Method for manufacturing cookware and cookware
The wear-resistant layer and amorphous carbon layer are formed on the surface of the cookware substrate through plasma carburizing treatment, which solves the problem of both initial non-stickness and long-lasting non-stickness of the cookware, and achieves the continuous non-stick effect of the cookware during use.
Patent Information
- Application Number
- CN202411181983.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-06
AI Technical Summary
It is difficult for existing cookware to have both initial non-stick and long-lasting non-stick. The initial non-stickness of the carbide coating is poor, and it is necessary to add grease or use a material with good non-stickness for modification, but it is difficult to form a stable and long-lasting oil film.
Using plasma carburizing treatment, an wear-resistant layer and an amorphous carbon layer are formed on the surface of the cooker substrate. The amorphous carbon layer has an amorphous form and interlayer gap, is located outside the wear-resistant layer, and is formed on its concave and convex structure, and is resistant to The abrasive layer provides hardness and protection to ensure the durable non-stickness of the amorphous carbon layer.
It achieves excellent non-stickness of the cookware during first use and continues to maintain long-term non-stickness during long-term use, avoiding peeling or damage of the coating and improving the overall performance of the cookware.
Smart Images

Figure CN119073778A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of kitchenware, and in particular to a method for manufacturing a cooker and the cooker. Background Art
[0002] In the field of cookware, non-stick properties have always been a hot topic of research. In order to obtain cookware with certain non-stick properties, a coating is usually provided on a substrate to ensure the non-stick properties of the formed cookware.
[0003] However, it is still difficult for existing coated cookware to achieve both initial non-stick and lasting non-stick properties. For example, although the coating formed by carbide materials is wear-resistant, the initial non-stick properties of the cookware with such coating are poor and cannot meet the national standard requirements for initial non-stick properties. It is usually necessary to add grease or modify it with materials with good non-stick properties (such as polysiloxanes and fluorinated materials) to improve its non-stick properties. Taking the addition of edible oil as grease as an example, to achieve a better non-stick effect, a uniform oil film needs to be formed on the surface of the cookware, but the bonding force between the carbide layer and the edible oil is weak, so it cannot form a stable and lasting oil film to exert non-stick properties.
[0004] For this reason, obtaining cookware with both initial non-stick and lasting non-stick properties remains an issue that requires ongoing attention. Summary of the invention
[0005] Therefore, the object of the present application is to provide a method for manufacturing cookware and the cookware, so as to solve the problem that the cookware in the prior art cannot have both initial non-stick properties and lasting non-stick properties.
[0006] According to a first aspect of the present application, a cooker is provided, wherein the cooker includes a cooker substrate and a carburized layer formed on the cooker substrate, the carburized layer includes a wear-resistant layer and an amorphous carbon layer, the wear-resistant layer is in contact with the cooker substrate, and has a concave-convex structure on its surface; the amorphous carbon layer is formed on the concave-convex structure of the wear-resistant layer, has an interlayer gap and serves as the surface layer of the cooker.
[0007] According to the cooker provided by the embodiment of the present application, the amorphous morphology and interlayer gap structure of the amorphous carbon layer enable the cooker to exhibit excellent non-stick properties when used for the first time. The amorphous carbon layer is located on the outside of the wear-resistant layer and is formed on the concave-convex structure of the wear-resistant layer. The wear-resistant layer has high hardness and wear resistance, and can protect the amorphous carbon layer located in the depressions of the concave-convex structure, so that the amorphous carbon layer is not easily worn due to use, ensuring that it is not easy to lose its non-stick properties during later use. As the use time increases, the grease or silicone oil stored in the interlayer gaps of the amorphous carbon layer can continue to play a role, ensuring the long-lasting non-stick properties of the cooker. Therefore, the cooker according to the present application can have both better initial non-stick properties and long-lasting non-stick properties.
[0008] In some embodiments, the wear-resistant layer includes a first sublayer located inside and a second sublayer located outside, the first sublayer is a solid solution layer in contact with the cookware substrate, and the second sublayer is a mixed layer of saturated solid solution and carbide in contact with the amorphous carbon layer.
[0009] In these embodiments, the first sublayer is a solid solution layer. As the inner sublayer of the wear-resistant layer, the first sublayer not only ensures the bonding strength between the wear-resistant layer and the substrate, but also ensures the hardness and strength of the wear-resistant layer due to the formation of the solid solution, thereby improving the wear resistance of the cooker, so that the cooker can resist wear and scratches during use. The second sublayer is the outer sublayer of the wear-resistant layer. The second sublayer is directly in contact with the amorphous carbon layer. Its high hardness and high wear resistance can protect the amorphous carbon layer from wear, and its surface characteristics can ensure the bonding strength between the wear-resistant layer and the amorphous carbon layer. In addition, the presence of carbides in the second sublayer can also have a positive effect on the formation and performance of the amorphous carbon layer. For example, carbides, as hard phases, can enhance the overall structural strength of the amorphous carbon layer with their high hardness and wear resistance. This enhanced structural stability helps to better carry and fix lubricating substances such as grease or silicone oil to prevent them from being easily squeezed out or lost during use. Therefore, the presence of carbides improves the durability and reliability of the amorphous carbon layer as a lubricating surface.
[0010] In some embodiments, the thickness of the cookware substrate is 1.5 mm-2.0 mm; and / or the thickness of the wear-resistant layer is 20 μm-40 μm, and / or the thickness of the amorphous carbon layer is 5 μm-15 μm.
[0011] In these embodiments, each layer has a certain thickness distribution, which can balance the factors of non-stickiness, wear resistance and manufacturing cost of the cookware, thereby improving the overall performance of the cookware.
[0012] In some embodiments, the amorphous carbon layer is oleophilic and has a surface energy of 15 dynes to 25 dynes, thereby improving the non-stick performance of the cookware.
[0013] In some embodiments, the cookware substrate includes one of a pure iron substrate, a cast iron substrate, a stainless steel substrate, an aluminum substrate, a titanium substrate, and a low-carbon steel substrate. There are many types of substrates for forming the cookware, which can facilitate the manufacture of multiple types of cookware according to actual needs.
[0014] In some embodiments, the interlayer gaps of the amorphous carbon layer are filled with grease or silicone oil to further improve the non-stick properties of the cookware.
[0015] In some embodiments, the concavo-convex structure is formed by a plurality of convex hulls, the spacing between adjacent convex hulls is 0.2 mm-0.5 mm, the height of the convex hulls is 15 μm-50 μm, and the width of the convex hulls is 0.2 mm-0.5 mm. In a preferred embodiment, the thickness of the amorphous carbon layer is not greater than the roughness value of the concavo-convex structure. The concavo-convex structure with such roughness can make most of the amorphous carbon layer formed in the concave part of the concavo-convex structure of the wear-resistant layer. In this way, the wear-resistant layer can provide protection for the amorphous carbon layer during the cooking process to optimize the long-lasting non-stickiness.
[0016] According to a second aspect of the present application, a method for manufacturing cookware is provided, wherein the method for manufacturing cookware comprises: performing plasma carburizing treatment on a cookware substrate having a rough structure to form a carburized layer including a wear-resistant layer and an amorphous carbon layer, wherein the wear-resistant layer is formed on the surface of the cookware substrate, and the surface has a concave-convex structure, and the amorphous carbon layer is formed on the concave-convex structure of the wear-resistant layer, has an interlayer gap, and serves as the surface layer of the cookware.
[0017] According to the method for manufacturing cookware provided by the embodiment of the present application, a plasma carburizing treatment is performed on a cookware substrate with a rough structure to form a carburized layer including a wear-resistant layer and an amorphous carbon layer, wherein the wear-resistant layer is formed on the surface of the cookware substrate, and the outer surface has a concave-convex structure similar to the rough structure of the cookware substrate, and the amorphous carbon layer has an amorphous morphology and is formed on the concave-convex structure of the wear-resistant layer. It can be understood that the amorphous morphology and interlayer gap structure of the amorphous carbon layer enable the cookware to exhibit excellent non-stick properties when used for the first time. The amorphous carbon layer is located on the outside of the wear-resistant layer and is formed on the concave-convex structure of the wear-resistant layer. The wear-resistant layer has high hardness and wear resistance, and can protect the amorphous carbon layer located in the concave part of the concave-convex structure, so that the amorphous carbon layer is not easily worn due to use, and it is ensured that it is not easy to lose its non-stick properties during later use. With the extension of the use time, the grease or silicone oil stored in the interlayer gap of the amorphous carbon layer can continue to play a role and maintain the lasting non-stick properties of the cookware. Therefore, the cookware manufactured according to the method for manufacturing cookware of the present application can have both better initial non-stick properties and lasting non-stick properties.
[0018] In some embodiments, the plasma carburizing treatment includes a first stage, in which a first flow rate of carburizing gas is introduced so that the carburizing gas decomposes and forms carbon ions, and the supply speed of the carbon ions is smaller than the penetration speed of the carbon ions, so as to form the wear-resistant layer at the surface of the cookware substrate with a preset depth. In this way, the carbon ions have enough time to diffuse inward and be evenly distributed on the surface of the cookware substrate, thereby ensuring that the carbon ions can fully and evenly penetrate into the surface of the cookware substrate in the first stage to promote the formation of the wear-resistant layer.
[0019] In some embodiments, the plasma carburizing treatment also includes a second stage, in which a second flow rate of carburizing gas is introduced so that the carburizing gas decomposes and forms carbon ions, and the second flow rate is greater than the first flow rate or the plasma carburizing power of the second stage is greater than the plasma carburizing power of the carburizing parameters of the first stage, so as to form the amorphous carbon layer with the interlayer gap on the wear-resistant layer.
[0020] In these embodiments, the second stage not only ensures the formation of an amorphous carbon layer and the introduction of interlayer gaps by adjusting the flux of the carburizing gas and the plasma carburizing power, but also improves the carburizing efficiency and the surface properties of the cookware, thereby ultimately achieving a higher level of wear resistance, non-stickiness, and other aspects of the cookware.
[0021] In some embodiments, the first flow rate is 10 L / h-20 L / h, and the carburizing gas of the first flow rate is introduced in a pulsed manner.
[0022] In these embodiments, a low flow rate of 10 L / h to 20 L / h is adopted, and a pulsed introduction method is used to control the supply speed of carbon ions to always be lower than the penetration speed of carbon ions, so that uniform and sufficient penetration of carbon ions into the surface layer of the cookware substrate can be achieved.
[0023] In some embodiments, the cookware substrate is controlled to contact the carbon ions under the conditions of a pressure of 80 Pa-100 Pa and a temperature of 700° C.-800° C., so that a supply speed of the carbon ions is lower than a penetration speed of the carbon ions.
[0024] In these embodiments, the first stage of carburizing is carried out under a pressure of 80Pa to 100Pa and a temperature of 500°C to 700°C. These conditions can form the diffusion kinetics of carbon ions and affect the penetration rate of carbon ions, thereby controlling the supply rate of carbon ions to be always lower than the penetration rate of carbon ions, thereby ensuring the depth, rate and uniformity of carburizing.
[0025] In some embodiments, the second flow rate is 150L / h-300L / h, the plasma carburizing power of the second stage is 10KW-20KW, the plasma carburizing power of the carburizing parameters of the first stage is 3KW-5KW; and / or the temperature of the second stage is 400℃-500℃.
[0026] In these embodiments, a high-flow, highly unsaturated acetylene gas is introduced as the carburizing gas. Under the influence of the plasma carburizing power in the second stage, the carburizing gas can be rapidly decomposed to form a high concentration of carbon ions, which impact the surface of the iron substrate to form an amorphous carbon layer with an interlayer structure and relatively dense.
[0027] In some embodiments, the plasma carburizing treatment of the cookware substrate having a rough structure further includes setting the voltage between the cathode and anode of the plasma carburizing device to 200 V-1500 V. In this way, the generation and maintenance of plasma can be enhanced, which is conducive to the rapid decomposition and deposition of carbon ions, thereby forming an amorphous carbon layer with a specific interlayer gap.
[0028] In some embodiments, before the plasma carburizing treatment, the cookware substrate is preheated at a temperature of 480°C-600°C to activate the atoms on the surface of the cookware substrate. During the preheating process, the atoms inside the cookware substrate material obtain sufficient energy and begin to vibrate and move, which helps to break the binding force between the atoms, making the surface atoms more active and easy to react with the carbon ions in the subsequent carburizing treatment process, providing more favorable conditions for the subsequent carburizing treatment, ensuring that in the subsequent plasma carburizing treatment process, the carbon ions can penetrate into the material of the cookware substrate more quickly and evenly to form a uniform and stable carburized layer.
[0029] In some embodiments, the cookware substrate is shot peened to provide a rough structure with a surface roughness of 60 μm-200 μm. The rough structure with such a roughness can protect the concave-convex structure of the wear-resistant layer formed subsequently, so that it has a suitable roughness, thereby providing suitable protection for the amorphous carbon layer to further improve the long-lasting non-stick performance.
[0030] In some embodiments, the method for manufacturing cookware further includes: placing the cookware substrate having the carburized layer in silicone oil or grease, so that the silicone oil and grease are filled into the carburized layer to further improve the non-stick performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The above and / or other features and aspects of the present invention will become clear and easily understood through the description of the embodiments in conjunction with the accompanying drawings.
[0032] Figure 1A schematic structural diagram of a cooker base of a cooker provided according to an embodiment of the present application is shown;
[0033] Figure 2 A schematic structural diagram of a cooker provided according to an embodiment of the present application is shown;
[0034] Figure 3 Shows Figure 2 A local enlarged schematic diagram of point I in the middle. DETAILED DESCRIPTION
[0035] The specific implementation methods of the present application are described in detail below. Although some embodiments have been shown and described, those skilled in the art should understand that these embodiments can be modified and improved without departing from the principles and spirit of the present application whose scope is defined by the claims and their equivalents.
[0036] In the field of cookware, non-stick properties have always been a hot topic of research. In order to obtain cookware with certain non-stick properties, a coating is usually provided on a substrate to ensure the non-stick properties of the formed cookware.
[0037] However, it is still difficult for existing coated cookware to achieve both initial non-stick and lasting non-stick properties. For example, although the coating formed by carbide materials is wear-resistant, the initial non-stick properties of the cookware with such coating are poor and cannot meet the national standard requirements for initial stickiness. It is usually necessary to add grease or modify it with materials with good non-stick properties (such as polysiloxanes and fluorinated materials) to improve its non-stick properties. Taking the addition of edible oil as grease as an example, to achieve a better non-stick effect, a uniform oil film needs to be formed on the surface of the cookware, but the bonding force between the carbide layer and the edible oil is weak, so it cannot form a stable and lasting oil film to exert non-stick properties.
[0038] Therefore, solving the poor initial non-stick and long-term non-stick properties of cookware remains an issue that requires continued attention.
[0039] The applicant has found that by performing plasma carburizing treatment on a substrate of an iron-based alloy having a rough structure, the outer layer of the cookware substrate is formed into a wear-resistant layer. In this case, the outer surface of the wear-resistant layer is formed into a concave-convex structure corresponding to the rough structure, and an amorphous carbon layer is also formed on the concave-convex structure of the wear-resistant layer. The amorphous carbon layer is the outer layer of the carburized layer and also serves as the outer layer of the cookware. It has an amorphous morphology and has good non-stick properties. In addition, the amorphous carbon layer has interlayer gaps, and grease or silicone oil can be locked in the interlayer gaps, so that the cookware can be convenient for continuous oil storage during use and further improve the non-stick properties. In addition, the amorphous carbon layer is located on the outside of the wear-resistant layer and is formed on the concave-convex structure of the wear-resistant layer. The wear-resistant layer has high hardness and wear resistance, and can protect the amorphous carbon layer located in the depressions of the concave-convex structure, so that the amorphous carbon layer is not easily worn due to use. In addition, unlike the traditional multi-layer coating structure, the carburized layer formed by plasma carburizing in the cookware of the present application does not have the problem of interlayer bonding with the substrate, so that the bonding between the carburized layer and the substrate is more solid and not easy to peel off or damage. In summary, the cookware according to the present application can have both good initial non-stickiness and long-lasting non-stickiness.
[0040] According to a first aspect of the present application, a method for manufacturing cookware is provided, wherein the method for manufacturing cookware includes performing plasma carburizing treatment on a cookware substrate having a rough structure to form a carburized layer including a wear-resistant layer and an amorphous carbon layer, wherein the wear-resistant layer is formed on the surface of the cookware substrate, the surface having a concave-convex structure, and the amorphous carbon layer is formed on the concave-convex structure of the wear-resistant layer.
[0041] According to the method for manufacturing cookware provided by the embodiment of the present application, a plasma carburizing treatment is performed on a cookware substrate with a rough structure to form a carburized layer including a wear-resistant layer and an amorphous carbon layer, wherein the wear-resistant layer is formed on the surface of the cookware substrate, and the outer surface has a concave-convex structure similar to the rough structure of the cookware substrate, and the amorphous carbon layer has an amorphous morphology and is formed on the concave-convex structure of the wear-resistant layer. It can be understood that the amorphous morphology and interlayer gap structure of the amorphous carbon layer enable the cookware to exhibit excellent non-stick properties when used for the first time. The amorphous carbon layer is located on the outside of the wear-resistant layer and is formed on the concave-convex structure of the wear-resistant layer. The wear-resistant layer has high hardness and wear resistance, and can protect the amorphous carbon layer located in the concave part of the concave-convex structure, so that the amorphous carbon layer is not easily worn due to use, and it is ensured that it is not easy to lose its non-stick properties during later use. With the extension of the use time, the grease or silicone oil stored in the interlayer gap of the amorphous carbon layer can continue to play a role and maintain the lasting non-stick properties of the cookware. Therefore, the cookware manufactured according to the method for manufacturing cookware of the present application can have both better initial non-stick properties and lasting non-stick properties.
[0042] According to the present application, the carburized layer is different from the traditional multi-layer coating structure. There is no problem of interlayer bonding between the carburized layer formed by plasma carburizing treatment and the substrate of the cookware of the present application. Therefore, the bonding between the carburized layer and the substrate is stronger and not easy to peel off or be damaged.
[0043] In summary, the cookware manufactured according to the method for manufacturing cookware of the present application can have both better initial non-stick properties and lasting non-stick properties.
[0044] It should be noted that the surface layer of the cookware base is the area from the surface of the cookware base to the inside in the thickness direction.
[0045] According to the present application, an amorphous carbon layer is formed on the outermost layer of the cookware, and its excellent self-lubricating effect, low surface energy and amorphous properties are utilized to ensure the non-stick effect of the cookware. In addition, it has good bonding force with edible oil and can lock the oil to form a stable oil film, thereby further improving the non-stick effect of the cookware.
[0046] Hereinafter, the method for manufacturing a cooker according to the present application will be described in conjunction with specific embodiments.
[0047] Provide cookware base
[0048] According to the present application, the cookware base 100 has the basic structure of a cookware formed by stretching a corresponding substrate. In some embodiments, the thickness of the cookware base 100 is 1.55 mm-2.5 mm, and such a thickness can ensure the overall strength of the cookware finally formed.
[0049] In some embodiments, the inner surface of the cookware base 100 has a rough structure, and as an example, the roughness of the rough structure may be 60 μm-200 μm. It should be noted that the present application does not overly limit the roughness of the rough structure, and those skilled in the art may select other suitable roughnesses under the guidance of the present application.
[0050] Figure 1 FIG. 1 shows a schematic structural diagram of a cooker base according to an embodiment of the present application. Figure 1 As shown, the inner surface of the cookware base 100 has a rough structure. As an example, the cookware base is pressed to have a rough structure with a surface roughness of 60 μm-200 μm. Such a rough structure with such a roughness can make the concave-convex structure of the formed wear-resistant layer have a suitable roughness, thereby providing suitable protection for the amorphous carbon layer to further improve the long-lasting non-stick performance.
[0051] In some embodiments, the cookware substrate includes one of a pure iron substrate, a cast iron substrate, an aluminum substrate, a titanium substrate, a stainless steel substrate, and a low carbon steel substrate.
[0052] According to the present application, the method for manufacturing cookware can be suitable for more types of substrates, thereby expanding the range of substrates that can be adapted to the manufacture of cookware, and has better versatility.
[0053] Vacuum
[0054] According to the present application, before the plasma carburizing treatment, the cookware substrate can be placed in a plasma carburizing device, and the plasma carburizing device can be evacuated to a low vacuum state (0.1Pa-1Pa) by a vacuum pump. In this way, the air and other impurities in the plasma carburizing device can be removed to avoid the influence of impurities on the carburizing process.
[0055] Preheating the cookware base
[0056] According to the present application, before the plasma carburizing treatment, the cookware substrate can be preheated at a preheating temperature of 480°C-600°C for 15min-30min to activate the atoms on the surface of the cookware substrate. During the preheating process, the atoms inside the cookware substrate material obtain sufficient energy and begin to vibrate and move, which helps to break the binding force between the atoms, making the surface atoms more active and easy to react with the carbon ions in the subsequent carburizing process, providing more favorable conditions for the subsequent carburizing process, ensuring that in the subsequent plasma carburizing process, the carbon ions can penetrate into the material of the cookware substrate more quickly and evenly to form a uniform and stable carburized layer.
[0057] Specifically, the cookware substrate can be placed in a plasma carburizing device, and the temperature of the plasma carburizing device can be set to place the cookware substrate at a predetermined preheating temperature. It should be noted that the preset temperature according to the present application can be set based on the thickness of the cookware substrate.
[0058] Hydrogen and Argon Bombardment Cleaning
[0059] In the ion carburizing equipment, it is necessary to clean the cookware substrate. Specifically, the cookware substrate can be cleaned by bombarding with hydrogen and argon. As an example, a mixed gas of hydrogen and argon is introduced into the ion carburizing equipment, and the pressure of the ion carburizing equipment is increased to 80Pa-100Pa. A plasma DC power supply is turned on, and a voltage of 200V-1500V is applied between the cathode and cathode to form a glow discharge. Then, hydrogen and argon are excited into an ion state, thereby bombarding and cleaning the surface of the cookware substrate. Through ion bombardment cleaning, oxides, oil stains and other impurities on the surface of the cookware substrate can be removed, providing a basis for the formation of a subsequent plasma carburized layer.
[0060] In some embodiments, the bombardment cleaning process may last for 5 minutes to 10 minutes to ensure that the surface of the cookware base is fully cleaned.
[0061] Plasma carburizing
[0062] According to the present application, carburizing gas is introduced, and during the plasma carburizing process, the carburizing gas decomposes and forms carbon ions, which are first adsorbed on the surface of the cookware substrate and then dissolved in the surface layer of the cookware substrate to form a solid solution. The formation of a solid solution is one of the key steps in the carburizing process, which enables carbon atoms to be evenly distributed inside the cookware substrate to form the form of a wear-resistant layer (first sublayer and second sublayer) according to the present application. When the adsorption rate of surface carbon ions is greater than the carburizing rate, that is, when the accumulation rate of carbon ions on the surface exceeds their diffusion rate to the inside, an amorphous layer (amorphous carbon layer) will be formed on the surface of the cookware substrate or the wear-resistant layer.
[0063] According to the present application, the plasma carburizing treatment includes a first stage and a second stage after the first stage. In the first stage, the main purpose is to form a wear-resistant layer at the surface layer of the cookware substrate with a preset depth. Specifically, in the first stage, a first flow rate of carburizing gas is introduced, so that the carburizing gas decomposes and forms carbon ions, and the supply speed of the carbon ions is less than the penetration speed of the carbon ions, so as to form a wear-resistant layer at the surface layer of the cookware substrate with a preset depth. In this way, the carbon ions have enough time to diffuse inward and evenly distribute on the surface of the cookware substrate, thereby ensuring that the carbon ions can fully and evenly penetrate into the surface layer of the cookware substrate in the first stage to promote the formation of the wear-resistant layer. As an example, the surface layer of the preset depth can be an area within a thickness range of 20μm-40μm from the surface of the cookware substrate.
[0064] In some embodiments, the first flow rate is 10 L / h-20 L / h, and the first flow rate of carburizing gas is introduced in a pulsed manner.
[0065] In these embodiments, a low flow rate of 10 L / h to 20 L / h is adopted, and a pulsed introduction method is used to control the supply speed of carbon ions to always be lower than the penetration speed of carbon ions, so that uniform and sufficient penetration of carbon ions into the surface layer of the cookware substrate can be achieved.
[0066] In some embodiments, the cookware base is controlled to contact with carbon ions under the conditions of a pressure of 80Pa-100Pa and a temperature of 500℃-700℃, and the first stage of carburizing is carried out under the conditions of a pressure of 80Pa to 100Pa and a temperature of 500℃ to 700℃. These conditions can form the diffusion motive force of carbon ions and affect the penetration speed of carbon ions, thereby controlling the supply speed of carbon ions to be always lower than the penetration speed of carbon ions, thereby ensuring the depth, rate and uniformity of carburizing.
[0067] According to the present application, after the first stage is completed, the carburizing gas is stopped and the temperature in the plasma carburizing equipment is reduced to 400°C-500°C. At this time, a part of the saturated solid solution carburized layer is precipitated in the form of carbides to form a wear-resistant layer.
[0068] According to the present application, the main factors affecting the thickness of the carburized layer are time and temperature. The higher the temperature, the faster the carburizing speed, the longer the time, and the thicker the carburized layer. In some embodiments, the duration of the first stage can be 4h-8h, and the temperature is 500℃-700℃, so that a wear-resistant layer with a thickness of 20μm-40μm can be formed. As an example, the surface layer of the cookware substrate has a high carbon concentration relative to the outside, and it first reaches a saturated state, and then continued carburizing and cooling will cause carbides to precipitate from the saturated solid solution of carbon and matrix metal. Therefore, the relative outside is a mixed layer of saturated solid solution and carbide, and the relative content of carbon ions in the inside is less than that in the outside, so a solid solution layer of carbon and matrix metal will be formed. More specifically, the wear-resistant layer 21 includes a first sublayer 211 located inside and a second sublayer 212 located outside, wherein the first sublayer is a solid solution layer of carbon and base metal, in contact with the cookware substrate, and the second sublayer is a mixed layer of a saturated solid solution of carbon and base metal and carbide, in contact with the amorphous carbon layer. The first sublayer 211 has a thickness of 15 μm-30 μm, and the second sublayer 212 has a thickness of 5 μm-15 μm.
[0069] Continuing with the above example, since the cookware substrate includes one of a pure iron substrate, a cast iron substrate, an aluminum substrate, a titanium substrate, a stainless steel substrate and a low-carbon steel substrate, in the wear-resistant layer formed in the present application, taking the pure iron substrate, the cast iron substrate and the low-carbon steel substrate as examples, the first sublayer is a solid solution layer of carbon and iron, which is in contact with the cookware base material, and the second sublayer is a mixed layer of a saturated solid solution of carbon and iron and iron carbide, which is in contact with the amorphous carbon layer.
[0070] Taking the stainless steel substrate as an example, the first sublayer is a solid solution layer of carbon and iron, which is in contact with the cookware base material, and the second sublayer is a mixed layer of a saturated solid solution of carbon and iron, chromium carbide and iron carbide, which is in contact with the amorphous carbon layer.
[0071] Taking the aluminum substrate as an example, the first sublayer is a solid solution layer of carbon and aluminum, which contacts the cookware substrate, and the second sublayer is a mixed layer of a saturated solid solution of carbon and aluminum and aluminum carbide, which contacts the amorphous carbon layer.
[0072] Taking the titanium substrate as an example, the first sublayer is a solid solution layer of carbon and titanium, which contacts the cookware substrate, and the second sublayer is a mixed layer of a saturated solid solution of carbon and titanium and titanium carbide, which contacts the amorphous carbon layer.
[0073] According to the present application, the plasma carburizing treatment also includes a second stage after the first stage, in which an amorphous carbon layer with interlayer gaps is constructed, and the amorphous carbon layer can improve the non-stick performance. Specifically, in the second stage, a second flow rate of carburizing gas is introduced, so that the carburizing gas decomposes and forms carbon ions, and the second flow rate is greater than the first flow rate or the plasma carburizing power of the second stage is greater than the plasma carburizing power of the carburizing parameters of the first stage, so as to form an amorphous carbon layer with interlayer gaps on the wear-resistant layer.
[0074] On the basis of the first stage, the second stage directly increases the supply of carbon ions by increasing the flux of carburizing gas, which can promote the adsorption and dissolution process of carbon ions on the surface of the cookware matrix and provide a more sufficient carbon source for the formation of the amorphous carbon layer.
[0075] As the supply of carbon ions increases, the adsorption rate of carbon ions on the substrate surface accelerates, thereby promoting the formation of surface solid solution. At the same time, due to the enrichment of carbon ions, when the surface carbon ion adsorption rate is greater than the carburizing rate, an amorphous amorphous carbon layer (amorphous carbon layer) will be formed on the surface. In addition, the increased carbon ion flux also helps to introduce more interlayer gaps in the formed amorphous carbon layer. These gaps provide space for the subsequent storage of grease or silicone oil, thereby further improving the non-stick properties of the cookware.
[0076] In addition, based on the first stage, the second stage can promote the formation and stability of plasma by increasing the carburizing power. As a key medium in the carburizing process, the quality and stability of plasma directly affect the activity of carbon ions and carburizing efficiency.
[0077] Compared with the first stage, the higher carburizing power can produce a more intense and stable plasma environment, making the movement of carbon ions in the plasma more intense and frequent. This high-intensity plasma environment helps to accelerate the interaction between carbon ions and the substrate surface, promotes carbon ion accumulation and forms an amorphous amorphous carbon layer with interlayer gaps. At the same time, the stable plasma can also reduce energy loss and unnecessary reactions during the carburizing process, thereby improving the carburizing efficiency. In the second stage, the increased carburizing power is combined with the increased carburizing gas flux, which can jointly promote the formation of an amorphous carbon layer with interlayer gaps and make the amorphous carbon layer more dense and uniform in structure.
[0078] In summary, the second stage, by adjusting the flux of carburizing gas and the plasma carburizing power, not only ensured the formation of amorphous carbon layer and the introduction of interlayer gaps, but also improved the carburizing efficiency and the surface properties of cookware.
[0079] In some embodiments, the carburizing gas can be a highly unsaturated acetylene gas, specifically, propylene, acetylene, propyne, etc. The second flow rate is 150L / h-300L / h, the plasma carburizing power of the second stage is 10KW-20KW, and the plasma carburizing power of the carburizing parameters of the first stage is 3KW-5KW.
[0080] In these embodiments, a high-flow, highly unsaturated acetylene gas is introduced as the carburizing gas. Under the influence of the plasma carburizing power in the second stage, the carburizing gas can be rapidly decomposed to form a high concentration of carbon ions, which impact the surface of the pure iron substrate to form an amorphous carbon layer (amorphous carbon film) with an interlayer structure and relatively dense.
[0081] According to the present application, the voltage in the reaction chamber can also be increased at the same time to increase the flying speed of the carbon ions, thereby enhancing the adhesion strength of the amorphous carbon layer.
[0082] In some embodiments, performing plasma carburizing on the cookware substrate having a rough structure further includes setting the voltage between the cathode and cathode of the plasma carburizing device to 200 V-1500 V. In a preferred embodiment, in the second stage, the voltage between the cathode and cathode of the plasma carburizing device is 1000 V-1500 V, so that the generation and maintenance of plasma can be enhanced, which is conducive to the rapid decomposition and deposition of carbon ions, thereby forming an amorphous carbon layer with a specific interlayer gap.
[0083] According to the present application, in the second stage, the temperature in the plasma carburizing equipment is 400°C-500°C. At low temperatures, carbon ions do not penetrate into the cookware matrix, and are non-directionally deposited on the wear-resistant layer to form an amorphous carbon layer with a specific interlayer gap.
[0084] In some embodiments, the duration of the second stage may be 6 h-10 h, thus, an amorphous carbon layer with a thickness of 5 μm-15 μm can be formed.
[0085] According to the present application, a phased plasma carburizing treatment method can construct a composite structure with excellent wear resistance on the surface of the cookware substrate by controlling parameters such as the flow rate of the carburizing gas, process conditions, and plasma carburizing power.
[0086] In the embodiment of the present application, during the plasma carburizing process, the carburizing gas may be a gas containing carbon elements, specifically, the carburizing gas may be at least one of methane, propane and acetylene. The carburizing gas can be decomposed into hydrogen ions, carbon ions and electrons under the action of the electric field to form a plasma. In the plasma, the potential from the anode to the cathode is basically the same in most areas, but a sharp voltage drop occurs near the cathode due to the release of a large number of electrons from the cathode. The voltage is the lowest and the charge density is the highest, so that the ions in the plasma are accelerated and collide with the cookware substrate.
[0087] The carbon ions collide with the surface of the cookware substrate and adhere to the surface and continue to diffuse inward, forming a wear-resistant layer (Fe3C, a solid solution of iron and carbon) on the surface of the cookware substrate. When the reaction continues, the penetration rate of the carbon ions decreases due to the decrease in temperature. The obstruction of the wear-resistant layer causes the surface cementite to reach the maximum thickness, and the excess carbon ions are enriched on the surface to form an amorphous non-crystalline carbon film, namely the amorphous carbon layer of the present application.
[0088] In these embodiments, the pressure of the plasma carburizing equipment can be 80Pa to 100Pa. Such a pressure range helps to maintain the stability and uniformity of the gas during the carburizing process. The cookware substrate is heated to 500°C to 700°C and is in contact with the carbon ions for 5h-10h. The appropriate temperature can accelerate the diffusion and penetration of the carbon ions, while avoiding excessively high temperatures that may reduce the performance of the cookware substrate (for example, reducing the strength of the pot body and making the pot body brittle). The carburizing treatment lasts for 5h-10h, which can ensure that the carbon ions fully penetrate the cookware substrate and form a wear-resistant layer and an amorphous carbon layer of sufficient thickness.
[0089] According to the present application, the plasma carburizing treatment of the cooker substrate also includes setting the voltage between the cathode and cathode of the plasma device to be 200V-1500V. Appropriate voltage setting can produce enough glow discharges, thereby forming high-energy plasma. These high-energy plasmas bombard the surface of the cooker substrate, which helps the diffusion and infiltration of carbon ions. Therefore, in the plasma carburizing treatment, the voltage setting between the cathode and cathode has a direct impact on the carburizing effect and the formation of the carburizing treatment layer. If the voltage is relatively low, (such as lower than 200V), it is not enough to produce enough plasma to drive the carburizing process. If the voltage is relatively high (such as higher than 1500V), it will cause energy waste or equipment damage.
[0090] In some embodiments, the carburizing gas is a carbon-containing gas. As an example, the carbon-containing gas can be a mixed gas of methane, propane and acetylene. It should be noted that the present application does not limit the volume ratio of each component in the mixed gas. As an example, methane, propane and acetylene can be (0.5-1): (0.5-1): (0.5-1). Continuing with the above example, the pressure of the ion carburizing equipment is set between 80Pa and 100Pa, so that the cooker substrate is under corresponding pressure conditions. In the step of plasma carburizing treatment, the carbon-containing gas of methane, propane and acetylene is passed, so that the cooker substrate is continuously contacted with carbon ions at 500°C to 700°C for 5h-10h, and the pressure of the ion carburizing equipment is maintained at 80-100Pa during this period. In this process, the carbon-containing gas decomposes under the action of high temperature and plasma, and forms a carburizing treatment layer on the surface of the cooker substrate.
[0091] cool down
[0092] In the cooling step, nitrogen is introduced to exhaust the carbon-containing gas in the plasma carburizing equipment, thereby avoiding the adverse effects of residual carbon-containing gas on the equipment. Turn off the plasma power supply and stop heating to avoid unnecessary energy waste and equipment loss. In this case, the cookware base will cool with the furnace. Cooling with the furnace can not only make the temperature of each part of the pot uniform during the cooling process, but also help to form a plasma carburized layer with a uniform and smooth organizational structure, and prevent the pot from deforming or cracking due to rapid cooling. When cooled to below 200°C, it can be taken out and cooled to room temperature, thereby obtaining the cookware according to the present application.
[0093] According to the present application, plasma carburizing treatment is performed on a cookware substrate having a rough structure to form a carburized layer including a wear-resistant layer and an amorphous carbon layer, wherein the wear-resistant layer is formed on the surface of the cookware substrate and has a concave-convex structure, and the amorphous carbon layer is formed on the concave-convex structure of the wear-resistant layer, and the amorphous carbon layer has an amorphous morphology and interlayer gaps, so that the amorphous carbon layer itself can have a certain non-stickiness due to its amorphousness, excellent self-lubricating effect and low surface energy, and can also have lasting non-stickiness due to being protected by the concave-convex structure of the wear-resistant layer.
[0094] According to the present application, the method for manufacturing cookware further includes placing the cookware substrate having the carburized layer in silicone oil or grease, so that the silicone oil and grease are filled into the carburized layer, specifically, into the interlayer gaps of the amorphous carbon layer.
[0095] In some embodiments, the silicone oil can be selected from at least one of methyl silicone oil, dimethyl silicone oil, hydroxy silicone oil, hydrogen silicone oil and polyether modified silicone oil. The above silicone oil has a specific viscosity and surface tension, and is easier to enter the pore structure of the carburized layer. Specifically, it is filled into the interlayer gap of the amorphous carbon layer. In addition, the silicone oil is adsorbed or bonded to the pore structure of the carburized layer. In addition, by weight percentage, the silicone oil includes 20%-30% of low molecular weight silicone oil, 40%-60% of medium molecular weight silicone oil, and 20%-30% of high molecular weight silicone oil, wherein the molecular weight of the low molecular weight silicone oil is between 500-1000, the molecular weight of the medium molecular weight silicone oil is between 3000-6000, and the molecular weight of the high molecular weight silicone oil is between 12000-30000.
[0096] In these embodiments, the silicone oil of high molecular weight is more firmly combined with the amorphous carbon layer, and the release speed is slower, the free mobility of the silicone oil of low molecular weight is better, so as to have better non-stickiness, and the silicone oil of medium molecular weight takes into account both free mobility and binding firmness. Therefore, by combining low molecular weight silicone oil, medium molecular weight silicone oil and high molecular weight silicone oil, on the one hand, the possibility of silicone oil entering the interlayer gap of the amorphous carbon layer is further increased, and on the other hand, silicone oils with different binding forces can be continuously released at each stage of use to exert a better non-stick effect. As an example, the binding force between silicone oil and the cooker substrate with carburized treatment layer is roughly 5MPa-10MPa. Such binding force can ensure the continuous release of silicone oil and avoid premature release or inability to release silicone oil.
[0097] According to the present application, after selecting the silicone oil, the silicone oil is used to impregnate the cookware substrate having the carburized layer, thereby obtaining a cookware in which the silicone oil is combined in the interlayer gap of the amorphous carbon layer. As an example, the silicone oil can be impregnated into the non-stick coating for 2h-3h at a temperature of 80°C-100°C.
[0098] According to a second aspect of the present application, a cooker is provided, wherein the cooker is manufactured by the method for manufacturing the cooker provided in each of the above embodiments.
[0099] In some embodiments, the cookware includes a cookware substrate 10 and a carburized layer 20 formed on the cookware substrate 10 . Figure 2 A schematic structural diagram of a cooker provided according to an embodiment of the present application is shown. Figure 3 Shows Figure 2 The local enlarged schematic diagram of point I in the figure. Figure 2 and Figure 3As shown, the cookware includes a cookware substrate 10 and a carburized layer 20 formed on the cookware substrate 10, the carburized layer 20 includes an amorphous carbon layer 22 located on the outside and a wear-resistant layer 21 located inside the amorphous carbon layer 22, the wear-resistant layer 21 contacts the cookware substrate 10, and has a concavo-convex structure on the surface, the amorphous carbon layer 22 is formed on the concavo-convex structure of the wear-resistant layer 21, has an interlayer gap, and serves as the surface layer of the cookware. In the amorphous carbon layer, carbon is in a disordered lamellar structure, and as an example, the interlayer spacing is between 0.3nm and 10nm.
[0100] In the embodiment of the present application, the cookware substrate 10 is a portion of the cookware base 100 that is not carbonized, the wear-resistant layer 21 is a carbonized surface area of the cookware base 100, and the amorphous carbon layer 22 is a carbon accumulation layer formed on the wear-resistant layer 21 to form a layered structure.
[0101] According to the cookware provided in the embodiment of the present application, the amorphous morphology and interlayer gap structure of the amorphous carbon layer enable the cookware to exhibit excellent non-stick properties when used for the first time. The amorphous carbon layer is located on the outside of the wear-resistant layer and is formed on the concave-convex structure of the wear-resistant layer. The wear-resistant layer has high hardness and wear resistance, and can protect the amorphous carbon layer located in the depressions of the concave-convex structure, so that the amorphous carbon layer is not easily worn due to use, ensuring that it is not easy to lose its non-stick properties during later use. As the use time increases, the grease or silicone oil stored in the interlayer gaps of the amorphous carbon layer can continue to play a role and maintain the lasting non-stick properties of the cookware. Therefore, the cookware according to the present application can have both better initial non-stick properties and lasting non-stick properties.
[0102] In some embodiments, the wear-resistant layer 21 includes a first sublayer 211 located inside and a second sublayer 212 located outside, the first sublayer 211 is a solid solution layer of carbon and matrix metal, in contact with the cookware substrate 10, and the second sublayer 212 is a mixed layer of a saturated solid solution of carbon and matrix metal and carbides, in contact with the amorphous carbon layer 22. Here, the saturated solid solution of carbon and matrix metal means that the solubility of carbon in the matrix metal has reached the limit, and the carbide is the compound precipitated and generated from the saturated solid solution of carbon and matrix metal as mentioned above. The second sublayer in the form of a mixed layer as above not only inherits the high hardness and strength of the saturated solid solution, but also further improves the wear resistance and corrosion resistance of the surface layer through the generation of carbides.
[0103] In these embodiments, the first sublayer is a solid solution layer. As the inner sublayer of the wear-resistant layer, the first sublayer not only ensures the bonding strength between the wear-resistant layer and the substrate, but also ensures the hardness and strength of the wear-resistant layer due to the formation of the solid solution, thereby improving the wear resistance of the cooker, so that the cooker can resist wear and scratches during use. The second sublayer is the outer sublayer of the wear-resistant layer. The second sublayer is directly in contact with the amorphous carbon layer. Its high hardness and high wear resistance can protect the amorphous carbon layer from wear, and its surface characteristics can ensure the bonding strength between the wear-resistant layer and the amorphous carbon layer. In addition, the presence of carbides in the second sublayer can also have a positive effect on the formation and performance of the amorphous carbon layer. For example, carbides, as hard phases, can enhance the overall structural strength of the amorphous carbon layer with their high hardness and wear resistance. This enhanced structural stability helps to better carry and fix lubricating substances such as grease or silicone oil to prevent them from being easily squeezed out or lost during use. Therefore, the presence of carbides improves the durability and reliability of the amorphous carbon layer as a lubricating surface.
[0104] According to the present application, the concavo-convex structure of the wear-resistant layer 21 is, as an example, formed by a plurality of convex hulls, the spacing between adjacent convex hulls is 0.2 mm-0.5 mm, the height of the convex hulls is 15 μm-50 μm, and the width of the convex hulls is 0.2 mm-0.5 mm. In a preferred embodiment, the thickness of the amorphous carbon layer is not greater than the roughness value of the concavo-convex structure. The concavo-convex structure with such roughness can make most of the amorphous carbon layer formed in the concave part of the concavo-convex structure of the wear-resistant layer. In this way, the wear-resistant layer can provide protection for the amorphous carbon layer during the cooking process to optimize the long-lasting non-stickiness.
[0105] In some embodiments, the thickness of the cookware substrate is 1.5 mm-2.0 mm, the thickness of the wear-resistant layer is 20 μm-40 μm, and the thickness of the amorphous carbon layer is 5 μm-15 μm. Continuing with the above example, the thickness of the wear-resistant layer is 20 μm-40 μm, and the wear-resistant layer 21 includes a first sublayer 211 and a second sublayer 212, wherein the thickness of the first sublayer 211 is 15 μm-30 μm, and the thickness of the second sublayer 212 is 5 μm-15 μm.
[0106] In these embodiments, each layer has a certain thickness distribution, which can balance the factors of non-stickiness, wear resistance and manufacturing cost of the cookware, thereby improving the overall performance of the cookware.
[0107] In some embodiments, the amorphous carbon layer is oleophilic and has a surface energy of 15 dynes to 25 dynes, which can improve the non-stick performance of the cookware.
[0108] In some embodiments, the cookware substrate includes one of a pure iron substrate, a cast iron substrate, an aluminum substrate, a titanium substrate, a stainless steel substrate and a low-carbon steel substrate. There are many types of substrates for forming the cookware, which can facilitate the manufacture of multiple types of cookware according to actual needs.
[0109] In some embodiments, the interlayer gaps of the amorphous carbon layer are filled with grease or silicone oil to further improve the non-stick performance of the cookware.
[0110] The present application will be described in detail below in conjunction with embodiments, but the protection scope of the present application is not limited to the embodiments.
[0111] Example 1
[0112] The non-stick cookware according to Example 1 was prepared by the following method.
[0113] Step S10, providing a pure iron substrate with a thickness of 1.8 mm and a surface roughness of 100 μm as a cookware substrate.
[0114] Step S20, after the cookware base is loaded into the plasma carburizing equipment, the plasma carburizing equipment is evacuated to a low vacuum state (0.5 Pa) by a vacuum pump.
[0115] Step S30, preheating at a preheating temperature of 550°C for 20 minutes to activate atoms on the surface layer of the cookware substrate.
[0116] Step S40, a mixture of hydrogen and argon is introduced into the plasma carburizing equipment, and the pressure in the plasma carburizing equipment is increased to 90 Pa. A plasma DC power supply is turned on, and a voltage of 200-1500V is applied between the cathode and cathode to form a glow discharge to bombard and clean the surface of the cookware substrate.
[0117] Step S50, replace the gas introduced into the plasma carburizing equipment with an alkane gas mixed with methane, propane and acetylene in a volume ratio of 1:1:1, and set the flow rate of the alkane gas to 15L / h. The alkane gas used as a carburizing gas can be decomposed into hydrogen ions, carbon ions and electrons under the action of the electric field. The cookware substrate is controlled to be in contact with the carbon ions under a pressure of 90Pa and a temperature of 600°C for 6h. During this period, the pressure in the plasma carburizing equipment is maintained at 90Pa to form a wear-resistant layer with a thickness of 30μm on the surface of the cookware substrate.
[0118] Step S60, setting the flow rate of the alkane gas to 200L / h. The alkane gas as a carburizing gas can be decomposed into hydrogen ions, carbon ions and electrons under the action of the electric field. The cookware substrate is controlled to be in contact with the carbon ions at a pressure of 80Pa-100Pa and a temperature of 450°C for 8h. During this period, the pressure in the plasma carburizing equipment is maintained at 90Pa to form an amorphous carbon layer with a thickness of 10μm on the surface of the cookware substrate.
[0119] Step S70, nitrogen is introduced to exhaust the carbon-containing gas in the plasma carburizing equipment, thereby preventing the residual carbon-containing gas from causing adverse effects on the plasma carburizing equipment. The power supply of the plasma carburizing equipment is turned off, and heating is stopped to avoid unnecessary energy waste and equipment loss. In this case, the cookware base will cool with the furnace, and when it cools to below 200° C., the cookware can be taken out, thereby obtaining the cookware of Example 1 having the above-mentioned carburized layer.
[0120] Example 2
[0121] The cookware of Example 2 was prepared by the same method as that of Example 1, except that in step S50, the thickness of the wear-resistant layer of the carburized layer was set to 20 μm.
[0122] Example 3
[0123] The cookware of Example 3 was prepared by the same method as that of Example 1, except that in step S50, the thickness of the wear-resistant layer of the carburized layer was set to 40 μm.
[0124] Example 4
[0125] The cookware of Example 4 was prepared by the same method as that of Example 1, except that in step S60, the thickness of the amorphous carbon layer of the carburized layer was set to 5 μm.
[0126] Example 5
[0127] The cookware of Example 5 was prepared by the same method as that of Example 1, except that in step S60, the thickness of the amorphous carbon layer of the carburized layer was set to 15 μm.
[0128] Example 6
[0129] The cookware of Example 6 was prepared by the same method as that of Example 1, except that in step S10, the pure iron substrate was replaced by a cast iron substrate.
[0130] Example 7
[0131] The cookware of Example 7 is prepared by the same method as that of Example 1, except that in step S10, the pure iron substrate is replaced by a low-carbon steel substrate.
[0132] Example 8
[0133] The cookware of Example 8 was prepared in the same manner as in Example 1, except that in step S10, the pure iron substrate was replaced with an aluminum substrate.
[0134] Example 9
[0135] The cookware of Example 9 is prepared by the same method as that of Example 1, except that in step S10, the pure iron substrate is replaced by a titanium substrate.
[0136] Example 10
[0137] The cookware of Example 10 was prepared in the same manner as in Example 1, except that in step S10, the pure iron substrate was replaced with stainless steel.
[0138] Embodiment 11
[0139] The cookware of Example 11 is prepared in the same manner as in Example 1, except that step S80 is added after step S70, ie, the cookware with the carburized layer is immersed in silicone oil at 90° C. for 2.5 hours.
[0140] Example 12
[0141] The cookware of Example 12 is prepared in the same manner as in Example 1, except that step S70 is added after step S70, i.e., the cookware having the carburized layer is immersed in edible oil at 90° C. for 2.5 hours.
[0142] Example 13
[0143] The cookware of Example 13 was prepared in the same manner as in Example 1, except that in step S10, a pure iron substrate having a thickness of 1.8 mm and a surface roughness of 60 μm was provided.
[0144] Embodiment 14
[0145] The cookware of Example 14 was prepared in the same manner as in Example 1, except that in step S10, a pure iron substrate having a thickness of 1.8 mm and a surface roughness of 200 μm was provided.
[0146] Comparative Example 1
[0147] In addition to using conventional carburizing to form a carburized layer (without dividing into stages, only controlling the cookware base to contact with the carbon ions generated by the carburizing gas under the conditions of a pressure of 80Pa-100Pa and a temperature of 500℃-700℃ for 8 hours, during which the pressure in the plasma carburizing equipment is maintained at 90Pa), the cookware of Comparative Example 1 is prepared by the same method as that of Example 1.
[0148] Comparative Example 2
[0149] The cookware of Comparative Example 2 was prepared in the same manner as in Example 1, except that in step S10, an iron substrate having a thickness of 1.8 mm and a surface roughness of 50 μm was provided.
[0150] Comparative Example 3
[0151] The cookware of Comparative Example 3 was prepared in the same manner as in Example 1, except that in step S10, an iron substrate having a thickness of 1.8 mm and a surface roughness of 250 μm was provided.
[0152] Comparative Example 4
[0153] The cookware of Comparative Example 4 was prepared by plasma spraying conventional iron carbide on the pure iron substrate of Example 1 to form a coating with a thickness of 40 μm.
[0154] Performance index test
[0155] The non-stick effects of the coatings of the cookware of Examples 1-14 and Comparative Examples 1-4 were tested and recorded in Table 1 below. The specific performance test method is as follows:
[0156] ① Initial non-stickiness test method: GB / T32095.2-2015 fried egg non-stickiness test method. This method is an initial non-stickiness test, which is divided into levels Ⅰ, Ⅱ, and Ⅲ. Level Ⅰ has the best non-stickiness and level Ⅲ has the worst non-stickiness.
[0157] ② Long-lasting non-stick test method: The long-lasting non-stick test method in GB / T32388-2015, the unit is the number of times, the higher the number, the longer the life, the non-stick result is evaluated once every 500 times, and the number of times when it is used to level III is recorded.
[0158] Table 1 Performance index test data of the embodiments of the present application and the comparative examples
[0159]
[0160] In summary, according to the cookware of the present application, the thicker the wear-resistant layer, the higher the hardness, the better the long-term non-stick property; the thicker the surface amorphous carbon layer, the better the long-term non-stick property; the higher the surface roughness, the better the long-term non-stick property; but beyond a certain range, the internal amorphous carbon layer cannot contact the food and will instead make the long-term non-stick property poor.
[0161] Although the embodiments of the present application have been described in detail above, those skilled in the art may make various modifications and variations to the embodiments of the present application without departing from the spirit and scope of the present application. However, it should be understood that, in the opinion of those skilled in the art, these modifications and variations will still fall within the spirit and scope of the embodiments of the present application defined by the claims.
Claims
1. A cooking utensil, characterized in that: The cookware comprises a cookware substrate and a carburized layer formed on the cookware substrate, wherein the carburized layer comprises: A wear-resistant layer, in contact with the cookware base material, and having a concave-convex structure on the surface; An amorphous carbon layer is formed on the concavo-convex structure of the wear-resistant layer, has interlayer gaps and serves as a surface layer of the cooker.
2. The cooker according to claim 1, characterized in that: The wear-resistant layer includes a first sublayer located inside and a second sublayer located outside. The first sublayer is a solid solution layer in contact with the cookware substrate, and the second sublayer is a mixed layer of a saturated solid solution of carbon and iron and carbide in contact with the amorphous carbon layer.
3. The cooker according to claim 1, characterized in that: The thickness of the cookware substrate is 1.5 mm-2.0 mm; and / or the thickness of the wear-resistant layer is 20 μm-40 μm, and / or the thickness of the amorphous carbon layer is 5 μm-15 μm.
4. The cooker according to claim 1, characterized in that: The amorphous carbon layer is oleophilic, and the surface energy of the amorphous carbon layer is 15 to 25 dynes; and / or the cookware substrate includes one of an iron substrate, a cast iron substrate, an aluminum substrate, a titanium substrate, a stainless steel substrate and a low-carbon steel substrate; and / or the surface roughness of the concave-convex structure is 60μm-200μm.
5. The cooker according to any one of claims 1 to 4, characterized in that: The interlayer gap is filled with grease or silicone oil.
6. A method for manufacturing a cooker, characterized in that: The method for manufacturing a cooker comprises: Plasma carburizing treatment is performed on a cookware substrate having a rough structure to form a carburized layer including a wear-resistant layer and an amorphous carbon layer, wherein the wear-resistant layer is formed on the surface of the cookware substrate and has a concave-convex structure on the surface, and the amorphous carbon layer is formed on the concave-convex structure of the wear-resistant layer, has interlayer gaps, and serves as the surface layer of the cookware.
7. The method according to claim 6, characterized in that The plasma carburizing treatment includes a first stage, in which a first flow rate of carburizing gas is introduced so that the carburizing gas decomposes and forms carbon ions, and the supply speed of the carbon ions is smaller than the penetration speed of the carbon ions, so as to form the wear-resistant layer at the surface layer of the cookware substrate with a preset depth.
8. The method according to claim 7, characterized in that The plasma carburizing treatment also includes a second stage, in which a second flow rate of carburizing gas is introduced so that the carburizing gas decomposes and forms carbon ions, and the second flow rate is greater than the first flow rate or the plasma carburizing power of the second stage is greater than the plasma carburizing power of the carburizing parameters of the first stage, so as to form the amorphous carbon layer with the interlayer gap on the wear-resistant layer.
9. The method according to claim 7, characterized in that: The first flow rate is 10 L / h-20 L / h, and the carburizing gas of the first flow rate is introduced in a pulsed manner.
10. The method according to claim 9, characterized in that The cookware base is controlled to contact with the carbon ions under the conditions of a pressure of 80Pa-100Pa and a temperature of 700°C-800°C, so that the supply speed of the carbon ions is lower than the penetration speed of the carbon ions.
11. The method according to claim 8, characterized in that The second flow rate is 150L / h-300L / h, the plasma carburizing power of the second stage is 10KW-20KW, the plasma carburizing power of the carburizing parameters of the first stage is 3KW-5KW; and / or the temperature of the second stage is 400℃-500℃.
12. The method according to claim 6, characterized in that The plasma carburizing treatment of the cookware substrate having the rough structure further includes setting the voltage between the cathode and anode of the plasma carburizing device to 200V-1500V.
13. The method according to claim 6, characterized in that Before the plasma carburizing treatment, the cookware substrate is preheated at a temperature of 480° C. to 600° C. to activate atoms of the surface layer of the cookware substrate.
14. The method according to claim 6, characterized in that The surface roughness of the rough structure of the cookware base is 60 μm-200 μm.
15. The method according to claim 6, characterized in that The method for manufacturing the cookware further includes placing the cookware substrate having the carburized layer in silicone oil or grease, so that the silicone oil and grease are filled into the carburized layer.