherein: The step of forming the second electrode comprises: forming a third sub-electrode and a fourth sub-electrode in sequence along a direction away from the base substrate; When the preparation method includes forming the temperature drift compensation layer on a side of the piezoelectric layer away from the substrate, the step of forming the temperature drift compensation layer is between the step of forming the third sub-electrode and the step of forming the fourth sub-electrode.

20. The method for preparing a bulk acoustic wave resonator according to claim 12, wherein: The preparation method further includes: processing the base substrate to form a first groove portion penetrating a portion of the base substrate along a thickness direction thereof; and providing an isolation layer on a side of the opening of the first groove portion facing the first electrode.

21. The method for preparing a bulk acoustic wave resonator according to claim 12, wherein: The preparation method further includes: forming an isolation layer before forming the first electrode; and defining a certain space between the isolation layer and the base substrate.

22. The method for preparing a bulk acoustic wave resonator according to claim 12, wherein: The preparation method further includes: processing the base substrate to form a first cavity penetrating along the thickness direction of the base substrate; and forming an isolation layer on a side of the base substrate close to the first electrode.