Environment-friendly flame-retardant waterproof cold-proof material adhesive and preparation method thereof

By using polymer emulsion, flame retardant and auxiliary agent in environmentally friendly flame retardant and waterproof cold-proof adhesives, combined with stirring treatment and silicone slip agent, the glue brushing problem is solved, and the product smoothness and bonding strength are improved. Improved production efficiency.

CN119081588AInactive Publication Date: 2024-12-06QINGDAO MINGJUFU IND PRODUCTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411423883.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing environmentally friendly flame retardant, water-resistant and cold-proof glue is prone to wire drawing when used, resulting in unsmoothing and uneven product surfaces, reducing bonding strength, affecting aesthetics and user experience, and significantly reducing production efficiency and increasing production costs.

Method used

Using environmentally friendly flame retardant and waterproof cold-proof adhesive composed of polymer emulsion, flame retardant, filler and additive, polyvinyl alcohol solution is added through raw material preparation, mixing ingredients, stirring and secondary mixing steps, and stirring is added and stirred. Add silicone slip agent during the process to ensure that the components are fully mixed and reduce the occurrence of wire drawing.

Benefits of technology

It effectively reduces the occurrence of wire drawing, makes the product surface smoother and more uniform, avoids the problem of reduced bonding strength, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081588A_ABST
    Figure CN119081588A_ABST
Patent Text Reader

Abstract

The invention discloses an environment-friendly flame-retardant water-resistant cold-proof material adhesive which comprises an environment-friendly flame-retardant water-resistant cold-proof adhesive body, and the environment-friendly flame-retardant water-resistant cold-proof adhesive body is composed of polymer emulsion, a flame retardant, a filler and an auxiliary agent; the polymer emulsion comprises a polyvinyl acetate emulsion, an acrylate emulsion and a polyurethane emulsion, the flame retardant comprises aluminum hydroxide, a hydroxide powder flame retardant and a phosphorus flame retardant, the filler comprises aluminum oxide, silicon dioxide and nano aluminum oxide, and the auxiliaries comprise a dispersing agent, a thickening agent, an antioxidant and polyvinyl alcohol. According to the environment-friendly flame-retardant water-resistant cold-proof material adhesive, five steps of raw material preparation, material mixing, stirring treatment, secondary mixing and mixing completion are set, and a polyvinyl alcohol solution is added in the steps, so that the wire drawing phenomenon of the flame-retardant water-resistant cold-proof material adhesive is effectively reduced, the surface of a product is smoother and more uniform, and the quality of the product is improved. And the problem that the bonding degree of glue is reduced is avoided, so that the production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesive processing, and in particular to an environmentally friendly flame-retardant, water-resistant and cold-proof material adhesive and a preparation method thereof. Background Art

[0002] As we all know, environmentally friendly flame retardant, water-resistant and cold-proof glue has mechanical properties such as high bonding strength, good flexibility, high impact resistance, and not easy to crack, and has good temperature resistance, water resistance, chemical resistance, and weather resistance. It can be widely used in the bonding between railway passenger car aluminum plates and cold-proof materials, as well as in other building decorations and decorations; in addition, the glue is non-toxic, pollution-free, and odor-free, and is suitable for the composite of various fabrics and sponges, aluminum foil composite glass fiber cloth, composite cloth fabrics, etc.

[0003] However, when the environmentally friendly, flame-retardant, water-resistant and cold-proof glue of the prior art is used, wiredrawing problems will inevitably occur due to factors such as too fast dispensing speed and the inability to accurately control the distance between the needle and the working surface. The wiredrawing phenomenon will cause the product surface to become rough and uneven, thereby affecting the product's aesthetics and user experience; in addition, wiredrawing may also reduce the bonding strength of the glue, causing the product to easily fall off or separate during use; more importantly, the wiredrawing phenomenon will significantly reduce production efficiency and increase production costs; for this reason, we propose an environmentally friendly, flame-retardant, water-resistant and cold-proof material adhesive and a preparation method thereof. Summary of the invention

[0004] The purpose of the present invention is to provide an environmentally friendly flame retardant, water-resistant and cold-proof material adhesive and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] An environmentally friendly flame retardant, water-resistant and cold-proof material bonding adhesive comprises an environmentally friendly flame retardant, water-resistant and cold-proof adhesive body, wherein the environmentally friendly flame retardant, water-resistant and cold-proof adhesive body is composed of a polymer emulsion, a flame retardant, a filler and an auxiliary agent.

[0007] Preferably, the polymer emulsion includes polyvinyl acetate emulsion, acrylate emulsion, polyurethane emulsion, the flame retardant includes aluminum hydroxide, hydroxide powder flame retardant, phosphorus flame retardant, the filler includes alumina, silica, nano alumina, and the additives include dispersants, thickeners, antioxidants and polyvinyl alcohol.

[0008] In addition, the present invention also provides a method for preparing an environmentally friendly flame retardant, water resistant and cold-proof material adhesive, comprising the following steps:

[0009] Step 1, raw material preparation, the polyvinyl acetate emulsion, acrylic emulsion, polyurethane emulsion, aluminum hydroxide, hydroxide powder flame retardant, phosphorus flame retardant, aluminum oxide, silicon dioxide, nano aluminum oxide, dispersant, thickener, antioxidant, polyvinyl alcohol and modified graphite, titanium dioxide, fumed silica and silane coupling agent required for the preparation of the environmentally friendly flame retardant water-resistant cold-proof adhesive body are prepared;

[0010] Step 2, mixing ingredients, polyvinyl acetate emulsion, acrylic emulsion, polyurethane emulsion, aluminum hydroxide, hydroxide powder flame retardant, phosphorus flame retardant, aluminum oxide, silicon dioxide, nano aluminum oxide, dispersant, thickener, antioxidant, polyvinyl alcohol and modified graphite, titanium dioxide, fumed silica and silane coupling agent are mixed in a certain proportion, the specific proportion is polyvinyl acetate emulsion accounts for 38-50 weight percent, acrylic emulsion accounts for 5-8 weight percent, polyurethane emulsion accounts for 5-8 weight percent, aluminum hydroxide accounts for 4-6 weight percent, Hydroxide powder flame retardant accounts for 6-10 weight percent, phosphorus flame retardant accounts for 5-8 weight percent, aluminum oxide accounts for 3-6 weight percent, silicon dioxide accounts for 3-6 weight percent, nano aluminum oxide accounts for 3-6 weight percent, dispersant accounts for 3-6 weight percent, thickener accounts for 1-3 weight percent, antioxidant accounts for 1-3 weight percent, polyvinyl alcohol accounts for 1-3 weight percent, modified graphite accounts for 1-5 weight percent, titanium dioxide accounts for 1-5 weight percent, fumed silica accounts for 1-3 weight percent, and silane coupling agent accounts for 1-3 weight percent;

[0011] Step 3: Take out the polyvinyl alcohol and store it separately, then stir the remaining mixed ingredients to ensure that the various components can be fully mixed, and the stirring speed of the stirring equipment is maintained at 160-190 revolutions per minute.

[0012] Step 4: Take out the polyvinyl alcohol solution with a good ratio and pour it into the stirred mixture for secondary mixing. Use a stirring device to mix for 10-20 minutes.

[0013] Step 5: Add the organosilicon slip agent to the secondary mixed material and stir it for 15-25 minutes. At this time, the environmentally friendly flame retardant, water-resistant and cold-proof adhesive body is prepared.

[0014] Preferably, in step one, the silane coupling agent is a chemical agent, the silane alkoxy groups it contains are reactive to inorganic substances, and the organic functional groups are reactive or compatible to organic substances, so when the silane coupling agent is located between the inorganic and organic interfaces, a bonding layer of organic matrix-silane coupling agent-inorganic matrix can be formed.

[0015] Preferably, in step 2, the mixing of various raw materials is mainly carried out by using a laboratory planetary mixer. After the power is turned on, the raw materials entering the mixer can be efficiently stirred and mixed.

[0016] Preferably, in step three, the stirring time of the raw materials by the stirring equipment is 20-40 minutes.

[0017] Preferably, in step 4, polyvinyl alcohol needs to be stored in a cool, ventilated warehouse, away from fire and heat sources, and should be stored separately from oxidants. Mixing should not be allowed. In addition, fire-fighting equipment of corresponding types and quantities should be equipped, and suitable materials should be available in the storage area to contain leaks to ensure that the components of polyvinyl alcohol will not be damaged before use.

[0018] Preferably, in step five, the organosilicon slip agent is specifically an organosiloxane emulsion, which is mainly divided into anionic, cationic and non-ionic types, is widely used in various coating systems, and has a durable slippery feel.

[0019] In summary, the present application includes at least one of the following beneficial technical effects:

[0020] The environmentally friendly flame retardant, water resistant and cold proof material adhesive is set up through five steps of raw material preparation, mixing ingredients, stirring treatment, secondary mixing and completing mixing, and polyvinyl alcohol solution is added in the steps, thereby effectively reducing the occurrence of wire drawing phenomenon of the flame retardant, water resistant and cold proof material adhesive, making the product surface smoother and more uniform, and avoiding the problem of reduced bonding strength of the glue, thereby improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic structural diagram of the environmentally friendly flame retardant, water resistant and cold-proof material adhesive of the present invention;

[0022] Figure 2 The present invention is a schematic flow chart of a method for preparing an environmentally friendly flame-retardant, water-resistant and cold-proof material adhesive.

[0023] In the picture: 1. Environmentally friendly flame retardant, water-resistant and cold-proof rubber body. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Embodiment 1

[0026] See also Figure 1-Figure 2This embodiment provides a technical solution: an environmentally friendly flame retardant, water-resistant and cold-proof material bonding adhesive, including: an environmentally friendly flame retardant, water-resistant and cold-proof adhesive body, the environmentally friendly flame retardant, water-resistant and cold-proof adhesive body is composed of a polymer emulsion, a flame retardant, a filler and an additive.

[0027] Preferably, the polymer emulsion includes polyvinyl acetate emulsion, acrylate emulsion, polyurethane emulsion, the flame retardant includes aluminum hydroxide, hydroxide powder flame retardant, phosphorus flame retardant, the filler includes alumina, silica, nano alumina, and the additives include dispersants, thickeners, antioxidants and polyvinyl alcohol.

[0028] In addition, this embodiment also provides a method for preparing an environmentally friendly flame retardant, water resistant and cold-proof material adhesive, comprising the following steps:

[0029] Step 1, raw material preparation, the polyvinyl acetate emulsion, acrylic emulsion, polyurethane emulsion, aluminum hydroxide, hydroxide powder flame retardant, phosphorus flame retardant, aluminum oxide, silicon dioxide, nano aluminum oxide, dispersant, thickener, antioxidant, polyvinyl alcohol and modified graphite, titanium dioxide, fumed silica and silane coupling agent required for the preparation of the environmentally friendly flame retardant water-resistant cold-proof adhesive body are prepared;

[0030] Step 2, mixing ingredients, polyvinyl acetate emulsion, acrylic emulsion, polyurethane emulsion, aluminum hydroxide, hydroxide powder flame retardant, phosphorus flame retardant, aluminum oxide, silicon dioxide, nano aluminum oxide, dispersant, thickener, antioxidant, polyvinyl alcohol and modified graphite, titanium dioxide, fumed silica and silane coupling agent are mixed in a certain proportion, the specific proportion being 50 weight percent of polyvinyl acetate emulsion, 5 weight percent of acrylic emulsion, 5 weight percent of polyurethane emulsion, 4 weight percent of aluminum hydroxide, 6 weight percent of hydroxide powder flame retardant, 5 weight percent of phosphorus flame retardant, 3 weight percent of aluminum oxide, 3 weight percent of silicon dioxide, 3 weight percent of nano aluminum oxide, 3 weight percent of dispersant, 1 weight percent of thickener, 1 weight percent of antioxidant, 1 weight percent of polyvinyl alcohol, 5 weight percent of modified graphite, 1 weight percent of titanium dioxide, 1 weight percent of fumed silica, and 2 weight percent of silane coupling agent;

[0031] Step 3: Take out the polyvinyl alcohol and store it separately, then stir the remaining mixed ingredients to ensure that all components can be fully mixed, and keep the stirring speed of the stirring equipment at 160 revolutions per minute.

[0032] Step 4: Take out the polyvinyl alcohol solution with a good ratio and pour it into the stirred mixture for secondary mixing. Use a stirring device to mix for 10 minutes.

[0033] Step 5: Add the organosilicon slip agent to the secondary mixed material and stir it for 15 minutes. At this time, the environmentally friendly flame retardant, water-resistant and cold-proof adhesive body is prepared.

[0034] It should be noted that: in step 1, the silane coupling agent is a chemical agent, the silane oxy group contained in it is reactive to inorganic substances, and the organic functional group is reactive or compatible to organic substances. Therefore, when the silane coupling agent is between the inorganic and organic interfaces, a bonding layer of organic matrix-silane coupling agent-inorganic matrix can be formed; in step 2, the mixing of various raw materials is mainly processed by a laboratory planetary mixer. After the power is turned on, the raw materials entering the mixer can be efficiently stirred and mixed; in step 3, the mixing equipment is used to mix the raw materials. The stirring time is 20 minutes; in step 4, polyvinyl alcohol needs to be stored in a cool, ventilated warehouse, away from fire and heat sources, and should be stored separately from oxidants, and mixed storage is strictly prohibited. In addition, fire-fighting equipment of corresponding types and quantities needs to be equipped, and suitable materials should be available in the storage area to contain leaks to ensure that the components of polyvinyl alcohol will not be damaged before use; in step 5, the organosilicon slip agent is specifically an organosiloxane emulsion, which is mainly divided into anionic, cationic and non-ionic types, is widely used in various coating systems, and has a more durable slippery feel.

[0035] Embodiment 2

[0036] See also Figure 1-Figure 2 This embodiment provides a technical solution: an environmentally friendly flame retardant, water-resistant and cold-proof material bonding adhesive, including: an environmentally friendly flame retardant, water-resistant and cold-proof adhesive body, the environmentally friendly flame retardant, water-resistant and cold-proof adhesive body is composed of a polymer emulsion, a flame retardant, a filler and an additive.

[0037] Preferably, the polymer emulsion includes polyvinyl acetate emulsion, acrylate emulsion, polyurethane emulsion, the flame retardant includes aluminum hydroxide, hydroxide powder flame retardant, phosphorus flame retardant, the filler includes alumina, silica, nano alumina, and the additives include dispersants, thickeners, antioxidants and polyvinyl alcohol.

[0038] In addition, this embodiment also provides a method for preparing an environmentally friendly flame retardant, water resistant and cold-proof material adhesive, comprising the following steps:

[0039] Step 1, raw material preparation, the polyvinyl acetate emulsion, acrylic emulsion, polyurethane emulsion, aluminum hydroxide, hydroxide powder flame retardant, phosphorus flame retardant, aluminum oxide, silicon dioxide, nano aluminum oxide, dispersant, thickener, antioxidant, polyvinyl alcohol and modified graphite, titanium dioxide, fumed silica and silane coupling agent required for the preparation of the environmentally friendly flame retardant water-resistant cold-proof adhesive body are prepared;

[0040] Step 2, mixing ingredients, polyvinyl acetate emulsion, acrylic emulsion, polyurethane emulsion, aluminum hydroxide, hydroxide powder flame retardant, phosphorus flame retardant, aluminum oxide, silicon dioxide, nano aluminum oxide, dispersant, thickener, antioxidant, polyvinyl alcohol and modified graphite, titanium dioxide, fumed silica and silane coupling agent are mixed in a certain proportion, and the specific proportion is polyvinyl acetate emulsion accounting for 38 weight percent, acrylic emulsion accounting for 6 weight percent, polyurethane emulsion accounting for 6 weight percent, aluminum hydroxide accounting for 5 weight percent, hydroxide powder flame retardant accounting for 8 weight percent, phosphorus flame retardant accounting for 6 weight percent, aluminum oxide accounting for 5 weight percent, silicon dioxide accounting for 5 weight percent, nano aluminum oxide accounting for 5 weight percent, dispersant accounting for 5 weight percent, thickener accounting for 2 weight percent, antioxidant accounting for 2 weight percent, polyvinyl alcohol accounting for 2 weight percent, modified graphite accounting for 3 weight percent, titanium dioxide accounting for 4 weight percent, fumed silica accounting for 3 weight percent, and silane coupling agent accounting for 3 weight percent;

[0041] Step 3: Take out the polyvinyl alcohol and store it separately, then stir the remaining mixed ingredients to ensure that all components can be fully mixed, and keep the stirring speed of the stirring equipment at 190 revolutions per minute.

[0042] Step 4: Take out the polyvinyl alcohol solution with a good ratio and pour it into the stirred mixture for secondary mixing. Use a stirring device to mix for 20 minutes.

[0043] Step 5: Add the silicone lubricant to the secondary mixed material and stir it for 25 minutes. At this time, the environmentally friendly flame retardant, water-resistant and cold-proof adhesive body is prepared.

[0044] It should be noted that: in step 1, the silane coupling agent is a chemical agent, the silane oxy group contained in it is reactive to inorganic substances, and the organic functional group is reactive or compatible to organic substances. Therefore, when the silane coupling agent is between the inorganic and organic interfaces, a bonding layer of organic matrix-silane coupling agent-inorganic matrix can be formed; in step 2, the mixing of various raw materials is mainly processed by a laboratory planetary mixer. After the power is turned on, the raw materials entering the mixer can be efficiently stirred and mixed; in step 3, the mixing equipment is used to mix the raw materials. The stirring time is 40 minutes; in step 4, polyvinyl alcohol needs to be stored in a cool, ventilated warehouse, away from fire and heat sources, and should be stored separately from oxidants, and mixed storage is strictly prohibited. In addition, fire-fighting equipment of corresponding types and quantities needs to be equipped, and suitable materials should be available in the storage area to contain leaks to ensure that the components of polyvinyl alcohol will not be damaged before use; in step 5, the organosilicon slip agent is specifically an organosiloxane emulsion, which is mainly divided into anionic, cationic and non-ionic types, is widely used in various coating systems, and has a more durable slippery feel.

[0045] In summary: this environmentally friendly flame retardant, water resistant and cold-proof material adhesive is set up through five steps of raw material preparation, mixing ingredients, stirring treatment, secondary mixing and completing mixing, and polyvinyl alcohol solution is added in the steps, which effectively reduces the occurrence of wire drawing phenomenon of flame retardant, water resistant and cold-proof material adhesive, makes the product surface smoother and more uniform, and avoids the problem of reduced glue bonding strength, thereby improving production efficiency.

[0046] Parts not involved in the present invention are the same as the prior art or can be implemented by the prior art. Although the embodiments of the present invention have been shown and described, it is understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An environmentally friendly flame retardant, water resistant and cold-proof material adhesive, characterized in that: include: An environmentally friendly flame retardant, water-resistant and cold-proof adhesive body (1), wherein the environmentally friendly flame retardant, water-resistant and cold-proof adhesive body (1) is composed of a polymer emulsion, a flame retardant, a filler and an auxiliary agent.

2. The environmentally friendly flame retardant, water resistant and cold-proof material adhesive according to claim 1, characterized in that: The polymer emulsion includes polyvinyl acetate emulsion, acrylate emulsion, polyurethane emulsion, the flame retardant includes aluminum hydroxide, hydroxide powder flame retardant, phosphorus flame retardant, the filler includes aluminum oxide, silicon dioxide, nano aluminum oxide, and the auxiliary agent includes dispersant, thickener, antioxidant and polyvinyl alcohol.

3. A method for preparing an environmentally friendly flame retardant, water resistant and cold-proof material adhesive, characterized in that: The following steps are involved: Step 1, raw material preparation, the preparation of the environmentally friendly flame retardant water-resistant cold-proof adhesive body (1) required for the preparation of polyvinyl acetate emulsion, acrylic emulsion, polyurethane emulsion, aluminum hydroxide, hydroxide powder flame retardant, phosphorus flame retardant, aluminum oxide, silicon dioxide, nano aluminum oxide, dispersant, thickener, antioxidant, polyvinyl alcohol and modified graphite, titanium dioxide, fumed silica and silane coupling agent are completed; Step 2, mixing ingredients, polyvinyl acetate emulsion, acrylic emulsion, polyurethane emulsion, aluminum hydroxide, hydroxide powder flame retardant, phosphorus flame retardant, aluminum oxide, silicon dioxide, nano aluminum oxide, dispersant, thickener, antioxidant, polyvinyl alcohol and modified graphite, titanium dioxide, fumed silica and silane coupling agent are mixed in a certain proportion, the specific proportion is polyvinyl acetate emulsion accounts for 38-50 weight percent, acrylic emulsion accounts for 5-8 weight percent, polyurethane emulsion accounts for 5-8 weight percent, aluminum hydroxide accounts for 4-6 weight percent, Hydroxide powder flame retardant accounts for 6-10 weight percent, phosphorus flame retardant accounts for 5-8 weight percent, aluminum oxide accounts for 3-6 weight percent, silicon dioxide accounts for 3-6 weight percent, nano aluminum oxide accounts for 3-6 weight percent, dispersant accounts for 3-6 weight percent, thickener accounts for 1-3 weight percent, antioxidant accounts for 1-3 weight percent, polyvinyl alcohol accounts for 1-3 weight percent, modified graphite accounts for 1-5 weight percent, titanium dioxide accounts for 1-5 weight percent, fumed silica accounts for 1-3 weight percent, and silane coupling agent accounts for 1-3 weight percent; Step 3: Take out the polyvinyl alcohol and store it separately, then stir the remaining mixed ingredients to ensure that the various components can be fully mixed, and the stirring speed of the stirring equipment is maintained at 160-190 revolutions per minute. Step 4: Take out the polyvinyl alcohol solution with a good ratio and pour it into the stirred mixture for secondary mixing. Use a stirring device to mix for 10-20 minutes. Step 5: Add an organic silicon lubricant to the secondary mixed material and stir for 15-25 minutes. At this time, the environmentally friendly flame retardant, water resistant and cold-proof adhesive body (1) is prepared.

4. The method for preparing an environmentally friendly flame retardant, water resistant and cold-proof material adhesive according to claim 3, characterized in that: In step one, the silane coupling agent is a chemical agent, the silane oxy groups it contains are reactive to inorganic substances, and the organic functional groups are reactive or compatible to organic substances. Therefore, when the silane coupling agent is located between the inorganic and organic interfaces, a bonding layer of organic matrix-silane coupling agent-inorganic matrix can be formed.

5. The method for preparing an environmentally friendly flame retardant, water resistant and cold-proof material adhesive according to claim 3, characterized in that: In step 2, the mixing of various raw materials is mainly carried out by a laboratory planetary mixer. After the power is turned on, the raw materials entering the mixer can be efficiently stirred and mixed.

6. The method for preparing an environmentally friendly flame retardant, water resistant and cold-proof material adhesive according to claim 3, characterized in that: In step three, the stirring time of the raw materials by the stirring equipment is 20-40 minutes.

7. The method for preparing an environmentally friendly flame retardant, water resistant and cold-proof material adhesive according to claim 3, characterized in that: In step four, polyvinyl alcohol needs to be stored in a cool, ventilated warehouse, away from fire and heat sources. It should be stored separately from oxidants and must not be mixed. In addition, fire-fighting equipment of corresponding types and quantities should be equipped. Suitable materials should be available in the storage area to contain leaks to ensure that the components of polyvinyl alcohol will not be destroyed before use.

8. The method for preparing an environmentally friendly flame retardant, water resistant and cold-proof material adhesive according to claim 3, characterized in that: In step five, the organosilicon slip agent is specifically an organosiloxane emulsion, which is mainly divided into anionic, cationic and non-ionic types, is widely used in various coating systems, and has a relatively durable slippery feel.