Colored release film and preparation method thereof
By applying a colored release agent layer on the transparent polyester film, the problem of difficult to distinguish the colorless release film is solved, visual monitoring and real-time quality control of the colored release film are realized, and the detection process is simplified.
Patent Information
- Application Number
- CN202311649745.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-04
- Publication Date
- 2024-12-06
AI Technical Summary
Existing release films are usually colorless, making it difficult to visually distinguish whether the release film is applied during use, and it is difficult to intuitively detect release residues, requiring additional complex testing for quality control.
Using a color release film, by applying a release agent layer containing colored pigments on the transparent polyester film base layer, the release agent layer can be visualized by using colored pigments, so that the release agent residue or the release agent can be observed through the human eye. Fog phenomenon, real-time monitoring and quality control.
It realizes the direct monitoring of the quality of the release film through visual means, reduces the need for complex testing, can correct residual errors in a timely manner, and improves the efficiency of product quality control.
Smart Images

Figure BDA0004586999490000051 
Figure BDA0004586999490000061
Abstract
Description
Technical Field
[0001] The present application relates to the field of chemical technology, in particular to the field of thin film material technology in the chemical industry, and more particularly to a colored release film and a preparation method thereof. Background Art
[0002] Release film is a kind of film material commonly used in the chemical industry. Release film is also called peeling film, isolation film, separation film, etc. It is a kind of film with separation properties on the surface. Release film is not sticky or slightly sticky after contacting with specific materials under limited conditions. Release film is widely used in packaging, printing, silk screen printing, pad printing, nameplates, membrane switches, flexible circuits, insulation products, circuit boards, laser anti-counterfeiting, lamination, electronics, sealing material films, reflective materials, waterproof materials, medicine (plaster paper), toilet paper, adhesive products, die-cutting and punching processing and other industries.
[0003] CN 112375437 B discloses a release film substrate, comprising a polyester film and a washcoat, wherein the washcoat is formed on the surface of the polyester film, and a silicone oil release agent is coated on the surface of the washcoat to form a release agent layer; the washcoat comprises the following components: 80-100 parts by weight of acrylic resin, 1-2 parts by weight of dimethyl silylate silica, 10-15 parts by weight of ethanolamine, 0.5-0.8 parts by weight of polyquaternary ammonium salt, 5-10 parts by weight of non-water-soluble carbonate, 1-2 parts by weight of melamine, and 80-100 parts by weight of propylene glycol. The porous hydrophilic washcoat formed on the surface of the polyester film of the prior art greatly improves the surface activity and hydrophilicity of the release film substrate, is conducive to close combination with the silicone oil release agent, and can prevent the release agent from detaching.
[0004] CN 112661995 B discloses a release film for polarizer, comprising a release film substrate and a release agent layer coated on the surface of the release film substrate, wherein the release agent layer is made of a UV-curable release agent prepared from the following raw materials in parts by weight: 60-140 parts by weight of polybutadiene polyurethane, 45-85 parts by weight of polyacrylate resin, 10-25 parts by weight of hydroxypropyl methacrylate, 25-55 parts by weight of trifluoroethyl methacrylate active monomer diluent, 25-55 parts by weight of octadecyl methacrylate active monomer diluent, and 1-5 parts by weight of an initiator of 2-hydroxy-2-methyl-1-phenyl-1-propanone. The UV-curable release agent of the prior art is a UV-curable release agent without silicone oil component, does not require high-temperature baking, has no silicone oil seepage, and eliminates the phenomenon that the PAS glue is pulled up due to the transfer of silicone oil component.
[0005] The release films in the prior art are usually colorless and transparent, and it is sometimes difficult to distinguish whether the release film is applied to the product.
[0006] CN 219544202 U discloses a blue PE double-sided release film, comprising a nano-scale carbon sponge layer and a blue PE film arranged on both sides of the nano-scale carbon sponge layer, a transparent film is arranged on the side of the blue PE film on both sides away from the nano-scale carbon sponge layer, a corona layer is arranged on the side of the transparent film away from the blue PE film, a release layer is arranged on the corona layer, and the release layer is a UV curing nano-mixture coated on the corona layer. The release film substrate of the prior art adopts a blue PE film, which can be easily identified by color.
[0007] Blue PE film is almost the most common film in the film field. Because PE is easily oxidized and turns blue, in order to keep the PE film colorless, it is necessary to add antioxidants to it to delay oxidation. Therefore, the price of colorless PE film is usually higher than that of blue. In short, the general impression is that the quality of blue PE film is worse than that of colorless PE film.
[0008] Except for the blue PE film, the films of other materials are usually colorless. Therefore, to prepare a colored release film, pigments are usually added to the film as the base material, so that the base film presents different colors. For example, the colored release films on the market are usually prepared from base films of various colors such as yellow, red, green, blue, and gray.
[0009] In the field of electronic product technology, the use of adhesive bonding is becoming more and more common. It is also common to bond release films of different colors on the surface of the adhesive layer to distinguish different surfaces. For example, CN 116023866 A discloses a highly weather-resistant ultra-thin adhesive sticker that is easy to attach, including a blue release film, AB glue and a transparent release film arranged in sequence from top to bottom, and the two opposite sides of the AB glue are both sticky. The blue release film used in the prior art is easy to remove quickly when used later.
[0010] As mentioned above, the release film in the prior art is generally colorless, and the color of the colored release film comes from the dyeing of the release film substrate. However, since the release agent on the surface of the release film substrate is generally colorless, it is difficult to distinguish whether the release agent remains after the colored release film is removed.
[0011] For example, CN 113155822 A discloses a method for testing the anti-fogging performance of a silicone release agent, including weighing a sample to be tested, covering with paper, stirring the sample, curing the release agent, dyeing the cover paper, and comparing the dyed sample with a standard sample, thereby intuitively obtaining the anti-fogging performance result of the test sample. The cover paper used in the prior art is a plant fiber material paper, and the dye used for dyeing is a dye that can color the fiber, such as Shirlastain A fiber identification agent or malachite green dye, etc. The working principle of the prior art is that under a suitable stirring state, the silicone release agent will form an aerosol that overflows from the liquid surface and is adsorbed on the cover paper of the stirring container, and the cover paper adsorbed with the cured release agent is used for dyeing, because the silicone release agent and the paper fiber will show different colors when encountering the dye, thereby obtaining the amount of release agent on the cover paper and reflecting the quality of the anti-fogging performance of the measured sample.
[0012] It can be seen from the prior art that the release agent is difficult to observe and distinguish in an intuitive way, and requires additional complex processes for prior testing. However, even if a release agent that meets the composite quality requirements can be obtained, the residue of the release agent is still difficult to distinguish during actual use, and quality control can only be carried out through testing. Summary of the invention
[0013] The technical problem to be solved by the present application is to provide a colored release film and a preparation method thereof, so as to reduce or avoid the above-mentioned problems.
[0014] In order to solve the above technical problems, the present application proposes a colored release film, comprising a substrate layer and a release agent layer, wherein the substrate layer is made of a transparent polyester film with a single-layer or multi-layer structure, the release agent layer is made of a colored release agent added with a colored pigment, and the colored release agent is made of the following components in parts by weight: 100-200 parts by weight of polyurethane acrylate, 60-80 parts by weight of 6(ethoxy)trimethylolpropane triacrylate, 20-40 parts by weight of diacetone alcohol, 30-50 parts by weight of tridecafluorooctyl acrylate, 2.5-4.5 parts by weight of a solid particle mixture of modified pigments, and 3-5 parts by weight of benzophenone.
[0015] Preferably, the color pigment is an alkali-resistant inorganic pigment that has been surface-modified.
[0016] Preferably, the inorganic pigment is red iron oxide, cadmium sulfide, ultramarine blue or a mixture thereof.
[0017] The present application also proposes a method for preparing a colored release film, comprising the following steps: uniformly mixing a mixture of 100-200 parts by weight of polyurethane acrylate, 60-80 parts by weight of 6(ethoxy)trimethylolpropane triacrylate, 20-40 parts by weight of diacetone alcohol, 30-50 parts by weight of tridecafluorooctyl acrylate, and 2.5-4.5 parts by weight of a solid particle mixture of a surface-modified modified pigment, adding 3-5 parts by weight of benzophenone, and magnetically stirring for 120-240 seconds to obtain a release agent; uniformly coating the release agent on the surface of a substrate layer with a thickness of 12-100 μm, vacuum defoaming for 1-2 hours, and curing under N2 conditions by ultraviolet light irradiation for 180-300 seconds to form a release agent layer, and the thickness of the release agent layer is measured to be 0.5-2 μm.
[0018] Preferably, the preparation method further comprises a surface modification treatment step of the modified pigment: adding 10-20 parts by weight of an inorganic pigment to 100-200 parts by weight of a polyvinyl alcohol aqueous solution, and continuously stirring for 60-120 minutes to fully disperse; then adding 6-8 parts by weight of sodium tripolyphosphate and continuing to stir for 60-120 minutes to fully mix to obtain a dispersed mixture; finally, subjecting the dispersed mixture to freeze-drying spray to obtain a solid particle mixture of the modified pigment with a surface modified treatment.
[0019] The colored release film of the present application can observe the colored release agent layer from the outside through the transparent substrate layer, so that the color can be visually felt, and the release agent residue or the fogging of the release agent can be observed by the human eye, so the quality of the release film can be intuitively obtained, and real-time monitoring can be achieved and residual errors can be corrected in time. DETAILED DESCRIPTION
[0020] In order to have a clearer understanding of the technical features, purposes and effects of the present application, the specific implementation methods of the present application will be described in detail below.
[0021] In view of the technical problems described in the background technology, the present application proposes a colored release film, comprising a substrate layer and a release agent layer, wherein the substrate layer is made of a transparent polyester film of a single-layer or multi-layer structure, and the release agent layer is made of a colored release agent added with a colored pigment.
[0022] The use of a transparent substrate layer makes it easy to observe the colored release agent layer from the outside, so that the color can be visually felt. If the substrate layer is not transparent, the color cannot be seen, and there is no so-called colored release film. In addition, the use of colored release agents can observe the release agent residue or the fogging of the release agent through the human eye, so there is no need to arrange complex tests in advance to intuitively obtain the quality of the release film, and can achieve real-time monitoring and timely correction of residual errors, which is of great help in real-time control of product quality.
[0023] In a specific embodiment of the present application, the thickness of the substrate layer is 12-100 μm, and the thickness of the release agent layer is 0.5-2 μm.
[0024] In another specific embodiment of the present application, the colored release agent is prepared from the following components in parts by weight: 100-200 parts by weight of polyurethane acrylate, 60-80 parts by weight of 6(ethoxy)trimethylolpropane triacrylate, 20-40 parts by weight of diacetone alcohol, 30-50 parts by weight of tridecafluorooctyl acrylate, 2.5-4.5 parts by weight of a solid particle mixture of modified pigments, and 3-5 parts by weight of benzophenone.
[0025] The modified pigment is preferably an inorganic pigment that has been surface-modified, such as one of alkali-resistant inorganic pigments such as red iron oxide, cadmium sulfide, ultramarine, or a mixture thereof. Although inorganic pigments are not as bright in color as organic pigments, they are cheap and easy to obtain. Moreover, inorganic pigments are relatively easier to disperse and are easy to maintain their original color after surface modification. In addition, alkali-resistant inorganic pigments are easy to change color after oxidation, making it easy to identify whether the release film is falling off or deteriorating.
[0026] Furthermore, the surface modification treatment step of the modified pigment includes: adding 10-20 parts by weight of inorganic pigment to 100-200 parts by weight of polyvinyl alcohol aqueous solution, stirring continuously for 60-120 minutes to fully disperse; then adding 6-8 parts by weight of sodium tripolyphosphate and stirring continuously for 60-120 minutes to fully mix to obtain a dispersed mixture; finally, freeze-drying and spraying the dispersed mixture to obtain a solid particle mixture of the modified pigment with surface modification treatment. The content of polyvinyl alcohol in the polyvinyl alcohol aqueous solution is 10wt%-15wt%.
[0027] Example 1
[0028] 100 parts by weight of polyurethane acrylate, 60 parts by weight of 6 (ethoxy) trimethylolpropane triacrylate, 20 parts by weight of diacetone alcohol, 30 parts by weight of octyl tridecafluoroacrylate, and 2.5 parts by weight of a surface-modified solid particle mixture (iron oxide red) were uniformly mixed, 3 parts by weight of benzophenone were added, and magnetic stirring was performed for 120 seconds to obtain a release agent. The release agent was uniformly coated on the surface of a substrate layer with a thickness of 12 μm, vacuum defoamed for 1 hour, and cured by ultraviolet light under N2 conditions for 180 seconds to form a release agent layer, and the thickness of the release agent layer was measured to be 0.5 μm.
[0029] Comparative Example 1
[0030] The release film was prepared by the same process as in Example 1, except that 6 (ethoxy) trimethylolpropane triacrylate was removed from the release agent component, and the contents of other components were adjusted. The specific components were: 140 parts by weight of polyurethane acrylate, 20 parts by weight of diacetone alcohol, 50 parts by weight of tridecafluorooctyl acrylate, 2.5 parts by weight of a modified pigment solid particle mixture (iron oxide red), and 3 parts by weight of benzophenone.
[0031] Example 2
[0032] 150 parts by weight of polyurethane acrylate, 70 parts by weight of 6 (ethoxy) trimethylolpropane triacrylate, 30 parts by weight of diacetone alcohol, 40 parts by weight of octyl tridecafluoroacrylate, and 3.0 parts by weight of a surface-modified solid particle mixture (cadmium sulfide) were uniformly mixed, 4 parts by weight of benzophenone were added, and magnetic stirring was performed for 180 seconds to obtain a release agent. The release agent was uniformly coated on the surface of a substrate layer with a thickness of 50 μm, vacuum defoamed for 1.5 hours, and cured under N2 conditions by ultraviolet light for 240 seconds to form a release agent layer, and the thickness of the release agent layer was measured to be 1 μm.
[0033] Comparative Example 2
[0034] The release film was prepared by the same process as in Example 2, except that diacetone alcohol was removed from the release agent component, and the contents of other components were adjusted. The specific components were: 170 parts by weight of polyurethane acrylate, 80 parts by weight of 6 (ethoxy) trimethylolpropane triacrylate, 40 parts by weight of acrylate tridecafluorooctyl ester, 3.0 parts by weight of a surface-modified solid particle mixture (cadmium sulfide), which were uniformly mixed, and 4 parts by weight of benzophenone were added.
[0035] Example 3
[0036] 200 parts by weight of polyurethane acrylate, 80 parts by weight of 6 (ethoxy) trimethylolpropane triacrylate, 40 parts by weight of diacetone alcohol, 50 parts by weight of acrylate tridecafluorooctyl ester, and 4.5 parts by weight of a surface-modified solid particle mixture (ultramarine) were uniformly mixed, 5 parts by weight of benzophenone were added, and magnetic stirring was performed for 240 seconds to obtain a release agent. The release agent was uniformly coated on the surface of a substrate layer with a thickness of 100 μm, vacuum defoamed for 2 hours, and cured by ultraviolet light under N2 conditions for 300 seconds to form a release agent layer, and the thickness of the release agent layer was measured to be 2 μm.
[0037] Comparative Example 3
[0038] The release film was prepared by the same process as in Example 3, except that 13-fluorooctyl acrylate was removed from the release agent component, and the contents of other components were adjusted. The specific components were: 230 parts by weight of polyurethane acrylate, 90 parts by weight of 6 (ethoxy) trimethylolpropane triacrylate, 50 parts by weight of diacetone alcohol, 4.5 parts by weight of a surface-modified solid particle mixture (ultramarine) were uniformly mixed, and 5 parts by weight of benzophenone was added.
[0039] The parameter performances of the above embodiments and comparative examples are shown in the following table.
[0040]
[0041] Examples 4-6 and Comparative Examples 4-6
[0042] The components of the modified pigments of Examples 1-3 were adjusted and tested for performance. The weight parts of the components of the modified pigments of Examples 4-6 and Comparative Examples 4-6 are shown in the following table.
[0043] Among them, comparative example 4 does not use polyvinyl alcohol aqueous solution, so it cannot be prepared by dispersion spraying, but only fully mixes iron oxide red and sodium tripolyphosphate into a solid particle mixture. Comparative example 5 does not add sodium tripolyphosphate, and comparative example 6 reduces the amount of polyvinyl alcohol and sodium tripolyphosphate. The particle size of the inorganic pigment is selected to be 10-15nm.
[0044] Through the aforementioned modification process, a solid particle mixture was prepared and applied to the release films of Examples 1 to 3, respectively. Among them, Example 4 and Comparative Example 4 were used for the release film of Example 1, Example 5 and Comparative Example 5 were used for the release film of Example 2, and Example 6 and Comparative Example 6 were used for the release film of Example 3.
[0045] The color distribution uniformity of the release films of Examples 4-6 and Comparative Examples 4-6 was tested respectively, and the index was the average density of color spots per 10 square centimeters (pieces / 10cm 2 ), wherein the values of Examples 4-6 are all less than 0.1, and the values of Comparative Examples 4-6 are 8.6, 5.4, and 2.3, respectively. Among them, the pigment dispersion of Comparative Example 4 is not good enough, and the agglomeration is more serious. The colors of Comparative Examples 5 and 6 are obviously lighter than those of Examples 5 and 6, and the color of Comparative Example 5 is almost colorless, and the reason is unknown.
[0046] Those skilled in the art should understand that although the present application is described in the form of multiple embodiments, not every embodiment contains only one independent technical solution. Such description in the specification is only for the sake of clarity, and those skilled in the art should understand the specification as a whole and regard the technical solutions involved in each embodiment as being able to be combined into different embodiments to understand the scope of protection of the present application.
[0047] The above description is only an illustrative embodiment of the present application and is not intended to limit the scope of the present application. Any equivalent changes, modifications and combinations made by any technician in the field without departing from the concept and principle of the present application shall fall within the scope of protection of the present application.
Claims
1. A colored release film, comprising a substrate layer and a release agent layer, It is characterized in that The substrate layer is made of a transparent polyester film with a single-layer or multi-layer structure, the release agent layer is made of a color release agent added with color pigments, and the color release agent is made of the following components in parts by weight: 100-200 parts by weight of polyurethane acrylate, 60-80 parts by weight of 6 (ethoxy) trimethylolpropane triacrylate, 20-40 parts by weight of diacetone alcohol, 30-50 parts by weight of tridecafluorooctyl acrylate, 2.5-4.5 parts by weight of a solid particle mixture of modified pigments, and 3-5 parts by weight of benzophenone.
2. The colored release film according to claim 1, It is characterized in that The color pigment is an alkali-resistant inorganic pigment that has been surface-modified.
3. The colored release film according to claim 2, It is characterized in that The inorganic pigment is red iron oxide, cadmium sulfide, ultramarine blue or a mixture thereof.
4. A method for preparing a colored release film as claimed in any one of claims 1 to 3, comprising the following steps: uniformly mixing 100-200 parts by weight of polyurethane acrylate, 60-80 parts by weight of 6 (ethoxy) trimethylolpropane triacrylate, 20-40 parts by weight of diacetone alcohol, 30-50 parts by weight of tridecafluorooctyl acrylate, and 2.5-4.5 parts by weight of a solid particle mixture of a surface-modified modified pigment, adding 3-5 parts by weight of benzophenone, and magnetically stirring for 120-240 seconds to obtain a release agent; uniformly coating the release agent on the surface of a substrate layer having a thickness of 12-100 μm, vacuum defoaming for 1-2 hours, N 2 The film was cured by ultraviolet light for 180-300 seconds under the given conditions to form a release agent layer. The thickness of the release agent layer was measured to be 0.5-2 μm.
5. The preparation method as claimed in claim 4 further comprises a surface modification treatment step of the modified pigment: adding 10-20 parts by weight of the inorganic pigment to 100-200 parts by weight of a polyvinyl alcohol aqueous solution, stirring continuously for 60-120 minutes to fully disperse; then adding 6-8 parts by weight of sodium tripolyphosphate and continuing stirring for 60-120 minutes to fully mix to obtain a dispersed mixture; finally, subjecting the dispersed mixture to freeze-drying spray to obtain a solid particle mixture of the modified pigment with surface modification treatment.
Citation Information
Patent Citations
Antibacterial release film with small release force
CN106243371A
Addition type solvent silicon oil mold release agent and application thereof
CN109762466A
Preparation method of color powdered ink
CN109946932A
Antistatic UV curing release agent and preparation method thereof
CN113234400A
Light-cured release film with low volume shrinkage and aging resistance and preparation process thereof
CN116769211A