Preparation method and application of organic long-afterglow material for afterglow emission of acridinium yellow dye induced by AB glue
Through the chemical curing process of using AB glue to induce acridine yellow dye at room temperature, the complex preparation of organic long-term afterglow materials in the prior art was solved, and a simple and environmentally friendly preparation method and stable afterglow performance were achieved, which is suitable for multiple A kind of application scenario.
Patent Information
- Application Number
- CN202411179954.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
The existing preparation methods for organic long afterglow materials are complex, with problems such as solvent loss and heating, making it difficult to achieve a simple and environmentally friendly preparation process.
AB glue is used to induce acridine yellow dye to stir and stand at room temperature to form a mixed solution. The organic long afterglow material is obtained through the chemical curing process of AB glue, avoiding the solvent addition and heating steps.
It realizes simple and environmentally friendly organic long afterglow material preparation, and the obtained materials have stable afterglow properties, which are suitable for the application of films and three-dimensional models, expanding the application scenarios of materials.
Smart Images

Figure CN119081676A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of organic long afterglow material preparation method, in particular to an organic long afterglow material preparation method and application for AB glue-induced acriflavine dye afterglow emission. Background Art
[0002] Long afterglow (LPL) refers to the long-lasting luminescence of a material after the excitation light source is turned off. So far, the organic long afterglow materials developed by researchers have the advantages of long luminescence lifetime, low cost, good processing performance and biocompatibility. Therefore, they have great application potential in the fields of bioimaging, organic light-emitting diodes, anti-counterfeiting, etc.
[0003] In general, the persistent phosphorescence effect of pure organic compounds or complexes can be induced by precisely controlling the inter-system crossover (ISC) constant and non-radiative decay. Methods to enhance phosphorescence performance, such as crystallization induction, supramolecular assembly, H-aggregation, host-guest doping, and polymerization, can effectively stabilize ternary excitons under ambient conditions and achieve high-performance persistent phosphorescence effects. Introducing a rigid polymer matrix into doped materials is a widely explored method that can effectively suppress molecular vibrations and thus efficiently obtain long afterglow emission. In the literature, solvent dissolution, volatilization, film formation, thermal curing, and photocuring are generally used to induce the afterglow emission of organic small molecules, but this usually involves heating, solvent addition, ultraviolet irradiation, etc. These methods have the disadvantages of solvent loss and complex preparation process. Based on this, it is necessary to find a universal and simple and convenient material composite strategy to induce its long afterglow phenomenon, thereby expanding the application scenarios of the luminescence function of pure organic molecules. Summary of the invention
[0004] The invention provides a method for preparing an organic long afterglow material for inducing afterglow emission of acridinium yellow dyes by AB glue and application thereof, so as to solve the problem of complex preparation process in the prior art method for preparing organic long afterglow materials.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is: The invention discloses a method for preparing an organic long afterglow material capable of inducing afterglow emission of acridinium yellow dyes by AB glue. The method comprises the following steps: using acridinium yellow dyes and AB glue as raw materials, mixing the acridinium yellow dyes with the AB glue, and stirring the mixture at room temperature of 20-25°C for at least 5 minutes to form a mixed solution; and then allowing the mixed solution to stand at room temperature of 20-25°C until solidified to obtain the organic long afterglow material.
[0006] Furthermore, the mass ratio of the acriflavine dye to the A glue in the AB glue is 1:(1500-3000), and the mass ratio of the A glue to the B glue in the AB glue is 3:1.
[0007] Furthermore, the acriflavine dye is acriflavine, or acriflavine hydrochloride, or proflavine sulfate.
[0008] Furthermore, in the AB glue, A glue is epoxy resin and B glue is crystal glue.
[0009] An application of an organic long afterglow material prepared by the method for preparing an organic long afterglow material for afterglow emission of acriflavine dyes induced by AB glue in preparing an organic long afterglow material film.
[0010] An application of an organic long afterglow material prepared by the method for preparing an organic long afterglow material for afterglow emission of acriflavine dyes induced by AB glue in preparing a three-dimensional model of an organic long afterglow material.
[0011] The present invention discloses a method for preparing an organic long afterglow material that induces afterglow emission of acridinium yellow dyes by AB chemical curing adhesive, and the application of the prepared organic long afterglow material. Compared with the prior art, the present invention has the following advantages: 1. In the preparation method of the present invention, afterglow emission of the acridinium yellow dye under white light excitation can be induced by mixing the acridinium yellow dye with AB chemical curing adhesive and performing a curing process.
[0012] 2. The preparation method of the present invention has a simple preparation process (prepared at room temperature, without heating), is environmentally friendly and easy to obtain (without adding any additional organic solvents); and the obtained organic long afterglow material has stable afterglow performance. The conditions for further obtaining long afterglow films and three-dimensional models through the method of the present invention are mild and not harsh, which will be very beneficial to the application of LPL materials in various scenarios.
[0013] 3. The organic long afterglow material prepared by the preparation method of the present invention can be used to form organic long afterglow material films and three-dimensional models, and has the advantage of wide application. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 The macroscopic LPL images of the organic long afterglow material film obtained in the example at room temperature (from left to right: during white light excitation, 1 s, and 3 s after turning off the white light lamp).
[0015] Figure 2 This is the afterglow performance attenuation spectrum of the organic long afterglow material film obtained using acriflavine as the raw material in the example.
[0016] Figure 3 The afterglow performance attenuation spectrum of the organic long afterglow material film obtained by using acriflavine hydrochloride as a raw material in the embodiment; Figure 4 This is the attenuation spectrum of the afterglow performance of the organic long afterglow material film obtained by using proflavine sulfate as the raw material in the embodiment; Figure 5This is a macroscopic LPL photo of a three-dimensional model prepared from an organic long afterglow material obtained using acriflavine as a raw material in the example ( Figure 5 The top row from left to right shows the model when it is excited by white light from the front, and 1 s, 2 s, and 3 s after the white light is turned off; Figure 5 The bottom row from left to right shows the model when excited by white light from the side, after turning off the white light, when excited by 430 nm visible light, and after turning off the excitation). DETAILED DESCRIPTION
[0017] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0018] This embodiment discloses a method for preparing an organic long afterglow material for inducing afterglow emission of acridinium yellow dyes by AB glue, using acridinium yellow dyes and AB glue as raw materials. In the raw materials, the mass ratio of acridinium yellow dyes to A glue in AB glue is 1: (1500-3000), in ml; the mass ratio of A glue to B glue in AB glue is 3: 1, in g.
[0019] In this embodiment, the manufacturer of acriflavine dyes is Tianjin Xiens Biochemical Technology Co., Ltd. (purity: 98%). Acriflavine dyes are acriflavine, or acriflavine hydrochloride, or proflavine sulfate. The structural formula of acriflavine is as follows:
[0020] The structural formula of Acriflavine hydrochloride is as follows:
[0021] The structural formula of proflavine sulfate is as follows:
[0022] In this embodiment, the A glue in the AB glue is epoxy resin, and the B glue is crystal glue, that is, the AB glue is epoxy resin-crystal glue. The purchase manufacturer of epoxy resin-crystal glue is Shenzhen Juhengchuang Co., Ltd.
[0023] In this embodiment, acridine yellow dye and AB glue are mixed and stirred at room temperature of 20-25°C for at least 5 minutes to form a mixed solution; then the mixed solution is allowed to stand at room temperature of 20-25°C until solidified, thereby obtaining an organic long afterglow material.
[0024] In this embodiment, after obtaining the mixed solution, the mixed solution is drop-coated on a glass substrate to form a thin film, and then the thin film is left to stand at room temperature of 20-25°C for 24 hours until solidified, thereby obtaining an organic long afterglow material thin film. Therefore, the organic long afterglow material prepared in this embodiment can be used to form an organic long afterglow material thin film.
[0025] Figure 1This is a macroscopic LPL picture of the organic long afterglow material film obtained by this embodiment at room temperature. The film is excited by a white light lamp, and the white light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 3 seconds. It can be seen that the organic long afterglow material film emits light more uniformly, indicating that the present invention can induce afterglow emission of acridinium yellow under white light excitation by mixing acridinium yellow and AB chemical curing adhesive and performing a curing process.
[0026] Figure 2 : is the afterglow performance attenuation diagram of the organic long afterglow material film obtained when the acridinium yellow dye is acridinium yellow in this embodiment. Figure 2 It can be seen that -2 s to 0 s is when the organic long afterglow material film prepared by this embodiment is irradiated by a white light lamp, and the organic long afterglow material film exhibits photoluminescence characteristics; 0 s to 3 s is when the organic long afterglow material film is removed from the white light lamp, and the afterglow time is about 3 s, which is similar to the afterglow time observed by the naked eye. This shows that the present invention can induce afterglow emission of acridinium yellow under white light excitation by mixing acridinium yellow and AB chemical curing adhesive and performing a curing process.
[0027] Figure 3 : is the afterglow performance attenuation diagram of the organic long afterglow material film obtained when the acridinium yellow dye is acridinium yellow hydrochloride in this embodiment. Figure 3 It can be seen that -2 s to 0 s is when the organic long afterglow material film prepared by this embodiment is irradiated by a white light lamp, and the organic long afterglow material film exhibits photoluminescence characteristics; 0 s to 2 s is when the organic long afterglow material film is removed from the white light lamp, and the afterglow time is about 2 s, which is similar to the afterglow time observed by the naked eye. This shows that the present invention can induce afterglow emission of acridinium yellow hydrochloride under white light excitation by mixing acridinium yellow hydrochloride and AB chemical curing adhesive and performing a curing process.
[0028] Figure 4 This is a graph showing the attenuation of the afterglow performance of an organic long afterglow material film obtained when the acridinium yellow dye is flavin sulfate. Figure 4 It can be seen that -2 s to 0 s is when the organic long afterglow material film prepared in Example 3 is irradiated by a white light lamp, and the organic long afterglow material film exhibits photoluminescence characteristics; 0 s to 1 s is when the organic long afterglow material film is removed from the white light lamp, and the afterglow time is about 1 s. This indicates that the present invention can induce afterglow emission of proflavine sulfate under white light excitation by mixing proflavine sulfate and AB chemical curing adhesive and performing a curing process.
[0029] Figure 5This is a macroscopic LPL picture of the three-dimensional model of organic long afterglow material at room temperature obtained by using acridine yellow as the acridine yellow dye in this embodiment. The upper row shows the three-dimensional model excited from the front with a white light lamp. The white light source is turned off after 3 seconds of irradiation, and the afterglow can be maintained for 3 s; the two pictures on the left side of the lower row show that the three-dimensional model is excited from the side with a white light lamp. The white light source is turned off after 3 seconds of irradiation, and there is a bright afterglow. The two pictures on the right side show that the three-dimensional model is excited from the side with 430 nm visible light. The light source is turned off after 3 seconds of irradiation, and there is a bright afterglow. It can be seen that the three-dimensional model of organic long afterglow material emits light more evenly. The pictures illustrate that the present invention can induce afterglow emission of acridine yellow under the excitation of 430 nm visible light and white light by mixing acridine yellow and AB chemically curing adhesive and performing a curing process.
[0030] In this embodiment, after obtaining the mixed solution, the mixed solution is applied to a large area of a three-dimensional mold, and then left to stand at room temperature of 20-25°C for 24 hours until solidified, and then demolded to obtain a three-dimensional model of an organic long afterglow material that emits uniform light under white light excitation. Therefore, the organic long afterglow material prepared in this embodiment can be used to form a three-dimensional model of an organic long afterglow material.
[0031] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. The embodiments described in the present invention are merely descriptions of the preferred embodiments of the present invention, and do not limit the concept and scope of the present invention. The various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction, and such combinations should also be regarded as the contents disclosed in the present disclosure as long as they do not violate the concept of the present invention. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0032] The present invention is not limited to the specific details of the above-mentioned embodiments. Within the technical concept of the present invention and without departing from the design concept of the present invention, various modifications and improvements made to the technical solution of the present invention by technical personnel in this field should fall within the protection scope of the present invention. The technical contents for which protection is sought in the present invention have been fully recorded in the claims.
Claims
1. A method for preparing an organic long afterglow material for afterglow emission of acridinium yellow dye induced by AB glue, characterized in that: Acridine yellow dye and AB glue are used as raw materials. The acridine yellow dye and AB glue are mixed and stirred at room temperature of 20-25°C for at least 5 minutes to form a mixed solution. The mixed solution is then allowed to stand at room temperature of 20-25°C until solidified to obtain an organic long afterglow material.
2. The method for preparing an organic long afterglow material for afterglow emission of acridinium yellow dye induced by AB glue according to claim 1, characterized in that: The mass ratio of the acridinium yellow dye to the A glue in the AB glue is 1:(1500-3000), and the mass ratio of the A glue to the B glue in the AB glue is 3:
1.
3. The method for preparing an organic long afterglow material for afterglow emission of acridinium yellow dyes induced by AB glue according to claim 1 or 2, characterized in that: The acriflavine dye is acriflavine, or acriflavine hydrochloride, or proflavine sulfate.
4. The method for preparing an organic long afterglow material for afterglow emission of acridinium yellow dye induced by AB glue according to claim 3, characterized in that: In the AB glue, A glue is epoxy resin and B glue is crystal glue.
5. An application of an organic long afterglow material prepared by the method for preparing an organic long afterglow material for afterglow emission of acridinium yellow dyes induced by AB glue as claimed in any one of claims 1 to 4 in preparing an organic long afterglow material film.
6. An application of an organic long afterglow material prepared by the method for preparing an organic long afterglow material with afterglow emission induced by AB glue of acriflavine dyes as claimed in any one of claims 1 to 4 in preparing a three-dimensional model of an organic long afterglow material.