Method for extracting selenium from lead-copper-zinc heavy metal smelting acid mud
Through wet low-temperature vulcanization slurry regulation and vacuum distillation technology, combined with the use of adsorbent, the problems of low selenium extraction efficiency and impurities in the smelting acid sludge in the prior art are solved, and efficient and environmentally friendly selenium extraction is achieved The effect improves the utilization rate and purity of selenium resources.
Patent Information
- Application Number
- CN202411209514.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art has problems such as complex processes, high energy consumption, and hazardous waste when extracting selenium from lead, copper, zinc and heavy metal smelting acid sludge, which is difficult to effectively improve the extraction efficiency and purity of selenium, especially when the selenium content is low. .
The wet low-temperature vulcanization slurry adjustment method is adopted, and the vulcanizing agent and adsorbent are added and heated, followed by vacuum distillation. Through the combination of vulcanization and adsorbent, selenium is effectively separated and purified, reducing the volatility of impurities, and improving the purity and yield of selenium.
It has achieved efficient extraction of selenium from lead, copper, zinc and heavy metal smelting acid sludge, with selenium purity reaching more than 99.5%, and the direct yield of selenium reaches 87.62%, effectively reducing the impurity content of mercury and lead. It has simple process and environmentally friendly and reduced production costs. .
Abstract
Description
Technical Field
[0001] The invention relates to a method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud, belonging to the technical field of extracting scattered metals. Background Art
[0002] Selenium is a rare metal element with an important strategic position and is widely used in the fields of electronics, chemicals, medicine, and health care. In industry, selenium is usually recovered comprehensively from selenium-containing slags such as copper electrolysis anode mud, acid mud from sulfuric acid plants, and smoke from lead and zinc smelting. However, the existing selenium extraction technology has disadvantages such as complex processes, generation of hazardous waste products during the process, and high energy consumption, which to a certain extent hinder the extraction, purification, and large-scale application of selenium. Therefore, how to extract selenium from the recovered selenium-containing acid mud in a green and efficient manner is of great significance for improving the utilization rate of selenium resources and reducing production costs.
[0003] The occurrence state of each element in the acid mud of lead, copper and zinc heavy metal smelting is very complex. It usually contains compounds or elements such as lead sulfate, lead sulfite, lead sulfide, lead selenide, mercury selenide, elemental selenium, elemental mercury, tellurium dioxide, and elemental tellurium. The target element selenium usually exists in the form of selenium compounds. It is difficult to obtain a good recovery effect by distillation and volatilization alone. Different elements or the same elements exist in different forms, and their physical and chemical properties are different or similar. This makes it difficult for us to recover the valuable elements in the acid mud.
[0004] Chinese patent CN115449637A discloses a method for extracting selenium, copper and tellurium from copper anode mud by high-efficiency stepwise separation. The method processes raw materials such as copper anode mud or materials containing copper telluride. The mass percentage of each element in the copper anode mud is Cu (5% to 40%), Te (0.5% to 10%), Se (0.5% to 10%), Pb (1% to 10%) and Ag (2% to 15%). The raw material is roasted at 600°C for 3 hours using O2-SO2 to separate selenium to obtain roasted sand and selenium-enriched material, and the selenium volatilization rate reaches 98.46%. This method is a pyrolysis roasting method to extract selenium, which has high energy consumption and involves harmful gas SO2.
[0005] Chinese patent CN116875800A discloses a method for extracting lead, selenium, copper and mercury by leaching and stepwise separation from acid mud. The method processes acid mud produced in the process of copper smelting acid production, and the main components of the acid mud are: Pb (30.61%), Cu (12.58%), Se (15.72%), Hg (4.32%), Zn (1.17%), Sb (0.1%), Bi (1.93%), As (0.93%), Te (0.16%), and Ag (0.11%). The method adopts the process of "sulfuric acid + sodium chlorate oxidation synergistic leaching - hydrochloric acid + sodium sulfite reduction selenium precipitation", which involves strong oxidants such as sulfuric acid and sodium chlorate, and has the problems of equipment corrosion and high reagent cost.
[0006] Chinese patent CN113716532A discloses a method for removing impurity mercury from crude selenium. The raw materials of the method are crude selenium with a mass fraction of 90% to 97%, a mass fraction of Hg of 3200ppm, and a mass fraction of Pb of 2% to 2.5%. The following method is used to extract selenium: a sulfiding agent is added to the crude selenium slag crushed to less than 200 meshes, and the mixture is uniformly mixed and pressed into blocks to obtain a mixed material. The mixed material is placed in a closed furnace and heated and sulfided under an inert atmosphere. The sulfided selenium slag is vacuum distilled, and selenium enters the gas phase and is collected in the form of volatiles, generating mercury sulfides and valuable elements enriched in the residue. Then, in order to further remove mercury, the obtained selenium is subjected to secondary distillation. The final direct selenium recovery rate of the method is greater than 98%, and the mercury removal rate is greater than 99.8%. The method is a full-fire method for extracting selenium, which has a good effect on the purification of crude selenium, but has a poor effect on extracting selenium from raw materials with a low selenium content. After one distillation, the selenium content can be increased from 10.22% to 76.21%. Summary of the invention
[0007] In order to extract selenium from lead, copper and zinc heavy metal smelting acid mud with low selenium content, the present invention provides a method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud, and the specific steps are as follows:
[0008] (1) Wet low-temperature sulfurization slurry preparation: Add sulfurizing agent and adsorbent to the aqueous lead, copper and zinc heavy metal smelting acid mud, mix evenly and heat to obtain a sulfurized product.
[0009] (2) The sulfidation product obtained in step (1) is dried and then subjected to vacuum distillation, and the condensate on the condensation plate after distillation is the obtained selenium product with high purity.
[0010] Preferably, the mass fraction of Se in the lead, copper and zinc heavy metal smelting acid mud is 10% to 20%, the mass fraction of Hg is 2% to 5%, the mass fraction of Pb is 30% to 40%, and the rest are other components.
[0011] Preferably, in step (1), the mass ratio of lead, copper and zinc heavy metal smelting acid mud to sulfidizing agent is (5-20):1.
[0012] Preferably, the vulcanizing agent in step (1) is elemental sulfur, ferrous disulfide or sodium sulfide.
[0013] Preferably, in step (1), the mass ratio of lead, copper and zinc heavy metal smelting acid mud to adsorbent is (8-15):1.
[0014] Preferably, the adsorbent in step (1) is sodium carbonate or silicon dioxide.
[0015] Preferably, in step (1), the heating temperature is 20 to 60° C. and the heating time is 30 to 60 min.
[0016] Preferably, the drying temperature in step (2) is 50 to 80° C., and the drying time is 12 to 24 hours.
[0017] Preferably, the temperature of the vacuum distillation in step (2) is 240-350° C., the insulation time is 1-2 h, and the pressure is below 10 Pa.
[0018] Beneficial effects of the present invention
[0019] (1) Adding adsorbent to the raw material to adsorb part of the lead sulfide and mercury sulfide impurities that decompose during the distillation process to prevent the volatilization of impurities from affecting the selenium extraction efficiency and product selenium purity.
[0020] (2) The method of the present invention can be used to extract selenium from lead, copper and zinc heavy metal smelting acid mud containing 10.22% selenium and make the selenium purity reach more than 99.5%, the direct selenium recovery rate reaches 87.62%, and the mercury and lead contents in the crude selenium product are reduced from 2.83% and 36.0% in the raw material to 0.139% and 0.111%, and the removal rates can reach 98.5% and 99.96%, respectively.
[0021] (3) The wet sulfidation reaction is more complete in the sulfidation stage of the present invention, and the adsorbent is used in the distillation process to react with residual heavy metal ions such as lead and mercury to form mercury salts and lead salts to further remove heavy metals such as lead and mercury, so that selenium in the acid mud is separated.
[0022] (4) This method is simple, efficient and environmentally friendly, and can be widely used in the recovery and utilization of selenium in lead, copper and zinc heavy metal smelting acid mud, thereby improving the utilization rate of selenium resources and reducing production costs. It has broad market prospects and application value. DETAILED DESCRIPTION
[0023] The technical solution of the present invention is further described below by specific implementation methods. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0024] The lead-copper-zinc heavy metal smelting acid mud used in all embodiments has a mass fraction of Se of 10.22%, a mass fraction of Hg of 2.83%, a mass fraction of Pb of 36.0%, and the rest are other components.
[0025] Example 1
[0026] A method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud comprises the following steps:
[0027] (1) Wet low-temperature sulfurization slurry preparation: Take 24.30 g of water-containing lead, copper and zinc heavy metal smelting acid mud, add 2.43 g of sulfur according to the mass ratio of lead, copper and zinc heavy metal smelting acid mud raw material to sulfurizing agent of 10:1, add 3.07 g of adsorbent sodium carbonate, then mix the slurry and stir evenly, put the beaker containing the slurry into a 50°C water bath and heat it for 40 min.
[0028] (2) After the vulcanization is completed, the slurry in the beaker is poured out to a drying tray, and the drying tray is placed in an 80°C drying oven for drying for 12 hours. After the drying is completed, the drying tray is taken out, and the agglomerated material is taken out and made into a block that can be placed in a crucible. The material is placed in a crucible, and then the crucible containing the material is placed in a vacuum furnace for distillation. The temperature is increased to 300°C at a heating rate of 10°C / min, and then the vacuum is evacuated to below 10Pa for vacuum distillation. The temperature is kept for 1 hour, and the distillation is terminated. After the furnace is cooled, the furnace cover is opened to collect volatiles and residues, and the weight is recorded. The condensate on the condensation tray is the target crude selenium product, and the residue in the crucible can be used as a raw material for refining rare and precious metals.
[0029] It is measured by ICP-AES and chemical titration that the purity of the obtained crude selenium can reach 99.62%, the Se direct recovery rate can reach 93.86%, the Hg removal rate can reach more than 99%, and the Pb removal rate can reach more than 99.9%.
[0030] Example 2
[0031] A method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud comprises the following steps:
[0032] (1) Wet low-temperature sulfurization slurry preparation: Take 24.30 g of water-containing lead, copper and zinc heavy metal smelting acid mud, add 4.86 g of ferrous disulfide according to the mass ratio of acid mud raw material to sulfurizing agent of 5:1, add 3.50 g of adsorbent silicon dioxide, then mix the slurry and stir evenly, put the beaker containing the slurry into a 50°C water bath and heat it for 40 min.
[0033] (2) After the vulcanization is completed, the slurry in the beaker is poured out to a drying tray, and the drying tray is placed in an 80°C drying oven for drying for 12 hours. After the drying is completed, the drying tray is taken out, and the agglomerated material is taken out and made into a block that can be placed in a crucible. The material is placed in a crucible, and then the crucible containing the material is placed in a vacuum furnace for distillation. The temperature is increased to 300°C at a heating rate of 10°C / min, and then the vacuum is evacuated to below 10Pa for vacuum distillation. The temperature is kept for 1 hour, and the distillation is terminated. After the furnace is cooled, the furnace cover is opened to collect volatiles and residues, and the weight is recorded. The condensate on the condensation tray is the target crude selenium product, and the residue in the crucible can be used as a raw material for refining rare and precious metals.
[0034] It is measured by ICP-AES and chemical titration that the purity of the obtained crude selenium can reach more than 99.5%, the Se direct recovery rate can reach 98.52%, the Hg removal rate can reach more than 99.5%, and the Pb removal rate can reach 99.96%.
[0035] Example 3
[0036] A method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud comprises the following steps:
[0037] (1) Wet low-temperature sulfurization slurry preparation: Take 24.30 g of water-containing lead, copper and zinc heavy metal smelting acid mud, add 1.62 g of sodium sulfide, that is, potassium sulfide, according to the mass ratio of acid mud raw material to sulfurizing agent of 15:1, add 3.50 g of adsorbent sodium carbonate, and then mix the slurry evenly, and put the beaker containing the slurry into a 50°C water bath and heat it for 40 minutes.
[0038] (2) After the vulcanization is completed, pour the slurry in the beaker into a drying tray, put the drying tray into an 80°C drying oven for drying for 12 hours, take out the drying tray after drying, take out the agglomerated material and make it into a block that can be put into a crucible, put the material into the crucible, and then put the crucible containing the material into a vacuum furnace for distillation. After heating to 300°C at a heating rate of 10°C / min, evacuate to below 10Pa for vacuum distillation, keep warm for 1 hour, and end the distillation. After the furnace cools down, open the furnace cover to collect volatiles and residues and weigh and record them. The condensate on the condensation tray is the target crude selenium product, and the residue in the crucible can be used as a raw material for rare and precious metal refining.
[0039] It is measured by ICP-AES and chemical titration that the purity of the obtained crude selenium can reach more than 99%, the Se direct recovery rate can reach 87.62%, the Hg removal rate can reach more than 99%, and the Pb removal rate can reach 99.8%.
[0040] Comparative Example 1
[0041] A method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud comprises the following steps:
[0042] (1) Take 24.30 g of hydrous lead, copper and zinc heavy metal smelting acid mud and put it on a drying tray. Put the drying tray into a drying oven at 80°C and dry it for 12 hours.
[0043] (2) After drying, the drying plate was removed, the agglomerated material was removed and crushed to less than 200 mesh, 1.62 g of sulfur was added to the raw material as a vulcanizing agent according to a mass ratio of raw material to vulcanizing agent of 15:1, the mixture was evenly mixed and briquetted to obtain a mixed material, the material was placed in a crucible, and the total weight of the crucible and the material was recorded.
[0044] (3) The crucible is placed in a vacuum furnace, and the temperature is raised to 150°C at a heating rate of 10°C / min in an inert gas atmosphere for a sulfidation reaction of 60 minutes to obtain a sulfidation product. The sulfidation product is directly subjected to vacuum distillation. After the sulfidation is completed, the furnace temperature is cooled to room temperature, and then the temperature is raised to 300°C at a heating rate of 10°C / min, and then the vacuum is evacuated to below 10Pa for vacuum distillation. The temperature is kept for 1 hour to end the distillation. After the furnace is cooled, the furnace cover is opened to collect volatiles and residues, and the weight is recorded. The condensate on the condensation plate is the target crude selenium product, and the residue in the crucible can be used as a raw material for rare and precious metal refining.
[0045] The results of ICP-AES and chemical titration showed that the purity of the crude selenium was 76.21%, the direct recovery rate of Se was 84.35%, the removal rate of Hg was 86.91%, and the removal rate of Pb could reach 99.97%.
[0046] By comparison, it can be seen that the method of the present application is more effective in extracting selenium from lead, copper, and zinc heavy metal smelting acid mud. In the sulfidation stage, wet sulfidation is used to make the impurity elements contact more fully with the sulfiding agent and react more completely. Adsorbents are added to the material to react with heavy metal ions such as lead and mercury to form corresponding salts that are less volatile, thereby reducing the volatilization of lead and mercury, and making the content of volatilized impurities lower, thereby achieving the purpose of improving product purity and reducing impurity content. Therefore, the extraction effect of this method is better.
[0047] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud, characterized in that: The specific steps include: (1) Wet low-temperature sulfurization slurry preparation: Add sulfurizing agent and adsorbent to the aqueous lead, copper and zinc heavy metal smelting acid mud, mix evenly and heat to obtain a sulfurized product; (2) The sulfidation product obtained in step (1) is dried and then subjected to vacuum distillation, and the condensate on the condensation plate after distillation is the obtained selenium product with high purity.
2. The method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud according to claim 1, characterized in that: The mass fraction of Se in the lead, copper and zinc heavy metal smelting acid mud is 10% to 20%, the mass fraction of Hg is 2% to 5%, the mass fraction of Pb is 30% to 40%, and the rest are other components.
3. The method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud according to claim 1, characterized in that: In step (1), the mass ratio of aqueous lead, copper and zinc heavy metal smelting acid mud to the sulfidizing agent is (5-20):
1.
4. The method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud according to claim 1, characterized in that: The sulfiding agent in step (1) is sulfur, ferrous disulfide or potassium sulfide.
5. The method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud according to claim 1, characterized in that: In step (1), the mass ratio of water-containing lead, copper and zinc heavy metal smelting acid mud to adsorbent is (8-15):
1.
6. The method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud according to claim 1, characterized in that: The adsorbent in step (1) is sodium carbonate or silicon dioxide.
7. The method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud according to claim 1, characterized in that: In step (1), the heating temperature is 20 to 60° C. and the heating time is 30 to 60 min.
8. The method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud according to claim 1, characterized in that: The drying temperature in step (2) is 50 to 80° C. and the drying time is 12 to 24 hours.
9. The method for extracting selenium from lead, copper and zinc heavy metal smelting acid mud according to claim 1, characterized in that: The temperature of the vacuum distillation in step (2) is 240-350° C., the insulation time is 1-2 hours, and the pressure is below 10 Pa.
Citation Information
Patent Citations
Method for producing low-impurity crude selenium from mercury-acid-sludge-containing oxygen pressure alkali leaching liquid
CN106542507A
Method for removing impurity mercury from crude selenium
CN113716532A