Application of photocuring adhesive in inducing long afterglow emission of organic dye
By mixing the photocuring glue with organic dye and curing ultraviolet light, the problem of difficult to induce long afterglow emission of organic dye under visible light excitation is solved, and a simple and environmentally friendly long afterglow material preparation is achieved. The obtained film shows good afterglow performance and stability.
Patent Information
- Application Number
- CN202411214170.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-31
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-31
AI Technical Summary
Under visible light excitation, it is difficult to induce long afterglow emission of organic traditional fluorescent dyes in a solid state, and the existing methods are complex and inconvenient for in-depth research.
A mixture of photocuring glue and organic dye is cured by ultraviolet light irradiation to prepare a material with long afterglow emission properties. The specific steps include mixing the photocuring glue and the organic dye in a specific ratio and curing it at room temperature using a 15W ultraviolet lamp. The resulting material can achieve a smooth and smooth film preparation without heating and no additional solvent.
It realizes simple and environmentally friendly long afterglow emission of organic dyes at room temperature. The obtained film has good afterglow performance and stability, and is suitable for various application scenarios.
Smart Images

Figure CN119081679A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic long afterglow materials, and in particular to application of a photocurable adhesive in inducing long afterglow emission of an organic dye. Background Art
[0002] Organic long afterglow materials have the advantages of low price, simple synthesis, good biocompatibility and easy modification of functional groups, etc., which have attracted widespread attention from scientific researchers. At present, many organic small molecules with long afterglow luminescence properties have been prepared and widely used in three-dimensional display, anti-counterfeiting and information encryption, and biological imaging.
[0003] Among various wavelengths of excitation, the afterglow of visible light excitation is particularly suitable for applications such as display, information encryption, and lighting equipment. However, this usually requires modification of the chemical structure of organic compounds or chromophores. This method usually requires complex molecular design and chemical synthesis, which hinders researchers from conducting deeper exploration. According to literature reports, dye molecules with charge transfer state (CT) characteristics help absorb light in the visible light region [Garain S, Ansari SN, Kongasseri AA, et al. Room temperature charge-transfer phosphorescence from organic donor-acceptor co-crystals[J]. Chemical Science, 2022, 13(34): 10011-10019; Garain S, Wagalgave SM, Kongasseri AA, et al. Anion-π-induced room temperature phosphorescence from emissive charge-transfer states[J]. Journal of the American Chemical Society, 2022, 144(24): 10854-10861; Wang J, Yang Y, Li K, et al. Purely organic fluorescence afterglow: visible-light-excitation, inherent mechanism, tunable color, and practical applications with very low cost[J]. Angewandte Chemie International Edition, 2023, 62(30): e202304020.]. Various environmental stimulus responses based on LPL emission can be achieved by blending organic dyes with polymer matrices (such as PVA, etc.). However, the diversity of the molecular structures of commercial organic dyes still poses a challenge to finding a universal and convenient material composite strategy to induce their LPL phenomenon, especially under visible light excitation. This challenge prompted us to develop a simple and universal strategy to conveniently endow organic traditional fluorescent dyes with excellent afterglow emission in the solid state under visible light excitation. Summary of the invention
[0004] The technical problem to be solved by the present invention is how to induce long afterglow emission of organic dyes.
[0005] The present invention solves the above technical problems through the following technical means:
[0006] A use of a photocurable adhesive in inducing long afterglow emission of an organic dye, wherein the photocurable adhesive is a mixture of one or more of UV curing adhesive 3491, UV curing adhesive 3492, UV drip glue D-606, and UV shadowless glue V-3218; and the organic dye is a mixture of one or more of safranin, basic fuchsin, Nile blue, hematoxylin, acid fuchsin, fluorescein, and solvent green 7.
[0007] The structural formula of the organic dye is shown below:
[0008]
[0009] Preferably, the UV curing adhesive 3491 is from Henkel Loctite (China) Co., Ltd. AA3491, UV curing adhesive 3491 of Guangdong Youyang New Materials Co., Ltd., or a mixture of two of them.
[0010] Preferably, the UV curing adhesive 3492 is from Henkel Loctite (China) Co., Ltd. AA3492, UV curing adhesive 3492 of Guangdong Youyang New Materials Co., Ltd., or a mixture of two of them.
[0011] Preferably, the UV glue D-606 comes from Foshan Jinggu Adhesive Co., Ltd.; the UV shadowless glue V-3218 comes from Dongguan Lelai Adhesive Products Co., Ltd.
[0012] The present invention also provides a method for inducing long afterglow emission of organic dyes with photocurable adhesive, comprising the following steps: uniformly mixing the photocurable adhesive and the organic dye, and curing them with ultraviolet light.
[0013] Preferably, the weight ratio of the photocurable adhesive to the organic dye is 300-600:1; during the irradiation process, a UV lamp with a power of 15W is used for irradiation, and the irradiation time is 20-40s.
[0014] Preferably, the mixture is stirred and mixed at room temperature.
[0015] The present invention also provides a method for preparing a long afterglow material, comprising the following steps: uniformly mixing the photocurable adhesive and the organic dye, and curing the mixture with ultraviolet light to obtain the long afterglow material.
[0016] Preferably, the weight ratio of the photocurable adhesive to the organic dye is 300-600:1; and a 15W ultraviolet lamp is used for irradiation and curing for 20-40 seconds.
[0017] Preferably, the method further comprises coating a product obtained by uniformly mixing the photocurable adhesive and the organic dye on the substrate.
[0018] Preferably, the coating method is drop coating.
[0019] Preferably, the coated substrate is glass.
[0020] The present invention also provides a long afterglow material, which is prepared by adopting the preparation method of the long afterglow material.
[0021] Preferably, the long afterglow material is a film, a coating or a luminescent body.
[0022] The advantages of the present invention are:
[0023] (1) By mixing the photocurable adhesive with organic traditional dyes, the curable adhesive provides a rigid environment for the dye molecules, which can induce the long afterglow emission of the organic traditional dyes.
[0024] (2) The preparation method of the present invention has a simple preparation process (prepared at room temperature, without heating), is environmentally friendly and easy to obtain (no additional organic solvent is added); and the obtained film is flat and smooth, has good afterglow performance, and has stable afterglow performance. The conditions for obtaining the film are mild and not harsh, which will be very beneficial to the application of LPL materials in various scenarios. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The macroscopic LPL images of the long afterglow film obtained in Example 1 of the present invention at room temperature (from left to right: when excited, 1 second after turning off the 430nm visible light lamp, and 2 seconds after turning off the 430nm visible light lamp);
[0026] Figure 2 This is the afterglow performance attenuation spectrum of the long afterglow film obtained in Example 1 of the present invention;
[0027] Figure 3 This is a macroscopic LPL picture of the long afterglow film obtained in Example 2 of the present invention at room temperature (from left to right: when excited and 1 second after turning off the 430nm visible light lamp);
[0028] Figure 4 This is the afterglow performance attenuation spectrum of the long afterglow film obtained in Example 2 of the present invention;
[0029] Figure 5 This is a macroscopic LPL picture of the long afterglow film obtained in Example 3 of the present invention at room temperature (from left to right: when excited and 1 second after turning off the 430nm visible light lamp);
[0030] Figure 6This is a macroscopic LPL picture of the long afterglow film obtained in Example 4 of the present invention at room temperature (from left to right: when excited and 1 second after turning off the 430nm visible light lamp);
[0031] Figure 7 This is a macroscopic LPL image of the long afterglow film obtained in Example 5 of the present invention at room temperature (from left to right: when excited and 1 second after turning off the 430nm visible light lamp);
[0032] Figure 8 This is the afterglow performance attenuation spectrum of the long afterglow film obtained in Example 6 of the present invention;
[0033] Fig. 9 This is a macroscopic LPL image of the long afterglow film obtained in Example 7 of the present invention at room temperature (from left to right: when excited and 1 second after turning off the 430nm visible light lamp);
[0034] Fig.10 The present invention is a traditional organic dye safranin in Example 1 and Afterglow performance decay spectrum of the long afterglow film obtained by AA3492 at room temperature;
[0035] Fig.11 The macroscopic LPL images of the long afterglow film obtained from the organic traditional dye safranin and the ultraviolet curing adhesive 3491 in Example 1 of the present invention at room temperature (from left to right: when excited, 1 second after turning off the 430nm visible light lamp, and 2 seconds after turning off the 430nm visible light lamp);
[0036] Fig.12 The macroscopic LPL images of the long afterglow film obtained from the organic traditional dye safranin and the ultraviolet curing adhesive 3492 (Guangdong Youyang New Materials Co., Ltd.) in Example 1 at room temperature (from left to right: when excited, 1 second after turning off the 430nm visible light lamp, and 2 seconds after turning off the 430nm visible light lamp);
[0037] Fig.13 The macroscopic LPL images of the long afterglow film obtained from the organic traditional dye safranin and UV glue D-606 in Example 1 of the present invention at room temperature (from left to right: when excited, 1 second after turning off the 430nm visible light lamp, and 2 seconds after turning off the 430nm visible light lamp);
[0038] Fig.14 This is the macroscopic LPL picture of the long afterglow film obtained from the traditional organic dye safranin and UV shadowless adhesive V-3218 in Example 1 of the present invention at room temperature (from left to right: during excitation, 1 second after turning off the 430nm visible light lamp, and 2 seconds after turning off the 430nm visible light lamp). DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0041] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0042] The sources of the drugs involved in the following Examples 1-7 and Comparative Examples 1-3 are as follows:
[0043] The organic dye was purchased from Tianjin Xiensi Biochemical Technology Co., Ltd. (purity: 98%); the light-curing adhesive was purchased from Henkel Loctite (China) Co., Ltd. AA3491, AA3491 is a transparent, low viscosity, modified acrylate liquid adhesive that cures after a few seconds of 365nm UV exposure.
[0044] The instruments and models involved in the following embodiments and comparative examples are as follows:
[0045] Ocean Optics multi-band spectrometer;
[0046] Room temperature: 20~25℃.
[0047] The substrate may be glass or paper. In the following embodiments, the substrate is glass.
[0048] In the following examples and comparative examples, the power of the ultraviolet lamp is 15 W (365 nm), and the power of the visible light lamp is 30 W (430 nm).
[0049] Examples 1 to 7
[0050] A method for inducing long afterglow of an organic dye with a photocurable adhesive, the specific method comprising: mixing 500 mg of photocurable adhesive and 1 mg of an organic dye, stirring for 5 min at room temperature of 20 to 25° C. to obtain a mixed solution of the photocurable adhesive and the dye, taking 0.5 mL of the mixed solution and drop-coating it on a glass substrate, and curing it with a 15 W ultraviolet lamp for 30 s to obtain a long afterglow film, wherein the organic dyes used in Examples 1 to 7 are respectively shown in Table 1 Examples 1 to 7.
[0051] Comparative Examples 1 to 3
[0052] A method for inducing long afterglow of an organic dye with a photocurable adhesive, the specific method comprising: mixing 500 mg of the photocurable adhesive and 1 mg of the organic dye, stirring for 5 min at room temperature of 20 to 25° C. to obtain a mixed solution of the photocurable adhesive and the dye, dropping 0.5 mL of the mixed solution on a glass substrate, and curing for 30 s with a 15 W ultraviolet lamp to obtain a thin film, wherein the organic dyes used in Comparative Examples 1 to 3 are respectively shown in Comparative Examples 1 to 3 in Table 1.
[0053] Table 1 Organic dyes used in Examples 1-7 and Comparative Examples 1-3 and the afterglow time of the obtained films
[0054]
[0055]
[0056] After the light-curing adhesive is introduced into the present invention and a light-curing process is performed, a LPL film with relatively uniform light emission can be obtained.
[0057] Figure 1 This is a macroscopic LPL picture of the long afterglow film obtained in Example 1 at room temperature. The film is excited by a 430nm visible light lamp, and the visible light lamp is turned off after irradiation for 3 seconds. The film can maintain the afterglow for 2s. It can be seen that the obtained film emits light more uniformly, indicating that the long afterglow emission of the traditional organic dye safranin is induced after the introduction of the photocurable adhesive in the present invention.
[0058] Figure 2 This is the afterglow performance attenuation spectrum of the film obtained in Example 1 at room temperature. It can be seen from the figure that -2s to 0s is when a 430nm visible light lamp irradiates the organic long afterglow material (i.e., the obtained long afterglow film), and the organic long afterglow material exhibits photoluminescence characteristics; 0s to 2s is when the organic long afterglow material exhibits orange-red long afterglow luminescence after the visible light lamp is removed, and the afterglow time is about 2s, which is similar to the afterglow time observed by the naked eye.
[0059] Figure 3 This is a macroscopic LPL picture of the long afterglow film obtained in Example 2 at room temperature. The film is excited by a 430nm visible light lamp, and the visible light lamp is turned off after irradiation for 3 seconds. The film can maintain the afterglow for 1 second. It can be seen that the obtained film emits light more uniformly, indicating that the long afterglow emission of the traditional organic dye basic fuchsin is induced after the photocuring adhesive is introduced into the present invention.
[0060] Figure 4This is the afterglow performance attenuation spectrum of the film obtained in Example 2 at room temperature. It can be seen from the figure that -2s to 0s is the 430nm visible light lamp irradiating the organic long afterglow material (i.e. the obtained long afterglow film), and the organic long afterglow material exhibits photoluminescence characteristics; 0s to 1s is the organic long afterglow material exhibiting red long afterglow luminescence after the visible light lamp is removed, and the afterglow time is about 1s, which is similar to the afterglow time observed by the naked eye.
[0061] Figure 5 This is a macroscopic LPL picture of the long afterglow film obtained in Example 3 at room temperature. The film is excited by a 430nm visible light lamp, and the visible light lamp is turned off after irradiation for 3 seconds. The film can maintain the afterglow for 1 second. It can be seen that the obtained film emits light more uniformly, indicating that the long afterglow emission of the traditional organic dye Nile blue is induced by the introduction of the photocurable adhesive in the present invention.
[0062] Figure 6 This is a macroscopic LPL picture of the long afterglow film obtained in Example 4 at room temperature. The film is excited by a 430nm visible light lamp, and the visible light lamp is turned off after irradiation for 3 seconds. The film can maintain the afterglow for 1 second. It can be seen that the obtained film emits light more uniformly, indicating that the introduction of the photocurable adhesive in the present invention induces the long afterglow emission of the traditional organic dye hematoxylin.
[0063] Figure 7 This is a macroscopic LPL picture of the long afterglow film obtained in Example 5 at room temperature. The film is excited by a 430nm visible light lamp, and the visible light lamp is turned off after irradiation for 3 seconds. The film can maintain the afterglow for 1 second. It can be seen that the obtained film emits light more uniformly, indicating that the long afterglow emission of the traditional organic dye acid fuchsin is induced after the introduction of the photocurable adhesive in the present invention.
[0064] Figure 8 This is the afterglow performance attenuation spectrum of the film obtained in Example 6 at room temperature. It can be seen from the figure that from -2s to 0s is the 430nm visible light lamp irradiating the organic long afterglow material (i.e. the obtained long afterglow film), and the organic long afterglow material exhibits photoluminescence characteristics; from 0s to 1s is the organic long afterglow material exhibiting long afterglow luminescence after the visible light lamp is removed, and the afterglow time is about 1s.
[0065] Fig. 9 This is a macroscopic LPL picture of the long afterglow film obtained in Example 7 at room temperature. The film is excited by a 430nm visible light lamp, and the visible light lamp is turned off after irradiation for 3 seconds. The film can maintain the afterglow for 1 second. It can be seen that the obtained film emits light more uniformly, indicating that the introduction of the photocurable adhesive in the present invention induces the long afterglow emission of the organic traditional dye Solvent Green 7.
[0066] In the above embodiments 1 to 7, the light-curing adhesive is replaced by AA3492 (Henkel Loctite (China) Co., Ltd.), UV curing adhesive 3491 (Guangdong Youyang New Materials Co., Ltd.) and UV curing adhesive 3492 (Guangdong Youyang New Materials Co., Ltd.), UV drip glue D-606 (Foshan Jinggu Adhesive Co., Ltd.), UV shadowless glue V-3218 (Dongguan Lelai Adhesive Products Co., Ltd.), V-3018 (Dongguan Lelai Adhesive Products Co., Ltd.) were prepared according to the above steps. Among them, the film prepared by V-3018 and the above dye molecules had no afterglow effect. The films prepared by the other five light-curing adhesives were able to achieve the same effect as the above embodiment, as shown in the effect diagram. Figure 10-14 shown.
[0067] Fig.10 The organic traditional dye safranin in Example 1 and The afterglow performance attenuation spectrum of the long afterglow film obtained from AA3492 (Henkel Loctite (China) Co., Ltd.) at room temperature. As can be seen from the figure, -2s to 0s is the 430nm visible light lamp irradiating the organic long afterglow material (i.e. the obtained film), and the organic long afterglow material exhibits photoluminescence characteristics; 0s to 2s is the orange-red long afterglow luminescence of the organic long afterglow material after the visible light lamp is removed, and the afterglow time is about 2s, which is similar to the afterglow time observed by the naked eye.
[0068] Fig.11 This is a macroscopic LPL picture of a long afterglow film obtained from the traditional organic dye safranin and the ultraviolet curing adhesive 3491 (Guangdong Youyang New Materials Co., Ltd.) in Example 1 at room temperature. The film is excited by a 430nm visible light lamp, and the visible light lamp is turned off after irradiation for 3 seconds. The film can maintain the afterglow for 2s. It can be seen that the obtained film emits light more uniformly, indicating that the long afterglow emission of the traditional organic dye safranin is induced after the introduction of the photocuring adhesive in the present invention.
[0069] Fig.12 This is a macroscopic LPL picture of a long afterglow film obtained from the traditional organic dye safranin and the ultraviolet curing adhesive 3492 (Guangdong Youyang New Materials Co., Ltd.) in Example 1 at room temperature. The film is excited by a 430nm visible light lamp, and the visible light lamp is turned off after irradiation for 3 seconds. The film can maintain the afterglow for 2s. It can be seen that the obtained film emits light more uniformly, indicating that the long afterglow emission of the traditional organic dye safranin is induced after the introduction of the photocuring adhesive in the present invention.
[0070] Fig.13This is a macroscopic LPL picture of a long afterglow film obtained from the traditional organic dye safranin and UV glue D-606 (Foshan Jinggu Adhesive Co., Ltd.) in Example 1 at room temperature. The film is excited by a 430nm visible light lamp, and the visible light lamp is turned off after irradiation for 3 seconds. The film can maintain the afterglow for 2s. It can be seen that the obtained film emits light more uniformly, indicating that the long afterglow emission of the traditional organic dye safranin is induced after the photocuring glue is introduced into the present invention.
[0071] Fig.14 This is a macroscopic LPL picture of a long afterglow film obtained from the traditional organic dye safranin and UV shadowless adhesive V-3218 (Dongguan Lelai Adhesive Products Co., Ltd.) in Example 1 at room temperature. The film is excited by a 430nm visible light lamp, and the visible light lamp is turned off after irradiation for 3 seconds. The film can maintain the afterglow for 2s. It can be seen that the obtained film emits light more uniformly, indicating that the long afterglow emission of the traditional organic dye safranin is induced after the introduction of the photocurable adhesive in the present invention.
[0072] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An application of a photocurable adhesive in inducing long afterglow emission of an organic dye, wherein the photocurable adhesive is a mixture of one or more of UV curing adhesive 3491, UV curing adhesive 3492, UV drip glue D-606, and UV shadowless glue V-3218; and the organic dye is a mixture of one or more of safranin, basic fuchsin, Nile blue, hematoxylin, acid fuchsin, fluorescein, and solvent green 7.
2. The use of the photocurable adhesive according to claim 1 in inducing long afterglow emission of organic dyes, characterized in that: The UV curing adhesive 3491 is from Henkel Loctite (China) Co., Ltd. AA3491, UV curing adhesive 3491 of Guangdong Youyang New Materials Co., Ltd., or a mixture of two of them.
3. The use of the photocurable adhesive according to claim 1 in inducing long afterglow emission of organic dyes, characterized in that: The UV curing adhesive 3492 is from Henkel Loctite (China) Co., Ltd. AA3492, UV curing adhesive 3492 of Guangdong Youyang New Materials Co., Ltd., or a mixture of two of them.
4. The use of the photocurable adhesive according to claim 1 in inducing long afterglow emission of organic dyes, characterized in that: The UV glue D-606 comes from Foshan Jinggu Adhesive Co., Ltd.; the UV shadowless glue V-3218 comes from Dongguan Lelai Adhesive Products Co., Ltd.
5. A method for inducing long afterglow emission of organic dyes by photocuring adhesive, characterized in that: The following steps are involved: The photocurable adhesive according to any one of claims 1 to 4 and the organic dye according to any one of claims 1 to 4 are uniformly mixed and cured by ultraviolet light.
6. The method for inducing long afterglow emission of organic dyes by photocuring adhesive according to claim 5, characterized in that: The weight ratio of the photocurable adhesive to the organic dye is 300-600:1; during the irradiation process, a 15W ultraviolet lamp is used for irradiation, and the irradiation time is 20-40s.
7. A method for preparing a long afterglow material, characterized in that: The following steps are involved: The photocurable adhesive according to any one of claims 1 to 4 and the organic dye according to any one of claims 1 to 4 are uniformly mixed, and the mixture is cured by ultraviolet light to obtain the long afterglow material.
8. The method for preparing the long afterglow material according to claim 7, characterized in that: The weight ratio of the photocurable adhesive to the organic dye is 300-600:1; a 15W ultraviolet lamp is used for irradiation and curing, and the time is 20-40s.
9. The method for preparing the long afterglow material according to claim 7 or 8, characterized in that: Before irradiating with ultraviolet light, the method also includes coating a product obtained by uniformly mixing the photocurable adhesive and the organic dye on the substrate.
10. A long afterglow material, characterized in that: The long afterglow material is prepared by the preparation method of any one of claims 7 to 9.
Citation Information
Patent Citations
Room temperature phosphorescence apparatus and methods